Single-walled carbon nanotube dispersion liquid and preparation method of single-walled carbon nanotube
By using ammonium salt etchant and high-temperature carbon dioxide calcining technology, the problems of low G/D ratio of single-wall carbon nanotubes and difficult to remove iron oxide impurities are solved, and the preparation and performance improvement of high-quality carbon nanotubes are achieved.
Patent Information
- Application Number
- CN202411212261.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-11-22
AI Technical Summary
The Raman spectrum G/D ratio of existing single-wall carbon nanotube dispersions is low, which cannot meet the requirements of high-quality single-wall carbon nanotubes, and the iron oxide impurities generated during air calcination are difficult to completely remove.
The ammonium salt is used as the etching agent, and the G/D ratio is increased by etching amorphous carbon, and the iron oxide impurities are removed by calcining under high temperature conditions, and the metal impurities are completely removed by stirring in combination with hydrochloric acid or sulfuric acid.
The G/D ratio of single-wall carbon nanotubes is significantly improved, its structural and performance characteristics are optimized, conductive and mechanical properties are improved, and the preparation of high-quality carbon nanotubes is realized.
Smart Images

Figure CN118993041A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of lithium batteries, and in particular to a single-walled carbon nanotube dispersion and a method for preparing the single-walled carbon nanotube. Background Art
[0002] In the field of carbon-based nanomaterial research and development, the combined use of chemical vapor deposition and vertical tube furnaces is a common and mature production strategy. This method introduces carbon-containing ligand gas into the reactor and reacts with the catalyst at high temperature to form single-walled carbon nanotubes with outstanding characteristics such as lightness, pressure resistance, wear resistance, heat resistance, high strength and high modulus. Due to their unique properties, this type of single-walled carbon nanotube is widely used in the optimization of various metals and polymer materials, thereby obtaining high-quality materials with higher strength, resistance to lightning strikes, invisible properties or resistance to freezing at extremely low temperatures. Considering the physical properties of single-walled carbon nanotubes, they are also increasingly used in chip manufacturing, battery development, aerospace material design, plastics and rubber.
[0003] The G / D ratio of Raman spectroscopy has always been one of the important criteria for measuring the quality of single-walled carbon nanotube products. The higher the G / D ratio of Raman spectroscopy, the better the quality of the single-walled carbon nanotube product. However, the G / D ratio of single-walled carbon nanotubes obtained by the existing dispersion ratio is generally low, which cannot meet the requirements for high-quality single-walled carbon nanotube products. Summary of the invention
[0004] The present application is made in view of the above-mentioned problems. The present application provides a single-walled carbon nanotube dispersion and a method for preparing single-walled carbon nanotubes. The present invention aims to use different types of ammonium salt etchants to etch the amorphous carbon in the crude single-walled carbon nanotubes, so as to achieve the ultimate goal of reducing the peak area of D peak amorphous carbon and improving the GD ratio.
[0005] In addition, the present invention is to completely remove the iron oxide impurities generated during the air calcination process. This method is to introduce 1000-1500sccm of carbon dioxide (CO2) into the rough product in an environment of 1400-1600°C for calcination for 1-2h. Under high temperature conditions, a small amount of carbon dioxide will decompose into twice the carbon monoxide, which is more economical than the traditional direct input of carbon monoxide. Carbon monoxide will react with iron oxide impurities to generate metallic iron (Fe) and carbon dioxide (CO2), and carbon dioxide can be discharged as tail gas. In addition, compared with iron oxide, metallic iron is easier to remove in hydrochloric acid (HCl) or sulfuric acid (H2SO4) solution. Iron oxide is not easily dissolved by hydrochloric acid due to its higher stability. Even in a strong acid environment, iron oxide may react to a certain extent, but due to the slow reaction rate, it affects the speed and effect of removing metal impurities in single-walled carbon nanotubes.
[0006] In the process of preparing single-walled carbon nanotubes, the ammonium salt is used as an etchant to not only improve the GD ratio (G / D ratio) of the single-walled carbon nanotubes by etching amorphous carbon, but also because the ammonium salt etchant has a certain acidity, its stronger etching effect further promotes the formation of single-walled carbon nanotubes and significantly improves the GD ratio. This not only optimizes the structure of the carbon nanotubes and enhances their performance characteristics such as conductivity and mechanical properties, but also considers the etching effect of the etchant on amorphous carbon and the comprehensive influence on the structure and performance of the carbon nanotubes when selecting the etchant, thereby achieving further improvement of the quality of the carbon nanotubes.
[0007] The first aspect of the present application provides a single-walled carbon nanotube dispersion, which includes a carbon source, a metal compound catalyst, a co-catalyst of a compound that helps to supply a sulfur source, and an ammonium salt etchant, which together form a dispersion.
[0008] In any embodiment, the metal compound is one or more of ferric chloride, ferric sulfide, ferric acetate and ferrocene; the co-catalyst is one or more of thiophenol, ethanethiol and selenophene; and the carbon source is toluene.
[0009] The present invention uses toluene, which has a higher solubility for metal compound solids, as a solvent to prepare single-walled carbon nanotubes by a floating catalytic method, so as to reduce the influence of liquid volatility factors on low product yield and poor quality.
[0010] Toluene, which has a higher solubility of metal compounds in solid form, can carry more catalysts into the reaction system, so the output can be greatly improved. The study found that there are benzene rings in toluene. During the experimental process of checking the Raman standard spectrum, it was found that the benzene rings provide a carbon source, which will lead to the production of carbon impurity graphite, resulting in a serious decrease in the average GD ratio of batch output products. Ethanol catalysts can produce fewer carbon impurities, but the production rate is relatively slow because the solubility of metal compounds in ethanol is relatively low, and ethanol can only carry less catalyst into the reaction system. Even if the dispersion prepared by ethanol solvent is injected into the tubular furnace at a rate approximately three times that of toluene solvent, the insufficient carbon source content of ethanol itself leads to a slower production rate, and the product is less per unit time. Therefore, the present application creatively uses the two in a compounded manner, and studies the effects of the compounding ratio and injection rate on the yield and product quality.
[0011] In any embodiment, the ammonium salt is one or more of ammonium sulfate, ammonium chloride, ammonium phosphate and ammonium acetate.
[0012] In any embodiment, the metal compound, liquid carbon source, promoter and ammonium salt etchant are used in a ratio of 1-5 g: 50-200 mL: 1-6 mL: 0.5-0.6 g.
[0013] Metal compounds have higher solubility in toluene solvent; toluene, which has higher solubility of metal compounds in solid form, can carry more catalysts into the reaction system, so the yield can be greatly increased. However, there are benzene rings in toluene. During the experimental process of checking the Raman standard spectrum, it was found that if too much toluene is added, too many benzene rings provide a carbon source, which will lead to the production of carbon impurity graphite, so the average GD ratio of batch output products will be seriously reduced. Ethanol catalysts can produce fewer carbon impurities, but the production rate is relatively slow because the solubility of metal compounds in ethanol is low, and ethanol can only carry a small amount of catalyst into the reaction system. If too much ethanol is added, the yield will drop significantly.
[0014] Adding too much co-catalyst will result in an excessively high sulfur content in the system, with the sulfur wrapping around the outside of the iron atom cluster, causing the catalyst to deactivate.
[0015] The G / D ratio of Raman spectrum has always been one of the important criteria for measuring the quality of single-walled carbon nanotube products. The higher the G / D ratio of Raman spectrum, the better the product quality of single-walled carbon nanotubes. Adding too little etchant will lead to a high content of amorphous carbon. Although adding too much etchant will etch more amorphous carbon and reduce the peak area of D peak in Raman spectrum, it will also etch more graphite carbon, so the intensity of its G peak will decrease more seriously, and the GD ratio will still be low.
[0016] The second aspect of the present application also provides a single-walled carbon nanotube dispersion and a method for preparing single-walled carbon nanotubes, comprising the following steps: 1) a liquid carbon source, an iron source, a sulfur source and an etchant are mixed to form a dispersion; 2) the dispersion is input through the top of a high-temperature furnace, and under the action of reducing gas and protective gas, a floating catalytic method is used to generate single-walled carbon nanotubes, and the crude product is deposited at the bottom of the high-temperature furnace and in a collection tank; 3) the crude product needs to be purified to obtain pure and high-quality single-walled carbon nanotubes.
[0017] In any embodiment, before adding the liquid feed in step 2), the dispersion is continuously heated to 100° C. and stirred.
[0018] Too low a temperature will slow down the dissolution of solids in the solvent, lead to insufficient solubility of metal compounds in the carbon source solvent, and result in low catalyst dispersion. Higher temperatures will lead to faster evaporation of the solvent, increase the volatility of the liquid carbon source, and may lead to safety hazards, especially in poorly ventilated conditions.
[0019] In any embodiment, in step 2), the ratio of reducing gas to protective gas is 1000-8000:4000 sccm.
[0020] In any embodiment, the injection rate of the feed liquid in step 2) is 120-150 μL / min.
[0021] Too fast an injection rate will lead to a significant increase in production, while a slower injection rate will improve the stability of the product Raman value. At the same time, a faster liquid feed rate is often accompanied by a larger gas flow rate.
[0022] In any embodiment, in step 2), the temperature of the furnace tube of the high temperature furnace is 1200-1250°C.
[0023] According to the iron-carbon alloy phase diagram, the maximum solubility of carbon in austenite is about 2.11% when the temperature is maintained at 1148°C. (Austenite is the interstitial solid solution of C in γ-Fe, with a solubility from 0 to 2.11%. At 912°C on the phase diagram, pure iron undergoes an allotropic transformation from α-Fe to γ-Fe, called the A3 transformation, and from a body-centered cubic structure to a face-centered cubic structure.) However, in actual experiments, it was found that a higher temperature is often required to significantly increase the yield of single-walled carbon nanotubes. At 1180°C, the yield using the same formula is twice that at 1150°C. By experimentally obtaining 1200-1250°C, more single-walled carbon nanotubes will be produced.
[0024] In any embodiment, in step 3), the crude product is calcined in air at a high temperature of 1200-1600°C.
[0025] In any embodiment, after calcination in step 3), calcination is continued at 1400-1600° C. by introducing 1000-1500 sccm of carbon dioxide (CO 2 ) for 1-2 h.
[0026] In this temperature range, calcination can effectively remove some organic and metal impurities on the surface of carbon nanotubes; it helps to improve the mechanical properties of carbon nanotubes because high temperature can promote the arrangement and structural optimization of carbon nanotubes. The calcination process can also increase the conductivity of carbon nanotubes.
[0027] Too high a temperature may cause damage to the carbon nanotube structure. Thermal decomposition at high temperatures may destroy the tubular structure of carbon nanotubes, leading to degradation of the carbon nanotube morphology. It may cause more defects to form on the surface of carbon nanotubes, thereby reducing their electrical and mechanical properties. High temperatures may also cause agglomeration between carbon nanotubes, affecting their dispersibility and application performance.
[0028] If the temperature is too low, surface impurities and catalysts may not be completely removed, affecting the purity of carbon nanotubes. If the temperature is too low, the morphology of carbon nanotubes may be poorly developed, such as uneven tube diameter or more defects. Calcination time at low temperature may take longer, resulting in increased costs and reduced production efficiency.
[0029] In any embodiment, in the air calcination, the time for exposing the crude product to oxygen is 1-2 hours (excluding the time for heating and cooling), and the heating rate is 10°C / min.
[0030] A heating rate that is too slow will shorten the production time and greatly affect the progress of industrial mass production. A heating rate that is too fast will cause the temperature inside the furnace to be unstable, fluctuating, affecting the output and deposition of the product.
[0031] Too high an oxygen content may reduce the thermal stability of carbon nanotubes, making them susceptible to oxidation reactions in high temperature environments, thereby reducing the stability and durability of their structure. It may also accelerate the corrosion of graphite carbon in carbon nanotubes, resulting in poor product quality. Too low an oxygen content may make it impossible to effectively purify carbon nanotubes, and residual impurities may affect their performance and applications. Too low an oxygen content may result in insufficient removal of amorphous carbon in carbon nanotubes.
[0032] In any embodiment, after the calcination treatment in step 3), hydrochloric acid (HCl) or sulfuric acid (H2SO4) solution is added, the temperature is controlled at 50-70°C, and stirred for 5-10 hours.
[0033] Too high agitation temperature may lead to faster evaporation of the pickling solution, which may increase the concentration of the acid solution and cause excessive corrosion to the treated material. Too low agitation temperature may lead to too slow pickling reaction rate, prolong the treatment time, increase cost and resource consumption. It may make it difficult for the material to fully contact with the treatment solution in a low temperature environment, affecting the purification effect.
[0034] Beneficial effects of the present invention: In the process of preparing single-walled carbon nanotubes, the present invention uses ammonium salt as an etchant, which has certain acidity and stronger etching strength, so that the growth process and morphology of carbon nanotubes can be regulated. In addition, when selecting the etchant, the etching effect on amorphous carbon and the comprehensive influence on the structure and performance of carbon nanotubes are considered, and the GD ratio of single-walled carbon nanotubes is improved by etching amorphous carbon, thereby achieving the preparation of high-quality carbon nanotubes. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Figure 1 A diagram of a single-walled carbon nanotube preparation device according to an embodiment of the present application;
[0036] Figure 2 The scanning electron microscope (SEM) and Raman images (Raman) of the purified single-walled carbon nanotubes (SWCNT) in Example 1 of the present application;
[0037] Figure 3 The scanning electron microscope (SEM) and Raman images (Raman) of the purified single-walled carbon nanotubes (SWCNT) in Example 2;
[0038] Figure 4 The scanning electron microscope (SEM) and Raman images (Raman) of the purified single-walled carbon nanotubes (SWCNT) in Example 3;
[0039] Figure 5 The scanning electron microscope (SEM) and Raman images (Raman) of the purified single-walled carbon nanotubes (SWCNT) in Example 4;
[0040] Figure 6 The scanning electron microscope (SEM) and Raman images (Raman) of the purified single-walled carbon nanotubes (SWCNT) in Comparative Example 1;
[0041] Figure 7 The scanning electron microscope (SEM) and Raman images (Raman) of the purified single-walled carbon nanotubes (SWCNT) of Comparative Example 2;
[0042] Figure 8 The scanning electron microscope (SEM) and Raman images of the purified single-walled carbon nanotubes (SWCNT) in Comparative Example 3 are shown.
[0043] Fig. 9 The scanning electron microscope (SEM) and Raman images of the purified single-walled carbon nanotubes (SWCNT) of Comparative Example 4 are shown.
[0044] Fig.10 The scanning electron microscope (SEM) and Raman images (Raman) of the purified single-walled carbon nanotubes (SWCNT) in Comparative Example 5 are shown.
[0045] Fig.11 The scanning electron microscope (SEM) and Raman images (Raman) of the purified single-walled carbon nanotubes (SWCNT) of Comparative Example 6 are shown. DETAILED DESCRIPTION
[0046] Hereinafter, an embodiment of a single-walled carbon nanotube dispersion and a method for preparing single-walled carbon nanotubes of the present application will be specifically disclosed in detail with appropriate reference to the accompanying drawings. However, there may be cases where unnecessary detailed descriptions are omitted. For example, there may be cases where detailed descriptions of well-known matters and repeated descriptions of actually the same structures are omitted. This is to avoid the following description from becoming unnecessarily lengthy and to facilitate understanding by those skilled in the art. In addition, the drawings and the following description are provided for those skilled in the art to fully understand the present application and are not intended to limit the subject matter described in the claims.
[0047] "Scope" disclosed in the present application is limited in the form of lower limit and upper limit, and a given range is limited by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundary of a special range. The scope limited in this way can be including end values or not including end values, and can be arbitrarily combined, that is, any lower limit can be combined with any upper limit to form a scope. For example, if the scope of 60-120 and 80-110 is listed for a specific parameter, it is understood that the scope of 60-110 and 80-120 is also expected. In addition, if the minimum range values 1 and 2 are listed, and if the maximum range values 3, 4 and 5 are listed, the following scope can be all expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5. In the present application, unless otherwise specified, the numerical range "ab" represents the abbreviation of any real number combination between a and b, wherein a and b are real numbers. For example, the numerical range "0-5" means that all real numbers between "0-5" are listed in this document, and "0-5" is just an abbreviation of these numerical combinations. In addition, when a parameter is expressed as an integer ≥ 2, it is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.
[0048] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.
[0049] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.
[0050] If there is no special explanation, all steps of the present application can be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), which means that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), which means that step (c) may be added to the method in any order. For example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.
[0051] If there is no special explanation, the "include" and "comprising" mentioned in this application are open-ended or closed-ended. For example, the "include" and "comprising" may mean that other components not listed may also be included or only the listed components may be included or only the listed components may be included.
[0052] If not specifically stated, in this application, the term "or" is inclusive. For example, the phrase "A or B" means "A, B, or both A and B". More specifically, any of the following conditions satisfies the condition "A or B": A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).
[0053] A single-walled carbon nanotube dispersion and a method for preparing single-walled carbon nanotubes. First, a liquid carbon source, an iron source, a sulfur source and an etchant are mixed to form a dispersion. Secondly, the dispersion is input through the top of a high-temperature furnace, and under the action of reducing gas and protective gas, a floating catalytic method is used to generate single-walled carbon nanotubes, and the crude product is deposited at the bottom of the high-temperature furnace and in a collection tank. Finally, the crude product needs to be purified, including high-temperature calcination with carbon dioxide to remove amorphous carbon to increase the degree of graphitization, and strong acid stirring is used to remove metal impurities and other impurities, thereby obtaining pure and high-quality single-walled carbon nanotubes.
[0054] The specific experimental process is as follows:
[0055] Experimental steps:
[0056] Mix 1-5g of metal compound, 50-200mL of liquid carbon source, 1-6mL of promoter and 0.5g of ammonium salt etchant in this ratio. Next, use 1000-8000sccm of ethylene reducing gas and 4000sccm of argon shielding gas to inject into the mixing tank for heating to achieve and maintain the optimal temperature and pressure values. Then, open the outlet valve of the mixing tank to allow the mixed gas to enter the furnace tube. Use a flow rate of 120-150μL / min to introduce the dispersion into a high-temperature furnace of 1180-1200℃, and take a sample every 30min. The reason for this is that the generated single-walled carbon nanotubes are mainly deposited at the top of the furnace tube and inside the collection tank, and their temperature is relatively mild relative to the position in the reactor. Generally speaking, the generation temperature of single-walled carbon nanotubes is 1150-1250℃, but the deposition temperature needs to be lower, about 500-850℃. If sampling is not done in time, the product will continue to deposit in the high temperature area, causing the product to become fragile. Therefore, in order to avoid excessive carbon nanotubes accumulating in the high temperature area for a long time and causing the quality of single-walled carbon nanotubes to decrease, it is recommended to take samples every half an hour.
[0057] Adding too little ammonium salt etchant will result in a high content of amorphous carbon. Although adding too much etchant will etch more amorphous carbon and reduce the D peak area in the Raman spectrum, it will also etch more graphite carbon, causing the intensity of its G peak to decrease more seriously, and the GD ratio will still be low.
[0058] First, the crude product is placed in a high temperature environment of 1400-1600℃ for 1-2h of air calcination. The main goal of this process is to eliminate surface amorphous carbon and improve the graphitization level of the product. At this stage, the oxygen in the air plays the role of an oxidant, oxidizing the amorphous carbon into carbon dioxide (CO2) or carbon monoxide (CO), which are immediately discharged to achieve the removal of amorphous carbon. At the same time, the calcination process will also remove amorphous carbon impurities in the form of particles or flakes, thereby exposing a larger surface area, so that the area ratio of the G peak to the D peak (GD ratio) in the Raman test is greater than 90. Subsequently, in order to eliminate the iron oxide impurities generated during the air calcination process, the original product is calcined for another 1-2h at the same high temperature of 1400-1600℃ with a carbon dioxide flow rate of 1000-1500sccm. At this stage, iron oxide and carbon monoxide will react to generate metallic iron (Fe) and carbon dioxide (CO2), and the generated carbon dioxide can be recycled in the purification process of single-walled carbon nanotubes. Next, we immerse the crude product in a 3-5M hydrochloric acid (HCl) or sulfuric acid (H2SO4) solution and stir it at 50-70°C for 5-10h. This step can effectively remove iron (Fe). It should be noted that since iron oxide (FeO2 or Fe2O3) has high stability and is not easy to react with hydrochloric acid, its reaction rate is slow, which may affect the removal efficiency of metal impurities. However, through the previous carbon monoxide reduction step, we have converted iron oxide into elemental iron, which greatly speeds up the metal removal speed and effect in the subsequent pickling process.
[0059] Example
[0060] Hereinafter, the embodiments of the present application will be described. The embodiments described below are exemplary and are only used to explain the present application, and should not be construed as limiting the present application. If no specific techniques or conditions are indicated in the embodiments, the techniques or conditions described in the literature in this area or the product specifications are used. If the manufacturer is not indicated in the reagents or instruments used, they are all conventional products that can be obtained commercially.
[0061] Embodiment 1:
[0062] Mix 5g of ferric chloride, 200mL of toluene, 6mL of thiophenol and 0.5g of ammonium phosphate in the specified proportion. Then, 8000sccm of ethylene reducing gas and 4000sccm of argon shielding gas are injected into the mixing tank simultaneously and heated to reach and maintain the appropriate temperature and pressure. After that, open the gas outlet valve of the mixing tank to allow the mixed gas to enter the furnace tube. Next, introduce the dispersion into a high-temperature furnace at 1180 to 1200℃ at a rate of 150μL / min. Take samples every 30min. The above steps and parameters must be strictly followed, and any changes may affect the experimental results.
[0063] In the first step, the crude product is calcined in a 1400°C environment, and this process lasts for 2 hours. In this process, the amorphous carbon on the surface of the product reacts with oxygen (O) in the air, is oxidized to carbon dioxide (CO2) or carbon monoxide (CO) by high temperature, and is immediately discharged. This process also removes carbon (C) impurities, so that the graphitization level of the product is improved, and the GD ratio of the Raman test is also greater than 90. In the second step, under the same temperature conditions, the present invention uses a carbon dioxide (CO2) flow rate of 1000sccm to calcine the product again, and this process also lasts for 2 hours. At this stage, the generated iron oxide (FeO) impurities react with carbon monoxide (CO) to produce iron (Fe) and carbon dioxide (CO2). The newly generated CO2 can be reused in the purification process of single-walled carbon nanotubes. In the third step, the treated crude product is immersed in a 5M hydrochloric acid (HCl) or sulfuric acid (H2SO4) solution and stirred for 10 hours. The temperature of the whole process is controlled at 70°C. This step can completely remove iron (Fe) to obtain a purified product.
[0064] After weighing and Raman testing, it was found that in Example 1, a machine with a 1m long and 60mm diameter tube could produce 2.36g of single-wall net product in 6 hours, and the Raman G / D was as high as 268.8.
[0065] Embodiment 2:
[0066] Mix 5g of ferric chloride, 200mL of toluene, 6mL of thiophenol and 0.5g of ammonium chloride in the specified proportion. Then, 8000sccm of ethylene reducing gas and 4000sccm of argon shielding gas are injected into the mixing tank simultaneously and heated to reach and maintain the appropriate temperature and pressure. Next, the dispersion is introduced into a high-temperature furnace at 1180 to 1200℃ at a rate of 150μL / min. Samples are taken every 30min. The above steps and parameters must be strictly followed, and any changes may affect the experimental results.
[0067] In the first step, the crude product is calcined in a 1400°C environment, and this process lasts for 2 hours. In this process, the amorphous carbon on the surface of the product reacts with oxygen (O) in the air, is oxidized to carbon dioxide (CO2) or carbon monoxide (CO) by high temperature, and is immediately discharged. This process also removes carbon (C) impurities, so that the graphitization level of the product is improved, and the GD ratio of the Raman test is also greater than 90. In the second step, under the same temperature conditions, the present invention uses a carbon dioxide (CO2) flow rate of 1000sccm to calcine the product again, and this process also lasts for 2 hours. At this stage, the generated iron oxide (FeO) impurities react with carbon monoxide (CO) to produce iron (Fe) and carbon dioxide (CO2). The newly generated CO2 can be reused in the purification process of single-walled carbon nanotubes. In the third step, the treated crude product is immersed in a 5M hydrochloric acid (HCl) or sulfuric acid (H2SO4) solution and stirred for 10 hours. The temperature of the whole process is controlled at 70°C. This step can completely remove iron (Fe) to obtain a purified product.
[0068] After weighing and Raman testing, it was found that in Example 1, a machine with a 1m long and 60mm diameter tube could produce 2.16g of single-wall net product in 6 hours, and the Raman G / D was as high as 381.0.
[0069] Embodiment 3:
[0070] Mix 5g of ferric chloride, 200mL of toluene, 6mL of thiophenol and 0.5g of ammonium sulfate in the specified proportion. Then, 8000sccm of ethylene reducing gas and 4000sccm of argon shielding gas are injected into the mixing tank simultaneously and heated to reach and maintain the appropriate temperature and pressure. After that, open the gas outlet valve of the mixing tank to allow the mixed gas to enter the furnace tube. Next, introduce the dispersion into a high-temperature furnace at 1180 to 1200℃ at a rate of 150μL / min. Take samples every 30min. The above steps and parameters must be strictly followed, and any changes may affect the experimental results.
[0071] In the first step, the crude product is calcined in a 1400°C environment, and this process lasts for 2 hours. In this process, the amorphous carbon on the surface of the product reacts with oxygen (O) in the air, is oxidized to carbon dioxide (CO2) or carbon monoxide (CO) by high temperature, and is immediately discharged. This process also removes carbon (C) impurities, so that the graphitization level of the product is improved, and the GD ratio of the Raman test is also greater than 90. In the second step, under the same temperature conditions, the present invention uses a carbon dioxide (CO2) flow rate of 1000sccm to calcine the product again, and this process also lasts for 2 hours. At this stage, the generated iron oxide (FeO) impurities react with carbon monoxide (CO) to produce iron (Fe) and carbon dioxide (CO2). The newly generated CO2 can be reused in the purification process of single-walled carbon nanotubes. In the third step, the treated crude product is immersed in a 5M hydrochloric acid (HCl) or sulfuric acid (H2SO4) solution and stirred for 10 hours. The temperature of the whole process is controlled at 70°C. This step can completely remove iron (Fe) to obtain a purified product.
[0072] After weighing and Raman testing, it was found that in Example 1, a machine with a 1m long and 60mm diameter tube could produce 1.98g of single-wall net product in 6 hours, and the Raman G / D was as high as 496.7.
[0073] Embodiment 4:
[0074] Mix 5g of ferric chloride, 200mL of toluene, 6mL of thiophenol and 0.5g of ammonium acetate in the specified proportion. Then, 8000sccm of ethylene reducing gas and 4000sccm of argon shielding gas are injected into the mixing tank simultaneously and heated to reach and maintain the appropriate temperature and pressure. After that, open the gas outlet valve of the mixing tank to allow the mixed gas to enter the furnace tube. Next, introduce the dispersion into a high-temperature furnace at 1180 to 1200℃ at a rate of 150μL / min. Take samples every 30min. The above steps and parameters must be strictly followed, and any changes may affect the experimental results.
[0075] In the first step, the crude product is calcined in a 1400°C environment, and this process lasts for 2 hours. In this process, the amorphous carbon on the surface of the product reacts with oxygen (O) in the air, is oxidized to carbon dioxide (CO2) or carbon monoxide (CO) by high temperature, and is immediately discharged. This process also removes carbon (C) impurities, so that the graphitization level of the product is improved, and the GD ratio of the Raman test is also greater than 90. In the second step, under the same temperature conditions, the present invention uses a carbon dioxide (CO2) flow rate of 1000sccm to calcine the product again, and this process also lasts for 2 hours. At this stage, the generated iron oxide (FeO) impurities react with carbon monoxide (CO) to produce iron (Fe) and carbon dioxide (CO2). The newly generated CO2 can be reused in the purification process of single-walled carbon nanotubes. In the third step, the treated crude product is immersed in a 5M hydrochloric acid (HCl) or sulfuric acid (H2SO4) solution and stirred for 10 hours. The temperature of the whole process is controlled at 70°C. This step can completely remove iron (Fe) to obtain a purified product.
[0076] After weighing and Raman testing, it was found that in Example 1, a machine with a 1m long and 60mm diameter tube could produce 2.03g of single-wall net product in 6 hours, and the Raman G / D was as high as 245.9.
[0077] Comparative Example 1:
[0078] The scheme of comparative example 1 is the same as the method of embodiment 1, except that no ammonium salt etchant is added.
[0079] After weighing and Raman testing, it was found that the comparative example 1 solution could produce 2.40g of single-walled net product in 6 hours, and the Raman G / D was 83.5.
[0080] Comparative Example 2:
[0081] The scheme of Comparative Example 2 is the same as that of Example 1, except that 1 g of ammonium sulfate is added in the experimental scheme.
[0082] After weighing and Raman testing, it was found that the comparative example 2 solution could produce 1.90g of single-walled net product in 6 hours, and the Raman G / D was 81.1.
[0083] Comparative Example 3:
[0084] The scheme of comparative example 3 is the same as the method of embodiment 2, except that 1 g of ammonium chloride is added in the experimental scheme.
[0085] After weighing and Raman testing, it was found that the comparative example 1 solution could produce 1.86g of single-walled net product in 6 hours, and the Raman G / D was 121.3.
[0086] Comparative Example 4:
[0087] The scheme of comparative example 3 is the same as the method of example 2, except that 1 g of water is added in the experimental scheme.
[0088] After weighing and Raman testing, it was found that the comparative example 1 solution could produce 1.86g of single-walled net product in 6 hours, and the Raman G / D was 140.75.
[0089] Comparative Example 5:
[0090] The scheme of comparative example 3 is the same as the method of example 2, except that 1 g of ethylene glycol is added in the experimental scheme.
[0091] After weighing and Raman testing, it was found that the comparative example 1 solution could produce 1.86g of single-walled net product in 6 hours, and the Raman G / D was 148.5.
[0092] Comparative Example 6:
[0093] The scheme of comparative example 3 is the same as the method of example 2, except that 1 g of propylene glycol is added in the experimental scheme.
[0094] After weighing and Raman testing, it was found that the comparative example 1 solution could produce 1.86g of single-walled net product in 6 hours, and the Raman G / D was 173.56.
[0095] Through Examples 1-4 and the corresponding Figure 2-5 It can be concluded that as the number of ammonium salts corresponding to the types of ammonium salt etchants increases, the GD ratio of the single-walled carbon nanotubes in the corresponding experimental scheme gradually increases, but the corresponding single-walled carbon nanotube output gradually decreases. Therefore, in the process of producing single-walled carbon nanotubes, it is necessary to pay attention to the relevant requirements of product quality and output at the same time. In addition, the order of the acidity of the ammonium salt etchants in Examples 1-4 is roughly: ammonium sulfate> ammonium chloride> ammonium phosphate> ammonium acetate. The experimental results show that the stronger the acidity of the ammonium salt etchant, the better the etching effect on amorphous carbon.
[0096] For Comparative Example 1, although the output is increased without adding any ammonium salt etchant, the amorphous carbon content is increased compared to the single-walled carbon nanotube product produced by adding ammonium salt etchant. Specifically, the D peak value in the Raman data test chart is significantly increased, and the overall GD ratio shows a significant downward trend. Therefore, the present invention embodies the necessity and selectivity of adding ammonium salt etchant in the process of preparing single-walled carbon nanotubes.
[0097] After comparing Application Example 2 with Comparative Example 1 and comparing Example 3 with Comparative Example 2 and referring to Figure 5-8The Raman peaks shown indicate that when the amount of ammonium salt etchant added exceeds the range specified in the present invention, not only the yield of single-walled carbon nanotubes decreases, but also its GD ratio value decreases. This is because excessive ammonium salts reduce the amount of graphite carbon and produce more amorphous carbon. Therefore, the amount of ammonium salt etchant needs to be maintained within a certain range, and it is not suitable to add excessive amounts.
[0098] It should be noted that the present application is not limited to the above-mentioned embodiments. The above-mentioned embodiments are only examples, and the embodiments having the same structure as the technical idea and exerting the same effect within the scope of the technical solution of the present application are all included in the technical scope of the present application. In addition, without departing from the scope of the main purpose of the present application, various modifications that can be thought of by those skilled in the art to the embodiments and other methods of combining some of the constituent elements in the embodiments are also included in the scope of the present application.
Claims
1. A single-walled carbon nanotube dispersion, characterized in that: The method comprises a carbon source, a metal compound catalyst, a co-catalyst of a compound that helps to supply a sulfur source, and an ammonium salt etchant, which are mixed in a certain proportion to form a dispersion.
2. The single-walled carbon nanotube dispersion according to claim 1, characterized in that: The metal compound is one or more of ferric chloride, ferric sulfide, ferric acetate and ferrocene; the co-catalyst is one or more of thiophenol, ethanethiol and selenophene; and the carbon source is toluene.
3. The single-walled carbon nanotube dispersion according to claim 1, characterized in that: The ammonium salt is one or more of ammonium sulfate, ammonium chloride, ammonium phosphate and ammonium acetate.
4. The single-walled carbon nanotube dispersion according to claim 1, characterized in that: The usage ratio of the metal compound, the liquid carbon source, the promoter and the ammonium salt etchant is 1-5 g: 50-200 mL: 1-6 mL: 0.5-0.6 g.
5. A method for preparing single-walled carbon nanotubes, comprising the following steps: 1) mixing a liquid carbon source, an iron source, a sulfur source and an etchant to form a dispersion; 2) The dispersion is input through the top of the high-temperature furnace, and under the action of reducing gas and protective gas, single-walled carbon nanotubes are generated using a floating catalytic method, and the crude product is deposited at the bottom of the high-temperature furnace and in a collection tank; 3) The crude product needs to be purified to obtain pure and high-quality single-walled carbon nanotubes.
6. The method for preparing single-walled carbon nanotubes according to claim 5, characterized in that: Before adding the liquid feed in step 2), the dispersion was continuously heated to 100°C and stirred.
7. The method for preparing single-walled carbon nanotubes according to claim 5, characterized in that: In step 2), the ratio of reducing gas to protective gas is 1000-8000:4000 sccm, the injection speed of the feed liquid is 120-150 μL / min, and the furnace tube temperature of the high-temperature furnace is 1200-1250°C.
8. The method for preparing single-walled carbon nanotubes according to claim 5, characterized in that: In step 3), the crude product is calcined in air at a high temperature of 1200-1600°C.
9. The method for preparing single-walled carbon nanotubes according to claim 5, characterized in that: After the calcination in step 3), calcination is continued at 1400-1600° C. by introducing 1000-1500 sccm of carbon dioxide (CO 2 ) for 1-2 hours.
10. The method for preparing single-walled carbon nanotubes according to claim 8 or 9, characterized in that: In the air calcination, the crude product is exposed to oxygen for 1-2 hours, and the heating rate is 10°C / min.