Method for preparing battery grade lithium carbonate by using battery black powder

Battery-grade lithium carbonate is prepared through steps such as calcining, leaching, pH adjustment, chelating resin adsorption and bipolar membrane electrodialysis, which solves the problems of low lithium ion loss and recovery in traditional processes, and achieves high recovery and low impurities content simplifies the process flow and improves economic benefits.

CN118993112AInactive Publication Date: 2024-11-22HUNAN DJY-TECH CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410970818.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-22
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The traditional battery black powder preparation process for battery-grade lithium carbonate has low equipment investment but long process flow and large reflow, resulting in low lithium ion loss and recovery rate, and the inability to completely remove anionic impurities, affecting product indicators.

Method used

By using steps such as roasting, leaching, pH adjustment, chelating resin adsorption, bipolar membrane electrodialysis and carbon dioxide carbonization, baking black powder is obtained by roasting black powder, leaching lithium-rich solution, adjusting pH and adsorption of chelating resin, bipolar membrane After electrodialysis treatment, carbonization was achieved, and the heating reaction finally obtained battery-grade lithium carbonate, which avoided the use of precipitants and exogenous cations, canceled the sodium sulfate evaporation system, and improved the lithium yield.

Benefits of technology

It achieves a high recovery rate of battery-grade lithium carbonate, reduces P, F, and Na content, simplifies the process flow, saves equipment investment and operation management costs, and improves economic benefits.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004953135700000091
    Figure BDA0004953135700000091
  • Figure BDA0004953135700000101
    Figure BDA0004953135700000101
Patent Text Reader

Abstract

The invention discloses a method for preparing battery grade lithium carbonate by using battery black powder, and belongs to the technical field of resource recycling and reutilization, the method comprises the following steps: roasting the battery black powder, leaching by using a leaching solution, adjusting the pH value to 3.9-4.1, carrying out adsorption treatment by using chelate resin to effectively remove heavy metal ions, and carrying out bipolar membrane electrodialysis treatment to obtain the battery grade lithium carbonate. The method comprises the following steps: firstly, preparing lithium carbonate, then performing carbon dioxide carbonization and heating reaction, and performing post-treatment to obtain the battery-grade lithium carbonate, the battery-grade lithium carbonate reaches the battery grade specified by YS / T582 2013, the recovery rate of lithium is high, and the contents of P, F and Na in the prepared battery-grade lithium carbonate are low.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of resource recycling and reuse, and in particular to a method for preparing battery-grade lithium carbonate by utilizing battery black powder. Background Art

[0002] Battery black powder mainly refers to the black powder obtained by processing the positive and negative active materials and electrolyte components in waste batteries. It mainly comes from the recycling of waste lithium-ion batteries and is obtained after the steps of primary crushing, sorting, anaerobic cracking, and sorting.

[0003] The traditional method of preparing battery-grade lithium carbonate from battery black powder is mainly achieved through the process of roasting, water leaching, impurity removal, concentration, lithium carbonate precipitation, carbonization, impurity removal, and pyrolysis refining. This technical feature is that the equipment investment is low, but the process flow is long and the reflux volume is large. Since lithium carbonate has a certain solubility, the lithium carbonate precipitation mother liquor and the centrifugal mother liquor of lithium carbonate after pyrolysis need to be continuously recycled to the lithium carbonate precipitation stage. The above mother liquor belongs to a high-sodium and low-lithium solution. When the sodium ion concentration is too high, the solubility of sodium carbonate is low, which will lead to incomplete precipitation of lithium carbonate and excessive sodium content in the precipitated lithium carbonate. Problems such as serious impact on yield and product indicators, therefore, it is necessary to add evaporation crystallization equipment to discharge sodium crystals from the system. However, as the sodium salt evaporates, lithium ions are also enriched, and a small amount of lithium will be entrained during the crystallization of the sodium salt. This process is the main loss point in the process of preparing lithium carbonate from a water-leached lithium solution.

[0004] CN11712728A discloses a device and method for recycling waste ternary lithium batteries, which converts water-insoluble lithium salts in ternary electrode powder into lithium salts with a certain solubility in water through reduction roasting; then fully leaches soluble lithium through a grinding and water leaching process, and fully reacts lithium hydroxide in a first slurry to generate lithium bicarbonate through a cyclic reaction process; then filters nickel, cobalt and manganese slag in the ternary electrode powder through an impurity removal and filtration process, removes calcium, magnesium and fluoride ion impurities through resin impurity removal, and obtains lithium bicarbonate solution after filtering through a precision filter; and pyrolysis produces lithium carbonate solids through a saturated lithium bicarbonate solution through a pyrolysis lithium extraction process, which requires a large amount of water to wash and remove sodium, and cannot completely remove anions (such as fluorine and phosphorus). The recovery rate decreases during washing due to the dissolution of lithium carbonate, resulting in a recovery rate of less than 92%.

[0005] CN115417434A discloses a method for recovering valuable metals from waste lithium-ion battery black powder by carbon thermal reduction and preparing a lithium carbonate product. In the impurity removal process, battery-grade lithium carbonate needs to be added as a seed crystal for heating and decomposition. While preparing lithium carbonate, battery-grade lithium carbonate is also consumed. The lithium carbonate product prepared by the method cannot reach the battery grade specified in YS / T582 2013 (Examples 1 and 3 are less than 99.5%).

[0006] In view of this, this application is filed. Summary of the invention

[0007] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a method for preparing battery-grade lithium carbonate using battery black powder. The method of the present invention prepares battery-grade lithium carbonate with a high lithium recovery rate.

[0008] To achieve the above object, the technical solution adopted by the present invention is:

[0009] A method for preparing battery-grade lithium carbonate using battery black powder comprises the following steps:

[0010] (1) calcining battery black powder to obtain calcined black powder;

[0011] (2) leaching the roasted black powder and filtering it to obtain a lithium-rich solution;

[0012] (3) adjusting the pH of the lithium-rich solution to 3.9-4.1, filtering, and adsorbing the filtrate with a chelating resin to obtain a purified lithium-rich solution;

[0013] (4) subjecting the purified lithium-rich solution to bipolar membrane electrodialysis to obtain a lithium hydroxide solution;

[0014] (5) adding water to the lithium hydroxide solution until the lithium concentration is 8 to 9 g / L, and introducing carbon dioxide into the lithium hydroxide solution for carbonization to obtain a carbonized liquid;

[0015] (6) The carbonized liquid is heated for reaction, centrifuged, dried, crushed, and sieved to obtain battery-grade lithium carbonate.

[0016] The invention firstly roasts the battery black powder, performs leaching with a leaching solution, then adjusts the pH value to 3.9-4.1, performs adsorption treatment with a chelating resin, can effectively remove heavy metal ions, then performs bipolar membrane electrodialysis treatment, and then performs carbon dioxide carbonization and heating reaction, and performs post-treatment to obtain battery-grade lithium carbonate. The battery-grade lithium carbonate reaches the battery grade specified in YS / T582 2013, has a high lithium recovery rate, and has low P, F and Na contents in the prepared battery-grade lithium carbonate.

[0017] As a preferred embodiment of the present invention, the battery black powder includes at least one of ternary lithium battery black powder and lithium iron phosphate battery black powder.

[0018] As a preferred embodiment of the present invention, the calcination temperature is 500-700°C, and the calcination time is 0.5-2h;

[0019] The calcination is carried out in the presence of a reducing agent or in a nitrogen atmosphere; the reducing agent comprises at least one of reducing carbon powder, hydrogen, carbon monoxide, sodium sulfate, ammonium sulfate and sulfuric acid solution.

[0020] As a preferred embodiment of the present invention, the leaching of the roasted black powder is specifically as follows: adding the roasted black powder into water for leaching, adding or not adding sulfuric acid solution during the leaching process, to obtain a lithium-rich solution;

[0021] The solid-liquid ratio of the roasted black powder to water is 1g: (3-10)mL;

[0022] The molar concentration of the sulfuric acid solution is 0.1 to 10 mol / L;

[0023] The solid-liquid ratio of the roasted black powder to the sulfuric acid solution is (1.5-2.5) g:1.

[0024] As a preferred embodiment of the present invention, the calcination is performed in a reducing atmosphere or an air atmosphere.

[0025] As a preferred embodiment of the present invention, the leaching temperature is 50-80°C, and the leaching time is 0.5-2h.

[0026] As a preferred embodiment of the present invention, the pH of the lithium-rich solution is adjusted to 3.9-4.1 by using a lithium hydroxide solution;

[0027] As a preferred embodiment of the present invention, the molar concentration of the lithium hydroxide solution is 1 to 10 mol / L.

[0028] The lithium hydroxide solution used in the present application can be a lithium hydroxide solution produced by an electrodialysis device.

[0029] As a preferred embodiment of the present invention, the molar concentration of the sulfuric acid solution is 1 to 10 mol / L.

[0030] As a preferred embodiment of the present invention, the current density of the bipolar membrane electrodialysis is 760-900A / m 2 , the voltage is 3.2~3.8V.

[0031] As a preferred embodiment of the present invention, the current density of the bipolar membrane electrodialysis is 860A / m 2 , the voltage is 3.6V.

[0032] As a preferred embodiment of the present invention, carbon dioxide is introduced into the lithium hydroxide solution for carbonization according to a molar ratio of Li to C of 3:(1.8-2.2).

[0033] As a preferred embodiment of the present invention, the temperature of the heating reaction is 90-100° C., and the time of the heating reaction is 0.5-2 h.

[0034] As a preferred embodiment of the present invention, the mother liquor produced by centrifugation in step (6) is incorporated into the purified lithium-rich solution in step (4).

[0035] The beneficial effects of the present invention are as follows: (1) the present invention first roasts the battery black powder, leaches it with a leaching solution, and then adjusts the pH to 3.9-4.1, and uses a chelating resin for adsorption treatment, which can effectively remove heavy metal ions, and then undergoes bipolar membrane electrodialysis treatment, and then undergoes carbonization of carbon dioxide and heating reaction, and after post-treatment, obtains battery-grade lithium carbonate, the battery-grade lithium carbonate reaches the battery grade specified in YS / T582 2013, and its lithium recovery rate is high, and the P, F, and Na contents in the prepared battery-grade lithium carbonate are low; (2) the present invention does not need to use a precipitant to precipitate lithium carbonate, nor does it need to add battery-grade lithium carbonate as a crystal seed, and no exogenous cations are introduced, so the process does not need to set up a sodium sulfate evaporation system, thereby avoiding the lithium loss caused by sodium sulfate crystallization out of the system in the traditional process, and improving the lithium yield; (3) the present invention can cancel a whole set of systems for treating byproduct sodium sulfate by optimizing the processing flow and creatively adjusting the process steps. Low-value byproducts are streamlined, the corresponding equipment investment and operation management costs are saved, and the economic benefits of the lithium extraction process are improved. DETAILED DESCRIPTION

[0036] In order to make the purpose, technical solutions and advantages of the embodiments of the present application clearer, the technical solutions in the embodiments of the present application are described clearly and completely below. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present application.

[0037] In the present application, the technical features described in an open manner include closed technical solutions composed of the listed features, and also include open technical solutions containing the listed features.

[0038] In this application, when it comes to numerical ranges, unless otherwise specified, the above numerical ranges are deemed to be continuous and include the minimum and maximum values ​​of the range, as well as each value between such minimum and maximum values. Further, when a range refers to an integer, each integer between the minimum and maximum values ​​of the range is included. In addition, when multiple ranges are provided to describe features or characteristics, the ranges can be merged. In other words, unless otherwise specified, all ranges disclosed herein should be understood to include any and all subranges included therein.

[0039] In the present application, there is no particular limitation on the specific dispersion and stirring treatment methods.

[0040] Unless otherwise specified, the components, raw materials or instruments used in the embodiments and comparative examples of the present invention are all commercially available raw materials or instruments, and the components and raw materials used in each parallel experiment are all of the same kind.

[0041] The following examples are provided to facilitate understanding of the present invention. These examples are not provided to limit the scope of the claims.

[0042] Example 1

[0043] A method for preparing battery-grade lithium carbonate using battery black powder comprises the following steps:

[0044] (1) calcining the ternary battery black powder in a hydrogen atmosphere to obtain calcined black powder, the calcination temperature is 600° C., and the calcination time is 1 h;

[0045] (2) leaching the roasted black powder with pure water at a solid-liquid ratio of 1 g:3 mL at 70° C. for 1 h, and adding 1 mol / L sulfuric acid at a solid-liquid ratio of 2 g:1 mL at a uniform rate during the leaching process, and filtering after leaching to obtain a lithium-rich solution;

[0046] (3) adjusting the pH of the lithium-rich solution to 4 with a 10 mol / L sulfuric acid solution, filtering the solution sequentially through a plate-and-frame filter and a microporous filter with a filtration accuracy of 0.1 μm, passing the filtrate through a chelating resin column, and performing adsorption treatment with the chelating resin to obtain a purified lithium-rich solution;

[0047] (4) Passing the purified lithium-rich solution into a bipolar membrane electrodialysis device for electrodialysis treatment, wherein the current density of the bipolar membrane electrodialysis is 860 A / m 2 , the voltage is 3.6V; lithium hydroxide solution is obtained;

[0048] (5) adding water to the lithium hydroxide solution until the lithium concentration is 8.5 g / L, and introducing carbon dioxide into the lithium hydroxide solution according to a molar ratio of Li to C of 3:2 for carbonization to obtain a carbonized liquid;

[0049] (6) The carbonized liquid is heated to 95° C. for reaction for 1 hour, centrifuged, dried, crushed, and sieved to obtain battery-grade lithium carbonate, wherein the mother liquor produced by centrifugation is incorporated into the purified lithium-rich solution in (4).

[0050] Example 2

[0051] A method for preparing battery-grade lithium carbonate using battery black powder comprises the following steps:

[0052] (1) calcining the ternary battery black powder in a hydrogen atmosphere to obtain calcined black powder, the calcination temperature is 600° C., and the calcination time is 1 h;

[0053] (2) leaching the roasted black powder with pure water at a solid-liquid ratio of 1 g:3 mL at 70° C. for 1 h, and adding 1 mol / L sulfuric acid at a solid-liquid ratio of 2 g:1 mL at a uniform rate during the leaching process, and filtering after leaching to obtain a lithium-rich solution;

[0054] (3) adjusting the pH of the lithium-rich solution to 4 with a 10 mol / L sulfuric acid solution, filtering the solution sequentially through a plate-and-frame filter press and a microporous filter with a filtration accuracy of 0.1 μm, and passing the filtrate through a chelating resin column for adsorption treatment with the chelating resin to obtain a purified lithium-rich solution;

[0055] (4) The purified lithium-rich solution is passed into a bipolar membrane electrodialysis device for electrodialysis treatment, and the current density of the bipolar membrane electrodialysis is 900A / m 2 , the voltage is 3.8V; lithium hydroxide solution is obtained;

[0056] (5) adding water to the lithium hydroxide solution until the lithium concentration is 8.5 g / L, and introducing carbon dioxide into the lithium hydroxide solution according to a molar ratio of Li to C of 3:2 for carbonization to obtain a carbonized liquid;

[0057] (6) The carbonized liquid is heated to 95° C. for reaction for 1 hour, centrifuged, dried, crushed, and sieved to obtain battery-grade lithium carbonate, wherein the mother liquor produced by centrifugation is incorporated into the purified lithium-rich solution in (4).

[0058] Example 3

[0059] A method for preparing battery-grade lithium carbonate using battery black powder comprises the following steps:

[0060] (1) calcining the ternary battery black powder in a hydrogen atmosphere to obtain calcined black powder, the calcination temperature is 600° C., and the calcination time is 1 h;

[0061] (2) leaching the roasted black powder with pure water at a solid-liquid ratio of 1 g:3 mL at 70° C. for 1 h, and adding 1 mol / L sulfuric acid at a solid-liquid ratio of 2 g:1 mL at a uniform rate during the leaching process, and filtering after leaching to obtain a lithium-rich solution;

[0062] (3) adjusting the pH of the lithium-rich solution to 4 with a 10 mol / L sulfuric acid solution, filtering the solution sequentially through a plate-and-frame filter press and a microporous filter with a filtration accuracy of 0.1 μm, and passing the filtrate through a chelating resin column for adsorption treatment with the chelating resin to obtain a purified lithium-rich solution;

[0063] (4) Passing the purified lithium-rich solution into a bipolar membrane electrodialysis device for electrodialysis treatment, wherein the current density of the bipolar membrane electrodialysis is 760 A / m 2 , the voltage is 3.2V; lithium hydroxide solution is obtained;

[0064] (5) adding water to the lithium hydroxide solution until the lithium concentration is 8.5 g / L, and introducing carbon dioxide into the lithium hydroxide solution according to a molar ratio of Li to C of 3:2 for carbonization to obtain a carbonized liquid;

[0065] (6) The carbonized liquid is heated to 95° C. for reaction for 1 hour, centrifuged, dried, crushed, and sieved to obtain battery-grade lithium carbonate, wherein the mother liquor produced by centrifugation is incorporated into the purified lithium-rich solution in (4).

[0066] Example 4

[0067] A method for preparing battery-grade lithium carbonate using battery black powder comprises the following steps:

[0068] (1) calcining the ternary battery black powder in a hydrogen atmosphere to obtain calcined black powder, the calcination temperature is 600° C., and the calcination time is 1 h;

[0069] (2) leaching the roasted black powder with pure water at a solid-liquid ratio of 1 g:3 mL at 70° C. for 1 h, and adding 1 mol / L sulfuric acid at a solid-liquid ratio of 2 g:1 mL at a uniform rate during the leaching process, and filtering after leaching to obtain a lithium-rich solution;

[0070] (3) adjusting the pH of the lithium sulfate solution to 4 with a 10 mol / L sulfuric acid solution, filtering the solution sequentially through a plate and frame filter press and a microporous filter with a filtration accuracy of 0.1 μm, and passing the filtrate through a chelating resin column for adsorption treatment using the chelating resin to obtain a purified lithium-rich solution;

[0071] (4) Passing the purified lithium-rich solution into a bipolar membrane electrodialysis device for electrodialysis treatment, wherein the current density of the bipolar membrane electrodialysis is 860 A / m 2 , the voltage is 3.6V; lithium hydroxide solution is obtained;

[0072] (5) adding water to the lithium hydroxide solution until the lithium concentration is 8.2 g / L, and introducing carbon dioxide into the lithium hydroxide solution according to a molar ratio of Li to C of 3:2 for carbonization to obtain a carbonized liquid;

[0073] (6) The carbonized liquid is heated to 95° C. for reaction for 1 hour, centrifuged, dried, crushed, and sieved to obtain battery-grade lithium carbonate, wherein the mother liquor produced by centrifugation is incorporated into the purified lithium-rich solution in (4).

[0074] Example 5

[0075] A method for preparing battery-grade lithium carbonate using battery black powder comprises the following steps:

[0076] (1) calcining the ternary battery black powder in a hydrogen atmosphere to obtain calcined black powder, the calcination temperature is 600° C., and the calcination time is 1 h;

[0077] (2) leaching the roasted black powder with pure water at a solid-liquid ratio of 1 g:3 mL at 70° C. for 1 h, and adding 1 mol / L sulfuric acid at a solid-liquid ratio of 2 g:1 mL at a uniform rate during the leaching process, and filtering after leaching to obtain a lithium-rich solution;

[0078] (3) adjusting the pH of the lithium sulfate solution to 4 with a 10 mol / L sulfuric acid solution, filtering the solution sequentially through a plate and frame filter press and a microporous filter with a filtration accuracy of 0.1 μm, and passing the filtrate through a chelating resin column for adsorption treatment using the chelating resin to obtain a lithium-rich solution;

[0079] (4) Passing the purified lithium-rich solution into a bipolar membrane electrodialysis device for electrodialysis treatment, wherein the current density of the bipolar membrane electrodialysis is 860 A / m 2 , the voltage is 3.6V; lithium hydroxide solution is obtained;

[0080] (5) adding water to the lithium hydroxide solution to a lithium concentration of 8 g / L, and introducing carbon dioxide into the lithium hydroxide solution according to a molar ratio of Li to C of 3:2 for carbonization to obtain a carbonized liquid;

[0081] (6) The carbonized liquid is heated to 95° C. for reaction for 1 hour, centrifuged, dried, crushed, and sieved to obtain battery-grade lithium carbonate, wherein the mother liquor produced by centrifugation is incorporated into the purified lithium-rich solution in (4).

[0082] Example 6

[0083] A method for preparing battery-grade lithium carbonate using battery black powder comprises the following steps:

[0084] (1) calcining lithium iron phosphate battery black powder in a nitrogen atmosphere to obtain calcined black powder, the calcination temperature is 600° C., and the calcination time is 1 h;

[0085] (2) leaching the roasted black powder with a 5 mol / L sulfuric acid solution at a solid-liquid ratio of 1 g:3 mL at 70° C. for 1 h, and filtering to obtain a lithium-rich solution;

[0086] (3) adjusting the pH of the lithium-rich solution to 4 with a 5 mol / L lithium hydroxide solution, filtering the solution sequentially through a plate and frame filter press and a microporous filter with a filtration accuracy of 0.1 μm, and passing the filtrate through a chelating resin column for adsorption treatment using the chelating resin to obtain a purified lithium-rich solution;

[0087] (4) Passing the lithium-rich solution into a bipolar membrane electrodialysis device for electrodialysis treatment, wherein the current density of the bipolar membrane electrodialysis is 860 A / m 2, the voltage is 3.6V; lithium hydroxide solution is obtained;

[0088] (5) adding water to the lithium hydroxide solution until the lithium concentration is 8.5 g / L, and introducing carbon dioxide into the lithium hydroxide solution according to a molar ratio of Li to C of 3:2 for carbonization to obtain a carbonized liquid;

[0089] (6) The carbonized liquid is heated to 95° C. for reaction for 1 hour, centrifuged, dried, crushed, and sieved to obtain battery-grade lithium carbonate, wherein the mother liquor produced by centrifugation is incorporated into the purified lithium-rich solution in (4).

[0090] Comparative Example 1

[0091] The difference between Comparative Example 1 and Example 1 is that Comparative Example 1 is not adsorbed by chelating resin.

[0092] A method for preparing lithium carbonate using battery black powder comprises the following steps:

[0093] (1) calcining the ternary battery black powder in a hydrogen atmosphere to obtain calcined black powder, the calcination temperature is 600° C., and the calcination time is 1 h;

[0094] (2) leaching the roasted black powder with pure water at a solid-liquid ratio of 1 g:3 mL at 70° C. for 1 h, and adding 1 mol / L sulfuric acid at a solid-liquid ratio of 2 g:1 mL at a uniform rate during the leaching process, and filtering after leaching to obtain a lithium-rich solution;

[0095] (3) adjusting the pH of the lithium-rich solution to 4 with a 5 mol / L sulfuric acid solution, and then filtering through a plate-and-frame filter press and a microporous filter with a filtration accuracy of 0.1 μm to obtain a purified lithium-rich solution;

[0096] (4) Passing the purified lithium-rich solution into a bipolar membrane electrodialysis device for electrodialysis treatment, wherein the current density of the bipolar membrane electrodialysis is 860 A / m 2 , the voltage is 3.6V; lithium hydroxide solution is obtained;

[0097] (5) adding water to the lithium hydroxide solution until the lithium concentration is 8.5 g / L, and introducing carbon dioxide into the lithium hydroxide solution according to a molar ratio of Li to C of 3:2 for carbonization to obtain a carbonized liquid;

[0098] (6) The carbonized liquid is heated to 95° C. for reaction for 1 hour, and centrifuged to obtain lithium carbonate solid, which is then dried, crushed, and sieved to obtain lithium carbonate, wherein the centrifugal mother liquor produced by centrifugation is incorporated into the purified lithium-rich solution in (4).

[0099] Comparative Example 2

[0100] The difference between Comparative Example 2 and Example 1 is that Comparative Example 2 is not subjected to bipolar membrane electrodialysis treatment.

[0101] A method for preparing lithium carbonate using battery black powder comprises the following steps:

[0102] (1) calcining the ternary battery black powder in a hydrogen atmosphere to obtain calcined black powder, the calcination temperature is 600° C., and the calcination time is 1 h;

[0103] (2) leaching the roasted black powder with a sulfuric acid solution at a solid-liquid ratio of 1 g:3.5 mL at 70° C. for 1 h, and filtering to obtain a lithium sulfate solution;

[0104] (3) adjusting the pH of the lithium sulfate solution to 4 with a 5 mol / L lithium hydroxide solution, filtering the solution through a plate and frame filter and a microporous filter with a filtration accuracy of 0.1 μm, passing the filtrate through a chelating resin column, and performing adsorption treatment with the chelating resin to obtain a lithium-rich solution;

[0105] (4) adding water to the lithium-rich solution to a lithium concentration of 8.5 g / L, and introducing carbon dioxide into the lithium carbonate slurry at a molar ratio of Li to C of 3:2 to obtain a carbonized liquid;

[0106] (5) The carbonized liquid was heated to 95°C for 1 hour, but no lithium carbonate solid was obtained.

[0107] Comparative Example 3

[0108] A method for preparing lithium carbonate using battery black powder comprises the following steps:

[0109] (1) calcining the ternary battery black powder in a hydrogen atmosphere to obtain calcined black powder, the calcination temperature is 600° C., and the calcination time is 1 h;

[0110] (2) leaching the roasted black powder with pure water at a solid-liquid ratio of 1 g:3.5 mL at 70° C. for 1 h, and filtering to obtain a lithium-rich solution;

[0111] (3) adjusting the pH of the lithium-rich solution to 4 with a 10 mol / L sulfuric acid solution, filtering the solution sequentially through a plate-and-frame filter and a microporous filter with a filtration accuracy of 0.1 μm, and passing the filtrate through a chelating resin column for adsorption treatment using the chelating resin to obtain a purified lithium-rich solution;

[0112] (4) Passing the purified lithium-rich solution into a bipolar membrane electrodialysis device for electrodialysis treatment, wherein the current density of the bipolar membrane electrodialysis is 860 A / m 2 , the voltage is 3.6V; lithium hydroxide solution is obtained;

[0113] (5) adding water to the lithium hydroxide solution until the lithium concentration is 8.5 g / L, and introducing carbon dioxide into the lithium hydroxide solution according to a molar ratio of Li to C of 3:2 for carbonization to obtain a carbonized liquid;

[0114] (6) The carbonized liquid is heated to 95° C. for reaction for 1 hour, centrifuged, dried, crushed, and sieved to obtain lithium carbonate, wherein the mother liquor produced by centrifugation is incorporated into the purified lithium-rich solution in (4).

[0115] Test Case

[0116] The same batch of ternary battery black powder (lithium content of 4.5%) was treated according to the methods of Examples 1 to 5 and Comparative Examples 1 to 2, and the indicators of the obtained lithium carbonate are shown in Table 1.

[0117] Table 1

[0118]

[0119]

[0120] Note: The heavy metal content in the table includes the total value of nickel, manganese, copper, zinc and other elements.

[0121] As can be seen from Table 1, the present invention prepares battery-grade lithium carbonate, which reaches the battery grade specified in YS / T582 2013, has a high lithium recovery rate, and the prepared battery-grade lithium carbonate has low P, F, and Na contents.

[0122] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.

Claims

1. A method for preparing battery-grade lithium carbonate using battery black powder, characterized in that: The following steps are involved: (1) calcining battery black powder to obtain calcined black powder; (2) leaching the roasted black powder and filtering it to obtain a lithium-rich solution; (3) adjusting the pH of the lithium-rich solution to 3.9-4.1, filtering, and adsorbing the filtrate with a chelating resin to obtain a purified lithium-rich solution; (4) subjecting the lithium-rich solution to bipolar membrane electrodialysis to obtain a lithium hydroxide solution; (5) adding water to the lithium hydroxide solution until the lithium concentration is 8 to 9 g / L, and introducing carbon dioxide into the lithium hydroxide solution for carbonization to obtain a carbonized liquid; (6) The carbonized liquid is heated for reaction, centrifuged, dried, crushed, and sieved to obtain battery-grade lithium carbonate.

2. The method for preparing battery-grade lithium carbonate using battery black powder according to claim 1, characterized in that: The calcination temperature is 500-700°C and the calcination time is 0.5-2h; The calcination is carried out in the presence of a reducing agent or in a nitrogen atmosphere; the reducing agent comprises at least one of reducing carbon powder, hydrogen, carbon monoxide, sodium sulfate, ammonium sulfate and sulfuric acid solution.

3. The method for preparing battery-grade lithium carbonate using battery black powder according to claim 1, characterized in that: The leaching of the roasted black powder specifically comprises: adding the roasted black powder into water for leaching, and adding or not adding sulfuric acid solution during the leaching process to obtain a lithium-rich solution; The solid-liquid ratio of the roasted black powder to water is 1g: (3-10)mL; The molar concentration of the sulfuric acid solution is 0.1 to 10 mol / L; The solid-liquid ratio of the roasted black powder to the sulfuric acid solution is (1.5-2.5) g:

1.

4. The method for preparing battery-grade lithium carbonate using battery black powder according to claim 1, characterized in that: The leaching temperature is 50-80° C., and the leaching time is 0.5-2 hours.

5. The method for preparing battery-grade lithium carbonate using battery black powder according to claim 1, characterized in that: The pH of the lithium-rich solution is adjusted to 3.9-4.1 by using a lithium hydroxide solution or a sulfuric acid solution.

6. The method for preparing battery-grade lithium carbonate using battery black powder according to claim 5, characterized in that: The molar concentration of the lithium hydroxide solution is 1 to 10 mol / L; The molar concentration of the sulfuric acid solution is 1-10 mol / L.

7. The method for preparing battery-grade lithium carbonate using battery black powder according to claim 1, characterized in that: The current density of the bipolar membrane electrodialysis is 760-900A / m 2 , the voltage is 3.2~3.8V.

8. The method for preparing battery-grade lithium carbonate using battery black powder according to claim 1, characterized in that: The current density of the bipolar membrane electrodialysis is 860A / m 2 , the voltage is 3.6V.

9. The method for preparing battery-grade lithium carbonate using battery black powder according to claim 1, characterized in that: Carbon dioxide is introduced into the lithium hydroxide solution at a molar ratio of Li to C of 3:(1.8-2.2) for carbonization.

10. The method for preparing battery-grade lithium carbonate using battery black powder according to claim 1, characterized in that: The temperature of the heating reaction is 90-100° C., and the time of the heating reaction is 0.5-2 hours.

Citation Information

Patent Citations

  • Method for preparing battery-grade lithium carbonate from lepidolite

    CN112142081A

  • Method for pressurizing and roasting waste lithium battery black powder to fix fluorine and extract lithium

    CN114132951A

  • Recycling method of lithium iron phosphate battery

    CN115367776A

  • Method and device for recycling battery black powder

    CN115764033A

  • Method for recycling battery material black powder

    CN116130817A