Method for extracting aluminum hydroxide from aluminum electrolyte
Through the method of crushing and step by step mixing and dissolving, the aluminum electrolyte slag is mixed with calcium hydroxide, heat up and stirred and adjusted the pH value, which solves the problem of low aluminum recovery efficiency in aluminum electrolyte slag, and achieves more efficient aluminum hydroxide recovery.
Patent Information
- Application Number
- CN202411028873.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-11-22
AI Technical Summary
In the prior art, the recycling efficiency of aluminum in aluminum electrolyte slag is low, and the process parameters are difficult to control, resulting in cumbersome recycling process.
By pulverizing and dissolving step by step, the aluminum electrolyte slag is mixed with calcium hydroxide, heated up and stirred, and the pH value is adjusted by acidic substances, and finally aluminum hydroxide is obtained by filtration and drying.
The recycling efficiency of aluminum in aluminum electrolyte slag is improved, making the entire process easier to control and ensuring the full conversion of aluminum into aluminum hydroxide.
Smart Images

Figure CN118993124A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of aluminum electrolyte slag treatment, and in particular to a method for extracting aluminum hydroxide from aluminum electrolyte. Background Art
[0002] Aluminum electrolyte slag is a by-product produced during the aluminum electrolytic smelting process, mainly composed of impurities and insolubles in the electrolyte. Aluminum electrolytic smelting is the process of producing aluminum metal by electrolyzing aluminum oxide. The electrolyte used in the electrolytic cell is usually molten aluminum fluoride salt and alumina. In this process, as the electrolytic reaction proceeds, some impurities and insolubles will gradually precipitate and form aluminum electrolyte slag. Aluminum electrolyte slag contains a large amount of metallic aluminum, and direct discharge will cause a waste of resources. Therefore, the aluminum in the aluminum electrolyte slag needs to be recovered.
[0003] At present, the aluminum in aluminum electrolyte slag is mainly recovered by filtering and precipitating the aluminum electrolyte slag first, and then roasting the aluminum electrolyte slag. Then, the aluminum electrolyte slag is put into a reaction vessel, and the aluminum in the aluminum electrolyte slag is recovered by leaching and dissolving. Although the aluminum in the aluminum electrolyte slag can be recovered under the above recovery method, the whole recovery process is relatively cumbersome, and the parameters in each process of the recovery process are difficult to control and fluctuate greatly, resulting in a relatively low recovery efficiency of aluminum in the aluminum electrolyte slag. Summary of the invention
[0004] The object of the present invention is to provide a method for extracting aluminum hydroxide from aluminum electrolyte in order to solve the above-mentioned problems.
[0005] The present invention achieves the above-mentioned purpose through the following technical solutions:
[0006] A method for extracting aluminum hydroxide from an aluminum electrolyte comprises the following steps:
[0007] Step 1: crushing the aluminum electrolyte slag and sieving it, the mesh size used is 100-300 mesh;
[0008] Step 2: Mix aluminum electrolyte slag with calcium hydroxide in a weight ratio of 1:(2-3) and stir evenly;
[0009] Step 3: Mix the mixture of step 2 with water at a solid-liquid ratio of 1:(1-5), and heat to 90-110 degrees Celsius;
[0010] Step 4: Stir the slurry in step 3 at 90-100 degrees Celsius for 4 hours, and add sodium hydroxide according to the pH value of the solution to adjust the pH value to greater than 14;
[0011] Step 5: filtering the slurry of step 4, and the resulting solution is a sodium aluminate solution, in which metals such as calcium and magnesium are completely precipitated under alkaline conditions, fluoride ions are combined with calcium to form calcium fluoride, and lithium ions are partially leached in the sodium aluminate solution;
[0012] Step 6: Treat the solution in step 5 by adding an acidic substance, which may be an organic weak acid or an inorganic strong acid, adjusting the pH to 9-12, and aging the solution at a temperature of 70-90 degrees Celsius for 2-6 hours;
[0013] Step 7: Filter the slurry in step 6, and stir and wash it in water at 80 degrees Celsius, and the obtained solid is aluminum hydroxide;
[0014] Step 8: Dry the aluminum hydroxide obtained in step 7 at 80-120 degrees Celsius to obtain aluminum hydroxide.
[0015] Furthermore, the aluminum electrolyte slag in step 1 is mainly composed of cryolite (Na3AlF6), alumina (Al2O3) and other salt additives.
[0016] Furthermore, other salt additives include AlF3, CaF2, MgF2, and LiF, ensuring that the above recovery method is applicable to aluminum electrolyte slag containing the above salt additives.
[0017] Furthermore, in the step 2, the preferred weight ratio of the aluminum electrolyte slag to the calcium hydroxide is 1:(2.5-3). By strictly controlling the mixing ratio of the aluminum electrolyte slag to the calcium hydroxide, sufficient reaction of the aluminum electrolyte slag and the calcium hydroxide can be ensured.
[0018] Furthermore, the preferred solid-liquid ratio in step 3 is 1:(2-3), and the preferred temperature for heating in step 3 is 95-100 degrees Celsius, which can ensure efficient reaction process.
[0019] Furthermore, the preferred stirring temperature of the slurry in step 4 is 95-100 degrees Celsius.
[0020] Furthermore, the preferred temperature during aging in step 6 is 85-90 degrees Celsius, and the aging time is preferably 3-4 hours, which can ensure sufficient precipitation of aluminum hydroxide after the reaction for subsequent filtration and separation.
[0021] The beneficial effects of the present invention are:
[0022] The present invention adopts the method of crushing and step-by-step mixed dissolution to realize the recovery of aluminum in aluminum electrolyte slag, and strictly controls the mixing ratio of the feed liquid, the reaction temperature after mixing and the reaction time in each step, so that the entire recovery process of aluminum in the aluminum electrolyte slag is easier to control, ensuring that the aluminum in the aluminum electrolyte slag can be fully converted into aluminum hydroxide, so that the recovery efficiency of aluminum in the aluminum electrolyte slag is improved. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 The present invention is a flow chart of a method for extracting aluminum hydroxide from aluminum electrolyte. DETAILED DESCRIPTION
[0024] A method for extracting aluminum hydroxide from an aluminum electrolyte comprises the following steps:
[0025] Step 1: crushing the aluminum electrolyte slag and sieving it, the mesh size used is 100-300 mesh;
[0026] Step 2: Mix aluminum electrolyte slag with calcium hydroxide in a weight ratio of 1:(2-3) and stir evenly;
[0027] Step 3: Mix the mixture of step 2 with water at a solid-liquid ratio of 1:(1-5), and heat to 90-110 degrees Celsius;
[0028] Step 4: Stir the slurry in step 3 at 90-100 degrees Celsius for 4 hours, and add sodium hydroxide according to the pH value of the solution to adjust the pH value to greater than 14;
[0029] Step 5: filtering the slurry of step 4, and the resulting solution is a sodium aluminate solution, in which metals such as calcium and magnesium are completely precipitated under alkaline conditions, fluoride ions are combined with calcium to form calcium fluoride, and lithium ions are partially leached in the sodium aluminate solution;
[0030] Step 6: Treat the solution in step 5 by adding an acidic substance, which may be an organic weak acid or an inorganic strong acid, adjusting the pH to 9-12, and aging the solution at a temperature of 70-90 degrees Celsius for 2-6 hours;
[0031] Step 7: Filter the slurry in step 6, and stir and wash it in water at 80 degrees Celsius, and the obtained solid is aluminum hydroxide;
[0032] Step 8: Dry the aluminum hydroxide obtained in step 7 at 80-120 degrees Celsius to obtain aluminum hydroxide.
[0033] In this embodiment, the aluminum electrolyte slag in step 1 is mainly composed of cryolite (Na3AlF6), alumina (Al2O3) and other salt additives.
[0034] In this embodiment, other salt additives include AlF3, CaF2, MgF2, and LiF, ensuring that the above recovery method is applicable to aluminum electrolyte slag containing the above salt additives.
[0035] In this embodiment, the preferred weight ratio of the aluminum electrolyte slag and calcium hydroxide when mixed in step 2 is 1:(2.5-3). By strictly controlling the mixing ratio of the aluminum electrolyte slag and calcium hydroxide, sufficient reaction of the aluminum electrolyte slag and calcium hydroxide can be ensured.
[0036] In this embodiment, the preferred solid-liquid ratio in step 3 is 1:(2-3), and the preferred temperature for heating in step 3 is 95-100 degrees Celsius, which can ensure efficient reaction process.
[0037] In this embodiment, the preferred stirring temperature of the slurry in step 4 is 95-100 degrees Celsius.
[0038] In this embodiment, the preferred temperature during aging in step 6 is 85-90 degrees Celsius, and the aging time is preferably 3-4 hours, which can ensure sufficient precipitation of aluminum hydroxide after the reaction for subsequent filtration and separation.
[0039] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for extracting aluminum hydroxide from aluminum electrolyte, Features: It includes the following steps: Step 1: crushing the aluminum electrolyte slag and sieving it, the mesh size used is 100-300 mesh; Step 2: Mix aluminum electrolyte slag with calcium hydroxide in a weight ratio of 1:(2-3) and stir evenly; Step 3: Mix the mixture of step 2 with water at a solid-liquid ratio of 1:(1-5), and heat to 90-110 degrees Celsius; Step 4: Stir the slurry in step 3 at 90-100 degrees Celsius for 4 hours, and add sodium hydroxide according to the pH value of the solution to adjust the pH value to greater than 14; Step 5: filtering the slurry of step 4, and the resulting solution is a sodium aluminate solution, in which metals such as calcium and magnesium are completely precipitated under alkaline conditions, fluoride ions are combined with calcium to form calcium fluoride, and lithium ions are partially leached in the sodium aluminate solution; Step 6: Treat the solution in step 5 by adding an acidic substance, which may be an organic weak acid or an inorganic strong acid, adjusting the pH to 9-12, and aging the solution at a temperature of 70-90 degrees Celsius for 2-6 hours; Step 7: Filter the slurry in step 6, and stir and wash it in water at 80 degrees Celsius, and the obtained solid is aluminum hydroxide; Step 8: Dry the aluminum hydroxide obtained in step 7 at 80-120 degrees Celsius to obtain aluminum hydroxide.
2. A method for extracting aluminum hydroxide from an aluminum electrolyte according to claim 1, Features: The aluminum electrolyte slag in step 1 is mainly composed of cryolite (Na3AlF6), alumina (Al2O3) and other salt additives.
3. A method for extracting aluminum hydroxide from an aluminum electrolyte according to claim 2, Features: Other salt additives include AlF3, CaF2, MgF2, and LiF.
4. A method for extracting aluminum hydroxide from an aluminum electrolyte according to claim 1, Features: In the step 2, the preferred weight ratio of the aluminum electrolyte slag and the calcium hydroxide when mixed is 1:(2.5-3).
5. A method for extracting aluminum hydroxide from an aluminum electrolyte according to claim 1, Features: The preferred solid-liquid ratio in step 3 is 1:(2-3), and the preferred temperature for heating in step 3 is 95-100 degrees Celsius.
6. A method for extracting aluminum hydroxide from an aluminum electrolyte according to claim 1, Features: The preferred stirring temperature of the slurry in step 4 is 95-100 degrees Celsius.
7. A method for extracting aluminum hydroxide from an aluminum electrolyte according to claim 1, Features: The preferred temperature during aging in step 6 is 85-90 degrees Celsius, and the aging time is preferably 3-4 hours.