Wear-resistant PET transfer film and preparation method thereof
Through the combination of modified alumina particles and other fillers, the wear resistance and mechanical properties of the PET transfer film are improved, and the problem of easy damage to the PET base film during the scraping process is solved, which extends the service life and improves recycling. sex.
Patent Information
- Application Number
- CN202411472292.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-22
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-10-22
AI Technical Summary
The PET transfer film is easily damaged during the pressing and scraping process, resulting in poor recycling of the base film and needs to improve its wear resistance.
Modified alumina particles are used as fillers and modified by PEG or silane coupling agent to improve the crystallization degree and surface strength of the PET base film, and play a supporting load and self-lubricating role in the friction process, combining mica powder and nanometers Fillers such as barium carbonate optimize the dispersion and bonding effect of the filler and increase the wear resistance of the base film.
The wear resistance and mechanical properties of the PET base film are significantly improved, the service life is extended, and the recycling of the base film and the overall performance of the transfer film are improved.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of transfer films, and more specifically, to a wear-resistant PET transfer film and a preparation method thereof. Background Art
[0002] The transfer film is an intermediate carrier that exists on a transfer paper base or a plastic base. It carries the printed or printed pattern and is a chemical elastic film used to transfer it to the printed object.
[0003] Commonly used transfer films mainly use BOPP and PET as carriers, but PET has a higher recycling rate, so it is more widely used. During the use of some transfer films, the base film needs to be pressed and scraped, which can easily cause the base film to break, making it difficult to recycle the base film. Therefore, the performance of the base film needs to be improved. Summary of the invention
[0004] In order to improve the wear resistance of the base film and enhance the reusability of the base film, the present application provides a wear-resistant PET transfer film and a preparation method thereof.
[0005] The present application provides a wear-resistant PET transfer film, which adopts the following technical solution: In a first aspect, the present application provides a wear-resistant PET transfer film, comprising a PET base film, a coating layer, a glue layer and an aluminum foil layer arranged in sequence; The PET base film comprises the following raw materials in parts by weight: 40-42 parts of ethylene glycol; 80-90 parts of terephthalic acid; Catalyst 0.04-0.06 parts; Additives 0.02-0.03 parts; 1-2 parts of filler; The filler comprises aluminum oxide particles, and the aluminum oxide particles are aluminum oxide particles modified by a modifier, and the modifier is selected from PEG or a silane coupling agent.
[0006] By adopting the above technical solution and selecting alumina particles as filler, the alumina particles can promote PET heterogeneous nucleation and improve the degree of crystallization of PET film, thereby improving the mechanical properties of PET base film, thereby improving the wear resistance of PET base film to a certain extent.
[0007] Secondly, alumina particles can be dispersed in the PET base film, effectively improving the surface strength of the base film, and can also play a role in supporting the load during the friction process. The fine alumina particles can also fill the friction surface and play a self-lubricating role, effectively improving the wear resistance of the base film.
[0008] Finally, the alumina particles are modified by PEG or silane coupling agent. The alumina particles can undergo hydroxylation and dehydration reaction with the modifier, so that the surface of the alumina particles is coated with a modifier layer, which reduces the possibility of agglomeration of the alumina particles and effectively improves the compatibility between the alumina particles and PET, reduces the possibility of the alumina particles detaching from PET and remaining on the friction dual surface, and enables the PET base film to obtain uniform and excellent wear resistance.
[0009] Optionally, the mass ratio of the modifier to the alumina particles is 1:10-20.
[0010] By adopting the above technical solution, the mass ratio between the modifier and the alumina particles is optimized. The appropriate mass ratio can enable the modifier to fully wrap the alumina particles, reduce the possibility of agglomeration of the alumina particles, and make the alumina particles evenly dispersed in the base film, so that the base film obtains uniform wear resistance and mechanical properties.
[0011] Optionally, the alumina particles are hollow structures.
[0012] By adopting the above-mentioned technical scheme and using hollow alumina particles as fillers, the mass of the alumina particles can be effectively reduced and the volume of the alumina particles can be appropriately increased, which is beneficial to reducing the surface polarity of the alumina particles, improving the dispersibility of the alumina particles in the base film, and reducing the possibility of alumina particles settling in the base film, so that the base film obtains a uniform and stable wear-resistant effect, thereby extending the service life of the base film.
[0013] Optionally, the alumina particles are prepared as follows: potassium aluminum sulfate, urea and water are mixed, heated for reaction, filtered, washed, solid matter is retained, dried, and calcined to obtain alumina particles with a hollow structure.
[0014] By adopting the above technical solution, the preparation process of alumina particles is optimized, and a hollow structure constructed by nanosheets with a macroporous structure can be obtained. The presence of the nanosheet structure can improve the bonding effect between the alumina particles and the base film, that is, the base film obtains a long-lasting wear-resistant effect.
[0015] Optionally, the filler further includes mica powder, and the mica powder is loaded on the alumina particles.
[0016] By adopting the above technical solution, the mica powder has a lamellar structure and can form a shielding layer in the base film, so that the base film obtains better thermal stability and barrier properties. At the same time, since the mica powder has a certain conductivity, it can be suspended and floated under the action of the electric field, and then a shielding and barrier layer can be formed on the surface of the base film. Since the mica powder is loaded on the alumina particles, the hollow structure and porous structure of the alumina particles are conducive to the loading of the mica powder. Under the action of the external electric field, the alumina particles can be suspended and floated driven by the mica powder, which fully improves the dispersion effect of the filler in the base film, so that the base film obtains uniform wear resistance. In addition, the mica powder dispersed around the alumina particles can also fully form a shielding layer.
[0017] Optionally, the aluminum oxide particles are coated with chitosan.
[0018] By adopting the above technical scheme, the alumina particles are wrapped with chitosan. On the one hand, the bonding effect between the mica powder and the alumina particles can be improved, so that the mica powder can drive the alumina particles to suspend and float under the action of an external electric field, so that the base film obtains uniform wear resistance; on the other hand, chitosan can wrap the edges and corners of the hollow alumina particles and the edges and corners of the mica powder layer, reducing the possibility of the sharp edges and corners of the alumina particles being exposed on the surface of the base film, and can further improve the bonding effect between the alumina particles and the base film, and between the alumina particles and the mica powder, so that the base film obtains uniform mechanical properties and wear resistance.
[0019] Optionally, the filler also includes any one of nano calcium carbonate, nano silicon dioxide and barium sulfate.
[0020] By adopting the above technical scheme, nano calcium carbonate can promote heterogeneous nucleation of PET and absorb the heat energy of decomposition of PET molecular chain, effectively improving the mechanical properties and thermal stability of PET base film. Silicon dioxide can also promote heterogeneous nucleation of PET, and realize the filling of PET, effectively improving the mechanical properties of PET base film. Nano barium sulfate can shorten the nucleation time of PET and improve the mechanical strength of base film. Therefore, adopting nano calcium carbonate, nano silicon dioxide or nano barium sulfate as filler can effectively improve the mechanical properties of base film, and is conducive to the reuse of transfer film.
[0021] In a second aspect, the present application provides a method for preparing a wear-resistant PET transfer film, using the following technical solution: A method for preparing a wear-resistant PET transfer film comprises the following steps: S1. Preparation of PET base film: ethylene glycol, terephthalic acid, a catalyst and an auxiliary agent are mixed and pulped, and an esterification reaction is carried out to obtain a composite material. Under vacuum conditions, fillers are added to the composite material, and the mixture is stirred, discharged, extruded and stretched to obtain a PET base film.
[0022] S2. Preparation of transfer film: a coating layer, a glue layer and an aluminum foil layer are sequentially arranged on a PET base film to obtain a transfer film.
[0023] Optionally, in step S1, an electric field is applied to the composite material, and the field strength of the applied electric field is 5×10 5 -15×10 5 V / m.
[0024] By adopting the above technical solution, by applying an electric field treatment outside the composite material, the conductive filler can be organized under the action of the electric field force, suspended under the action of the electric field and partially floated to the surface of the composite material, further improving the uniformity of the dispersion of the filler in the base film, so that the base film obtains uniform wear resistance and mechanical strength; and the filler floating on the surface of the composite material can fully play the role of supporting load, lubricating, filling, etc. on the surface of the base film, effectively improving the wear resistance of the base film surface. In addition, after the treatment of the external electric field, the possibility of sedimentation and agglomeration of the filler in the base film can be reduced, so that the side of the base film close to the coating layer can have a relatively flat surface, which is conducive to maintaining the integrity of the coating layer.
[0025] Optionally, the side of the PET base film away from the coating layer is plasma treated.
[0026] By adopting the above technical solution, by plasma treatment on the surface of the PET base film, a micro-nano hierarchical rough structure can be constructed on the surface of the PET base film, which can effectively improve the hydrophobic effect of the PET base film, thereby reducing the possibility of dust accumulation on the PET base film, which is conducive to the recycling of the PET base film. It can also improve the bonding effect between the PET base film and the coating layer, and improve the use effect of the transfer film.
[0027] In summary, this application has the following beneficial effects: 1. Since the present application uses PEG or silane coupling agent to modify the alumina particles, the alumina particles can undergo hydroxylation and dehydration reaction with the modifier, so that the surface of the alumina particles is coated with a modifier layer, which reduces the possibility of agglomeration of the alumina particles, and effectively improves the compatibility between the alumina particles and PET, reduces the possibility of the alumina particles detaching from PET and staying on the friction dual surface, and enables the PET base film to obtain uniform and excellent wear resistance.
[0028] 2. In the present application, hollow alumina particles are preferably used as fillers, which can effectively reduce the mass of the alumina particles and appropriately increase the volume of the alumina particles, which is beneficial to reduce the surface polarity of the alumina particles, improve the dispersibility of the alumina particles in the base film, and reduce the possibility of alumina particles settling in the base film, so that the base film obtains a uniform and stable wear-resistant effect, thereby extending the service life of the base film.
[0029] 3. In this application, since the mica powder is loaded on the alumina particles, the hollow structure and porous structure of the alumina particles are conducive to the loading of the mica powder. Under the action of the external electric field, the alumina particles can be suspended and floated under the drive of the mica powder, which fully improves the dispersion effect of the filler in the base film and enables the base film to obtain uniform wear resistance. In addition, the mica powder dispersed around the alumina particles can also fully form a shielding layer.
[0030] 4. By applying an electric field treatment outside the composite material, the conductive filler can be activated and suspended under the action of the electric field and partially floated to the surface of the composite material, further improving the uniformity of the dispersion of the filler in the base film, so that the base film can obtain uniform wear resistance and mechanical strength; and the filler floating on the surface of the composite material can fully support the load, lubricate, fill, etc. on the surface of the base film, effectively improving the wear resistance of the base film surface. In addition, after the treatment of the external electric field, the possibility of sedimentation and agglomeration of the filler in the base film can be reduced, so that the side of the base film close to the coating layer can have a relatively flat surface, which is conducive to maintaining the integrity of the coating layer. DETAILED DESCRIPTION
[0031] The present application is further described in detail below in conjunction with embodiments.
[0032] Preparation Example: Alumina Particle Preparation Example Preparation Example 1: Add 50g of nano α-Al2O3 powder into 500mL of ethylene glycol and shear disperse for 2h. Put 5g of polyethylene glycol and 60mL of deionized water in a container, heat to 50℃ and stir until completely dissolved. Then mix the PEG solution in the Al2O3 dispersion, heat to about 65℃, rotate at 800r / min, stir at constant temperature for 3h, stop the reaction, filter and dry to obtain alumina particles.
[0033] Preparation Example 2: Add 50g of nano α-Al2O3 powder to 500mL of ethylene glycol and shear disperse for 2h, add 0.5ml of hydrochloric acid to 60mL of deionized water, adjust the pH to 3, add 2.5mL of silane coupling agent in a container and stir for 0.5h, then mix the KH-560 solution in the Al2O3 dispersion, heat to about 65°C, rotate at 800r / min, stir at constant temperature for 3h, stop the reaction, filter, and dry to obtain alumina particles.
[0034] Preparation Example 3: Mix potassium aluminum sulfate and urea in a mass ratio of 1:2 and dissolve in deionized water, stir vigorously at room temperature, heat to react at 180°C, filter, wash, retain the solid, dry at 80°C for 12h, and calcine at 600°C for 3h to obtain hollow structure alumina particles.
[0035] Add 50g of hollow alumina particles into 500mL of ethylene glycol and shear disperse for 2h, add 0.5ml of hydrochloric acid into 60mL of deionized water, adjust the pH to 3, add 2.5mL of silane coupling agent into the container and stir for 0.5h, then mix the KH-560 solution into the Al2O3 dispersion, heat to about 65℃, rotate at 800r / min, stir at constant temperature for 3h, stop the reaction, filter and dry to obtain alumina particles.
[0036] Preparation Example 4: Potassium aluminum sulfate and urea are mixed in a mass ratio of 1:2 and dissolved in deionized water, stirred vigorously at room temperature, heated to react at 180°C, filtered, washed, and the solids retained. The solids were dried at 80°C for 12 hours and calcined at 600°C for 3 hours to obtain hollow structured alumina particles.
[0037] Add 50g of hollow alumina particles into 500mL of ethylene glycol and shear disperse for 2h, add 0.5ml of hydrochloric acid into 60mL of deionized water, adjust the pH to 3, add 2.5mL of silane coupling agent and 2.5g of chitosan, stir in a container for 0.5h to obtain a mixed solution, mix the mixed solution with the Al2O3 dispersion, heat to about 65°C, rotate at 800r / min, stir at constant temperature for 3h, stop the reaction, filter, and dry to obtain alumina particles.
[0038] Embodiment 1, on the one hand, the present application provides a wear-resistant PET transfer film, comprising a PET base film, a coating layer, a glue layer and an aluminum foil layer arranged in sequence. The PET base film comprises the following raw materials: ethylene glycol, terephthalic acid, a catalyst, an additive and a filler, and the specific mass is shown in the table below.
[0039] Wherein, terephthalic acid is polymer-grade purified terephthalic acid, ethylene glycol is polymer-grade ethylene glycol, the catalyst is industrial-grade ethylene glycol antimony, the auxiliary agent includes trimethyl phosphate, and the filler is the alumina particles prepared in Preparation Example 1.
[0040] On the other hand, the present application provides a method for preparing a wear-resistant PET transfer film, comprising the following steps: S1. Preparation of PET base film: Ethylene glycol, terephthalic acid, catalyst and additives are mixed to make pulp, replaced with N2, stirred and heated in a 0.1MPa N2 atmosphere, the pressure in the autoclave is adjusted to 0.3MPa, and the reaction temperature is 220-260℃ for esterification reaction for 1.5h to obtain a composite material. Fillers are added to the composite material under vacuum conditions, stirred at a power of 300W, discharged, extruded and stretched to obtain a PET base film.
[0041] S2. Preparation of transfer film: a coating layer, a glue layer and an aluminum foil layer are sequentially arranged on a PET base film to obtain a transfer film.
[0042] The coating layer is formed by light-curing polyurethane coating, the adhesive layer is UV adhesive, and the aluminum foil layer is prepared by vacuum aluminum plating.
[0043] Table 1 Composition of Examples 1-3
[0044] Embodiment 2: On the one hand, the present application provides a wear-resistant PET transfer film, comprising a PET base film, a coating layer, a glue layer and an aluminum foil layer arranged in sequence. The PET base film comprises the following raw materials: ethylene glycol, terephthalic acid, a catalyst, an additive and a filler, and the specific mass is shown in Table 1.
[0045] Wherein, terephthalic acid is polymer-grade purified terephthalic acid, ethylene glycol is polymer-grade ethylene glycol, the catalyst is industrial-grade ethylene glycol antimony, the auxiliary agent includes trimethyl phosphate, and the filler is the alumina particles prepared in Preparation Example 1.
[0046] On the other hand, the present application provides a method for preparing a wear-resistant PET transfer film, comprising the following steps: S1. Preparation of PET base film: Ethylene glycol, terephthalic acid, catalyst and additives are mixed to make pulp, replaced with N2, stirred and heated in a 0.1MPa N2 atmosphere, the pressure in the autoclave is adjusted to 0.3MPa, and the reaction temperature is 220-260℃ for esterification reaction for 1.5h to obtain a composite material. Fillers are added to the composite material under vacuum conditions, stirred at a power of 300W, discharged, extruded and stretched to obtain a PET base film.
[0047] S2. Preparation of transfer film: a coating layer, a glue layer and an aluminum foil layer are sequentially arranged on a PET base film to obtain a transfer film.
[0048] The coating layer is formed by light-curing polyurethane coating, the adhesive layer is UV adhesive, and the aluminum foil layer is prepared by vacuum aluminum plating.
[0049] Embodiment 3: On the one hand, the present application provides a wear-resistant PET transfer film, comprising a PET base film, a coating layer, a glue layer and an aluminum foil layer arranged in sequence. The PET base film comprises the following raw materials: ethylene glycol, terephthalic acid, a catalyst, an additive and a filler, and the specific mass is shown in Table 1.
[0050] Wherein, terephthalic acid is polymer-grade purified terephthalic acid, ethylene glycol is polymer-grade ethylene glycol, the catalyst is industrial-grade ethylene glycol antimony, the auxiliary agent includes trimethyl phosphate, and the filler is the alumina particles prepared in Preparation Example 1.
[0051] On the other hand, the present application provides a method for preparing a wear-resistant PET transfer film, comprising the following steps: S1. Preparation of PET base film: Ethylene glycol, terephthalic acid, catalyst and additives are mixed to make pulp, replaced with N2, stirred and heated in a 0.1MPa N2 atmosphere, the pressure in the autoclave is adjusted to 0.3MPa, and the reaction temperature is 220-260℃ for esterification reaction for 1.5h to obtain a composite material. Fillers are added to the composite material under vacuum conditions, stirred at a power of 300W, discharged, extruded and stretched to obtain a PET base film.
[0052] S2. Preparation of transfer film: a coating layer, a glue layer and an aluminum foil layer are sequentially arranged on a PET base film to obtain a transfer film.
[0053] The coating layer is formed by light-curing polyurethane coating, the adhesive layer is UV adhesive, and the aluminum foil layer is prepared by vacuum aluminum plating.
[0054] Example 4: The difference from Example 2 is that the filler is the aluminum oxide particles prepared in Preparation Example 2, which replaces the filler in Example 2 to prepare the PET base film and the transfer film.
[0055] Example 5: The difference from Example 2 is that the filler is the aluminum oxide particles prepared in Preparation Example 3, which replaces the filler in Example 2 to prepare the PET base film and the transfer film.
[0056] Example 6: The difference from Example 2 is that the filler is the aluminum oxide particles prepared in Preparation Example 4, which replaces the filler in Example 2 to prepare the PET base film and the transfer film.
[0057] Example 7: The difference from Example 2 is that the filler is the alumina particles and mica powder prepared in Preparation Example 3, which replace the filler in Example 2 to prepare the PET base film and the transfer film.
[0058] The preparation of the filler is as follows: Add 50g of hollow alumina particles into 500mL of ethylene glycol and shear disperse for 2h, add 0.5ml of hydrochloric acid into 60mL of deionized water, adjust the pH to 3, add 2.5mL of silane coupling agent and 20g of nano-mica powder, stir in a container for 0.5h to obtain a mixed solution, then mix the mixed solution with the Al2O3 dispersion, heat to about 65°C, rotate at 800r / min, stir at constant temperature for 3h, stop the reaction, filter, and dry to obtain alumina particles loaded with mica powder.
[0059] Embodiment 8: The difference from Embodiment 2 is that: The fillers are the alumina particles and mica powder prepared in Preparation Example 4, which are used to replace the fillers in Example 2 to prepare the PET base film and the transfer film.
[0060] The preparation of the filler is as follows: Add 50g of hollow alumina particles into 500mL of ethylene glycol and shear disperse for 2h, add 0.5ml of hydrochloric acid into 60mL of deionized water, adjust the pH to 3, add 2.5mL of silane coupling agent, 2.5g of chitosan and 20g of nano-mica powder, stir in a container for 0.5h to obtain a mixed solution, then mix the mixed solution with the Al2O3 dispersion, heat to about 65°C, rotate at 800r / min, stir at constant temperature for 3h, stop the reaction, filter, and dry to obtain alumina particles loaded with mica powder.
[0061] Embodiment 9: The difference from Embodiment 8 is that: The fillers are the alumina particles, mica powder and nano-calcium carbonate prepared in Preparation Example 4, which are used to replace the fillers in Example 2 to prepare the PET base film and the transfer film.
[0062] The mass ratio of alumina particles, mica powder and nano-calcium carbonate is 5:2:1, and the nano-calcium carbonate is calcium carbonate modified by a silane coupling agent.
[0063] Embodiment 10: The difference from Embodiment 8 is that: The present application provides a method for preparing a wear-resistant PET transfer film, comprising the following steps: S1. Preparation of PET base film: Ethylene glycol, terephthalic acid, catalyst and additives were mixed and slurried, replaced by N2, stirred and heated in a 0.1MPa N2 atmosphere, the pressure in the reactor was adjusted to 0.3MPa, the reaction temperature was 220-260℃, and the esterification reaction was carried out for 1.5h to obtain a composite material. Fillers were added to the composite material under vacuum conditions, stirred at a power of 300W, and an external electric field was applied with a field strength of 10×10 5 V / m, the electric field treatment time is 10 min, and the material is discharged, extruded, and stretched to obtain a PET base film.
[0064] Embodiment 11: The difference from Embodiment 2 is that: The present application provides a method for preparing a wear-resistant PET transfer film, comprising the following steps: S1. Preparation of PET base film: Ethylene glycol, terephthalic acid, catalyst and additives are mixed to make pulp, replaced with N2, stirred and heated in a 0.1MPa N2 atmosphere, the pressure in the autoclave is adjusted to 0.3MPa, and the reaction temperature is 220-260℃ for esterification reaction for 1.5h to obtain a composite material. Fillers are added to the composite material under vacuum conditions, stirred at a power of 300W, discharged, extruded and stretched to obtain a PET base film.
[0065] The PET base film is subjected to plasma treatment. The PET is placed in a plasma vacuum chamber. The PET film is subjected to low-temperature plasma treatment at an oxygen flow of 35 kPa, with a power of 140 W and a treatment time of 2 min to obtain a plasma-treated PET base film.
[0066] Comparative Example 1: This comparative example is different from Example 2 in that no filler is added in this comparative example.
[0067] Comparative Example 2: The difference between this comparative example and Example 3 is that nano-alumina is selected as the filler in this comparative example.
[0068] Performance testing: The performance of the PET base film is tested as follows: (1) Wear resistance test: refer to standard GB / T1768-2006, first clean the surface of the coating, record the mass at this time, add 500g weights to both ends of the abrasion tester, control the speed of the abrasion tester to rotate at 60r / min for 3min, record the mass at this time, repeat multiple times, take the average value, and calculate the weight loss rate.
[0069] (2) Tensile properties test: The transverse tensile properties are measured using the national standard GB / T 13022-1991 "Test method for tensile properties of plastic films".
[0070] Table 2 Performance test
[0071] Combining the performance test comparison in Table 2, we can find that: 1. By comparing Examples 1-3, Example 4 and Comparative Examples 1-2, it can be found that the weight loss rate of the PET base film prepared in Examples 1-3 is reduced and the tensile strength is improved. This shows that in the present application, the alumina particles are modified by PEG or a silane coupling agent, and the alumina particles can undergo a hydroxylation dehydration reaction with the modifier, so that the surface of the alumina particles is coated with a modifier layer, which reduces the possibility of agglomeration of the alumina particles, and effectively improves the compatibility between the alumina particles and PET, reduces the possibility of the alumina particles detaching from the PET and staying on the friction dual surface, and enables the PET base film to obtain uniform and excellent wear resistance.
[0072] 2. By comparing Example 5 with Example 2, it can be found that the weight loss rate of the PET base film prepared in Example 5 is reduced and the tensile strength is improved. This shows that the use of hollow alumina particles as fillers in the present application can effectively reduce the mass of the alumina particles and appropriately increase the volume of the alumina particles, which is beneficial to reduce the surface polarity of the alumina particles, improve the dispersibility of the alumina particles in the base film, and reduce the possibility of alumina particles settling in the base film, so that the base film obtains a uniform and stable wear-resistant effect and extends the service life of the base film.
[0073] 3. By comparing Examples 6-7 with Example 2, it can be found that the weight loss rate of the PET base film prepared in Examples 6-7 is reduced and the tensile strength is improved. This shows that in the present application, since the mica powder is loaded on the alumina particles, the hollow structure and porous structure of the alumina particles are conducive to the loading of the mica powder. Under the action of the external electric field, the alumina particles can be suspended and floated under the drive of the mica powder, which fully improves the dispersion effect of the filler in the base film and enables the base film to obtain uniform wear resistance.
[0074] 4. By comparing Example 6 and Example 8 with Example 2, it can be found that the weight loss rate of the PET base film prepared in Example 6 and Example 8 is reduced, and the tensile strength is improved. This shows that in the present application, the alumina particles are wrapped by chitosan. On the one hand, the bonding effect between the mica powder and the alumina particles can be improved, so that the mica powder can drive the alumina particles to suspend and float under the action of an external electric field, so that the base film obtains uniform wear resistance; on the other hand, chitosan can wrap the edges and corners of the hollow alumina particles and the edges and corners of the mica powder flakes, reducing the possibility of the sharp edges and corners of the alumina particles being exposed on the surface of the base film, and can further improve the bonding effect between the alumina particles and the base film, and between the alumina particles and the mica powder, so that the base film obtains uniform mechanical properties and wear resistance.
[0075] 5. By comparing Example 9, Example 11 with Example 2, it can be found that the weight loss rate of the PET base film prepared in Example 9 and Example 11 is reduced, and the tensile strength is improved, which shows that the nano calcium carbonate in the present application can promote PET heterogeneous nucleation and absorb the heat energy of PET molecular chain decomposition, effectively improving the mechanical properties and thermal stability of the PET base film. Plasma treatment can construct a micro-nano hierarchical rough structure on the surface of the PET base film, which can effectively improve the hydrophobic effect of the PET base film, thereby reducing the possibility of dust accumulation on the PET base film, which is conducive to the recycling of the PET base film.
[0076] 6. By comparing Example 10 with Example 8, it can be found that the weight loss rate of the PET base film prepared in Example 10 is reduced and the tensile strength is improved. This shows that in the present application, applying an electric field treatment to the outside of the composite material can make the filler with conductive properties plan and suspend under the action of the electric field force and partially float to the surface of the composite material, further improving the dispersion uniformity of the filler in the base film, so that the base film obtains uniform wear resistance and mechanical strength.
[0077] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.
Claims
1. A wear-resistant PET transfer film, characterized in that: It includes a PET base film, a coating layer, a glue layer and an aluminum foil layer which are arranged in sequence; The PET base film comprises the following raw materials in parts by weight: 40-42 parts of ethylene glycol; 80-90 parts of terephthalic acid; Catalyst 0.04-0.06 parts; Additives 0.02-0.03 parts; 1-2 parts of filler; The filler comprises aluminum oxide particles, and the aluminum oxide particles are aluminum oxide particles modified by a modifier, and the modifier is selected from PEG or a silane coupling agent.
2. The wear-resistant PET transfer film according to claim 1, characterized in that: The mass ratio of the modifier to the alumina particles is 1:10-20.
3. The wear-resistant PET transfer film according to claim 1, characterized in that: The aluminum oxide particles are hollow in structure.
4. The wear-resistant PET transfer film according to claim 2, characterized in that: The alumina particles are prepared as follows: potassium aluminum sulfate, urea and water are mixed, heated for reaction, filtered, washed, solids are retained, dried, and calcined to obtain alumina particles with a hollow structure.
5. The wear-resistant PET transfer film according to claim 4, characterized in that: The filler further comprises mica powder, and the mica powder is loaded on the alumina particles.
6. The wear-resistant PET transfer film according to claim 5, characterized in that: The aluminum oxide particles are coated with chitosan.
7. The wear-resistant PET transfer film according to claim 1, characterized in that: The filler also includes any one of nano calcium carbonate, nano silicon dioxide and barium sulfate.
8. The method for preparing a wear-resistant PET transfer film according to any one of claims 1 to 7, characterized in that: The following steps are involved: S1. Preparation of PET base film: ethylene glycol, terephthalic acid, a catalyst and an auxiliary agent are mixed and pulped, and an esterification reaction is performed to obtain a composite material. A filler is added to the composite material under vacuum conditions, and the composite material is stirred, discharged, extruded and stretched to obtain a PET base film; S2. Preparation of transfer film: a coating layer, a glue layer and an aluminum foil layer are sequentially arranged on a PET base film to obtain a transfer film.
9. The wear-resistant PET transfer film according to claim 8, characterized in that: In step S1, an electric field is applied to the composite material, and the field strength of the applied electric field is 5×10 5 -15×10 5 V / m.
10. The wear-resistant PET transfer film according to claim 9, characterized in that: The PET base film is plasma treated.
Citation Information
Patent Citations
Preparation method of alpha-Al2O3 cage-structure hollow microspheres
CN103232049A
Anti-shrinkage PET laser transfer film and preparation method thereof
CN115534553A
Heat-resistant environment-friendly plastic woven bag and preparation process thereof
CN115819821A
Silicone oil-based flexible heat-conducting composite material modified by chitosan and silane coupling agent and preparation method of silicone oil-based flexible heat-conducting composite material
CN116218231A
Polyester resin containing the nanoparticles and the preparing process thereof
KR1020130063679A
Cited By
Composite material and application thereof in preparation of high-transparency colorful color-changing anti-counterfeiting film
CN121736456A