Lithium ion ternary positive electrode material, preparation method thereof and lithium ion battery
By forming a lithium titanate cladding layer on the surface of the single crystal active particles of the positive electrode material of the lithium ion battery, the problem of insufficient circulation performance of the lithium ion battery is solved, and the circulation performance and safety performance of the battery are significantly improved.
Patent Information
- Application Number
- CN202310554765.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-17
- Publication Date
- 2024-11-22
AI Technical Summary
The cycling performance of lithium-ion batteries has not yet met the requirements for improvement, especially under high current density, the capacity of the cathode material is severely attenuated, making it difficult to meet the large-rate discharge requirements of powered cars.
Single crystal active particles are prepared using ternary precursors and lithium source substances, and a clad layer containing lithium titanate and doped elements is formed on their surface. The doped elements are Mg, Al, Zr, Er, Sr, Nd, Y And W, the cladding layer accounts for 0.05% to 5% of the total mass of the cathode material, and a stable cladding layer is formed by sintering treatment.
The layered structure of the positive electrode material is stabilized, phase change during charging and discharging is suppressed, and the conductive performance of the cladding layer is improved, thereby significantly improving the cycle performance and safety performance of the battery.
Smart Images

Figure CN118993165A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of lithium ion batteries, and in particular to a lithium ion ternary positive electrode material and a preparation method thereof, and a lithium ion battery. Background Art
[0002] As the core part of lithium batteries, developing a ternary positive electrode material with high energy density, long cycle and high safety has become the top priority for improving the performance of lithium batteries.
[0003] Lithium-ion batteries have the advantages of high operating voltage, high energy density, long cycle life, light weight, small size, low self-discharge rate, no memory effect, and environmental protection. They are considered to be the most attractive choice among rechargeable batteries. In the past few decades, lithium-ion batteries have been widely used in small electronic devices, including mobile phones, laptops, and cameras. However, the cycle performance of lithium-ion batteries needs to be improved. The commonly used improvement method in the industry is to coat the positive electrode material. At present, the commonly used commercial coating method is solid-phase mixed coating, which mainly uses other metals and metal oxides (such as MgO, Al2O3, ZrO2, etc.) for surface coating. It can only improve the cycle performance of the positive electrode material to a certain extent. Under high current density, the capacity attenuation of the positive electrode material is relatively serious, and it is difficult to meet the requirements of high-rate discharge of power vehicles. Summary of the invention
[0004] The object of the present invention is to provide a lithium ion ternary positive electrode material and a preparation method thereof, and a lithium ion battery, which can improve the cycle performance of the lithium ion ternary positive electrode material.
[0005] To achieve the above object, the present invention provides the following technical solution: a method for preparing a lithium ion ternary positive electrode material, comprising: Preparation of single crystal active particles using ternary precursors and lithium source materials; The single crystal active particles and the coating material are mixed in a first preset ratio and subjected to a first sintering to form a coating layer on the surface of the single crystal active particles, wherein the coating material comprises a lithium compound, a titanium compound and a first dopant, and the coating layer comprises lithium titanate and a first doping element, and the first doping element is one or more of Mg, Al, Zr, Er, Sr, Nd, Y and W, and the first preset ratio makes the coating layer account for 0.05% to 5% of the total mass of the positive electrode material.
[0006] The first dopant is one or more of oxides, halides, hydroxides, metal organics, metal fluorides, nitrates, sulfates, carbonates, phosphates and oxalates of the first doping element, or a composite oxide of the first doping element and other metal elements.
[0007] The lithium compound included in the coating material is one or more of lithium hydroxide, lithium carbonate and lithium oxalate, and the titanium compound included in the coating material is one or more of titanium dioxide, titanium hydroxide, titanium nitrate, titanium tetrachloride and titanium oxysulfate.
[0008] The temperature of the first sintering is 300° C. to 800° C., the sintering time is 3 h to 25 h, and air or oxygen is introduced during the sintering process.
[0009] Wherein, the temperature of the first sintering is 700° C. to 800° C., and the sintering time is 15 h to 18 h.
[0010] The step of preparing single crystal active particles using a ternary precursor and a lithium source material comprises: Provide the ternary precursor, the chemical formula of the ternary precursor is Ni x Co y Mn 1-x-y (OH)2, where 0≤x≤1, 0≤y≤1, x+y≤1; The lithium source material, the ternary precursor, and the second dopant are mixed in a second preset ratio, and a second sintering is performed to obtain the single crystal active particle; wherein the second dopant is a compound including a second doping element, and the second preset ratio makes the chemical formula of the single crystal active particle Li n Ni x Co y Mn 1-x-y M m O2 holds true, wherein 0.95≤n≤1.2, M represents the second doping element, and 0.01≤m≤0.10.
[0011] The second doping element is one or more of Mg, Al, Zr, Er, Sr, Nd, Y and W, and the second dopant is one or more of oxides, halides, hydroxides, metal organics, metal fluorides, nitrates, sulfates, carbonates, phosphates and oxalates of the second doping element, or a composite oxide of the second doping element and other metal elements.
[0012] To achieve the above object, the present invention also provides the following technical solution: a lithium ion ternary positive electrode material prepared by the preparation method described in the above technical solution, the positive electrode material comprising single crystal active particles and a coating layer coating the surface of the single crystal active particles; The coating layer includes lithium titanate and a first doping element, and the first doping element is one or more of Mg, Al, Zr, Er, Sr, Nd, Y and W, and the coating layer accounts for 0.05% to 5% of the total mass of the positive electrode material.
[0013] Wherein, the coating layer accounts for 0.05% to 2% of the total mass of the positive electrode material.
[0014] To achieve the above objectives, the present invention also provides the following technical solutions: a lithium-ion battery, comprising a lithium-ion ternary positive electrode material prepared according to the preparation method described in the above technical solution, or a lithium-ion ternary positive electrode material described in the above technical solution.
[0015] Compared with the prior art, the beneficial effects of the present invention are as follows: the present invention first prepares single crystal active particles, and then forms a lithium titanate coating layer containing a first doping element on the surface of the single crystal active particles, and limits the coating layer to 0.05% to 5% of the total mass of the positive electrode material, which can not only stabilize the layered structure of the positive electrode material and inhibit phase change during charging and discharging, but also improve the conductivity of the coating layer, thereby improving the cycle performance of the battery. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the following briefly introduces the drawings required for describing the embodiments. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work. Among them: Figure 1 It is a schematic flow chart of an embodiment of a method for preparing a lithium-ion ternary positive electrode material according to the present invention; Figure 2 for Figure 1 A schematic flow chart of an implementation method of step S11; Figure 3 is the SEM photo of Example 1; Figure 4 for Figure 1 TEM photo of Example 1; Figure 5 It is a comparison chart of the rate performance of the batteries corresponding to the comparative example and each embodiment; Figure 6 It is a comparison chart of 45°C cycle capacity retention rate of the batteries corresponding to the comparative example and each embodiment; Figure 7 It is a comparison chart of low temperature DCR data at 20% SOC of the batteries corresponding to the comparative example and each embodiment. DETAILED DESCRIPTION
[0017] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0018] See also Figure 1 , Figure 1 1 is a flow chart of an embodiment of a method for preparing a lithium-ion ternary positive electrode material according to the present invention. The method comprises the following steps S11-S12.
[0019] Step S11, preparing single crystal active particles using a ternary precursor and a lithium source material.
[0020] In this embodiment, a commercially available ternary precursor or a self-prepared ternary precursor may be used. The ternary precursor is then mixed with a lithium source material and additives that meet other application requirements and sintered, and the sintered material is then processed by crushing, grading, iron removal, and other processes to obtain single crystal active particles. The specific process details will be described below.
[0021] Step S12, mixing the single crystal active particles and the coating material according to a first preset ratio, and performing a first sintering to form a coating layer on the surface of the single crystal active particles, wherein the coating material includes a lithium compound, a titanium compound and a first dopant, and the coating layer includes lithium titanate and a first doping element, and the first doping element is one or more of Mg, Al, Zr, Er, Sr, Nd, Y and W, and the first preset ratio makes the coating layer account for 0.05% to 5% of the total mass of the positive electrode material.
[0022] The first doping elements are all metal elements and exist in the coating layer in the form of metal cations. After many experiments, the present embodiment limits the coating layer to 0.05% to 5% of the total mass of the positive electrode material, for example, 0.1%, 0.2%, 0.5%, 0.8%, 1%, 1.5%, 2%, 3%, 4%, 5%, etc. Within this range, the performance of the positive electrode material can be better improved.
[0023] The first dopant is one or more of oxides, halides, hydroxides, metal organics, metal fluorides, nitrates, sulfates, carbonates, phosphates and oxalates of the first doping element, or a composite oxide of the first doping element and other metal elements.
[0024] The lithium compound included in the coating material is one or more of lithium hydroxide, lithium carbonate and lithium oxalate, and the titanium compound included in the coating material is one or more of titanium dioxide, titanium hydroxide, titanium nitrate, titanium tetrachloride and titanium oxysulfate.
[0025] Wherein, the temperature of the first sintering is 300°C to 800°C, such as 350°C, 500°C, 600°C, 700°C, 750°C, 780°C, etc., and the sintering time is 3h to 25h, such as 4h, 6h, 10h, 12h, 15h, 16h, 17h, 18h, 20h, 24h, etc., and air or oxygen is introduced during the sintering process. In some embodiments, it is preferred that the temperature of the first sintering is 700°C to 800°C, and the sintering time is 15h to 18h.
[0026] It is understandable that the sintered material can be processed by crushing, grading, screening, iron removal and other processes as needed, and these processing processes can be carried out according to the schemes disclosed in the prior art.
[0027] In this embodiment, single-crystal active particles are first prepared, and then a lithium titanate coating layer containing a first doping element is formed on the surface of the single-crystal active particles, and the coating layer is limited to 0.05% to 5% of the total mass of the positive electrode material. This can not only stabilize the layered structure of the positive electrode material and inhibit phase changes during charging and discharging, but also improve the conductivity of the coating layer, thereby improving the cycle performance of the battery.
[0028] In some embodiments, see Figure 2 , single crystal active particles are prepared through the following steps S21-S22.
[0029] Step S21, providing a ternary precursor, the chemical formula of the ternary precursor is Ni x Co y Mn 1-x-y (OH)2, where 0≤x≤1, 0≤y≤1, x+y≤1.
[0030] Specifically, the ternary precursor can be prepared by the following steps AD: A. Solution preparation: Prepare a mixed salt solution L1 of nickel, cobalt and manganese in a molar ratio of Ni:Co:Mn=x:y:1-xy, so that the metal ion concentration in the salt solution is 0.5-3 mol / L; prepare an alkali solution with a concentration of 1.5-12 mol / L, such as a mixed solution of one or more of sodium hydroxide, potassium hydroxide and lithium hydroxide; prepare a complexing agent solution with a concentration of 0.5-5 mol / L, and the complexing agent is a mixed solution of one or more of ammonia water, ammonium bicarbonate, ammonium sulfate, ammonium carbonate, citric acid and disodium ethylenediaminetetracarboxylate.
[0031] B. Preparation of initial solution: Pour pure water into the reaction vessel, and adjust the pH value of the solution to 8.5-13.5 with alkaline solution, and maintain the temperature in the reaction vessel at 40-80°C, while introducing inert gas throughout the entire reaction process.
[0032] C. Reaction of precursor: Add L1 solution into the reaction vessel, control the flow rate to 5-30 L / min, slowly add appropriate amount of complexing agent and alkaline solution, maintain the temperature in the reaction vessel at 40-80°C, and adjust the stirring speed to 120-950 r / min.
[0033] D. Solid-liquid separation: The material in step C is transferred to a aging tank for solid-liquid separation, and the solid material obtained by solid-liquid separation is washed with deionized water and dried to obtain the desired ternary precursor. In this embodiment, the D50 range of the ternary precursor is 2 to 8 μm.
[0034] Step S22, mixing the lithium source material, the ternary precursor, and the second dopant according to a second preset ratio, and performing a second sintering to obtain single crystal active particles; wherein the second dopant is a compound including a second doping element, and the second preset ratio makes the chemical formula of the single crystal active particles Li n Ni x Co y Mn 1-x-y M m O2 holds true, where 0.95≤n≤1.2, M represents a second doping element, and 0.01≤m≤0.10.
[0035] The lithium source material is selected from one or more of lithium hydroxide, lithium carbonate and lithium oxalate. The second doping element is one or more of Mg, Al, Zr, Er, Sr, Nd, Y and W. The second dopant is one or more of the oxide, halide, hydroxide, metal organic, metal fluoride, nitrate, sulfate, carbonate, phosphate and oxalate of the second doping element, or a composite oxide of the second doping element and other metal elements.
[0036] The second sintering temperature is 550-950° C., the sintering time is 4-40 hours, and air or oxygen is introduced during the sintering process.
[0037] In this embodiment, the ternary precursor is a continuous coprecipitation reaction, each element is evenly mixed, the reaction is sufficient, and it is conducive to the control of morphology, so that the particle size of the single crystal active particles prepared by the ternary precursor is more consistent, which is beneficial to further improve the performance of the positive electrode material. In addition, the second doping element can promote the stability of the single crystal active particles, thereby improving the structural stability of the positive electrode material.
[0038] Based on the same inventive concept, the present invention also provides a lithium ion ternary positive electrode material prepared according to the preparation method described in the above embodiment, the positive electrode material includes single crystal active particles and a coating layer coating the surface of the single crystal active particles. Wherein, the coating layer includes lithium titanate and a first doping element, and the first doping element is one or more of Mg, Al, Zr, Er, Sr, Nd, Y and W, and the coating layer accounts for 0.05% to 5% of the total mass of the positive electrode material. In a preferred embodiment, the coating layer accounts for 0.05% to 2% of the total mass of the positive electrode material. This embodiment has the same beneficial effects as the above embodiment, which will not be repeated here.
[0039] Based on the same inventive concept, the present invention also provides a lithium-ion battery, including a lithium-ion ternary positive electrode material prepared according to the preparation method described in the above embodiment, or including the lithium-ion ternary positive electrode material described in the above embodiment. Of course, the lithium-ion battery also includes a negative electrode material, a separator, an electrolyte, etc. that can be obtained from the scheme disclosed in the prior art. The lithium-ion battery also has the same beneficial effects as the above embodiment, which will not be repeated here.
[0040] The performance improvement brought about by the technical solution of the present invention is explained below with reference to specific embodiments and comparative examples.
[0041] The single crystal active particles used in the following examples and comparative examples are all prepared by the following method: Step 1: prepare a 1.5 mol / L mixed solution L1 according to Ni:Co:Mn=0.7:0.1:0.2, prepare 1.5 mol / L sodium hydroxide solution and 0.5 mol / L ammonium sulfate solution; inject pure water into the reaction container, adjust the pH value to 11.5 with sodium hydroxide solution, maintain the temperature in the reaction container at 50°C, and introduce nitrogen; add L1 solution to the reaction container, control the flow rate of L1 solution to 5L / min, and slowly add sodium hydroxide solution and ammonium sulfate solution dropwise, maintain the temperature in the reaction container at 50°C, and adjust the stirring speed to 200 r / min; when the particle size reaches D50 of about 4μm, perform solid-liquid separation and drying to obtain the required ternary precursor S1.
[0042] Step 2: Lithium hydroxide, ternary precursor S1, and aluminum hydroxide are mixed according to the molecular formula Li n Ni x Co y Mn 1-x- y M mThe mixture is mixed in a ratio of n=1.05, x=0.70, y=0.10, and m=0.20 in O2, and the sintering temperature is controlled to be 950°C and the sintering time is 4h. Air is introduced during the sintering process. The sintered material is processed by crushing, grading, and iron removal to obtain the required single crystal active particles.
[0043] The positive electrode material prepared according to the following steps is recorded as a comparative example: The above-mentioned single crystal active particles, lithium carbonate (lithium compound), and titanium hydroxide (titanium compound) are mixed in a certain proportion, and then the mixed materials are subjected to the first sintering. The main sintering temperature is controlled at 800°C, the sintering time in the main temperature zone is 15h, and oxygen is introduced during the sintering process with a ventilation volume of 200 m 3 / h, and after sintering, a comparative positive electrode material is obtained, wherein the surface of the single crystal active particles is coated with a lithium titanate coating layer, which accounts for 1.00% of the total mass of the positive electrode material.
[0044] The positive electrode material prepared according to the following steps is recorded as Example 1: The above-mentioned single crystal active particles, lithium carbonate (lithium compound), titanium hydroxide (titanium compound), and aluminum oxide (first dopant) are mixed in a certain proportion, and then the mixed materials are subjected to the first sintering. The main sintering temperature is controlled at 800°C, the sintering time in the main temperature zone is 15h, and oxygen is introduced during the sintering process with a ventilation volume of 200 m 3 / h, after sintering, the positive electrode material of Example 1 is obtained, wherein the surface of the single crystal active particles is coated with a layer of Al-doped lithium titanate coating layer, which accounts for 1.00% of the total mass of the positive electrode material. Figure 3 SEM photos and Figure 4 From the TEM photograph, it can be seen that a coating layer is formed on the surface of the single crystal active particles.
[0045] The difference between Example 2 and Example 1 is that the first dopant is zirconium oxide, and in the obtained positive electrode material of Example 2, the surface of the single crystal active particles is coated with a Zr-doped lithium titanate coating layer.
[0046] Embodiment 3 is different from Embodiment 1 in that the first dopant is magnesium oxide, and in the obtained positive electrode material of Embodiment 3, the surface of the single crystal active particles is coated with a Mg-doped lithium titanate coating layer.
[0047] Example 4 is different from Example 1 in that the first dopant is yttrium oxide, and in the obtained positive electrode material of Example 4, the surface of the single crystal active particles is coated with a Y-doped lithium titanate coating layer.
[0048] The difference between Example 5 and Example 1 is that the first dopant is tungsten oxide, and in the obtained positive electrode material of Example 5, the surface of the single crystal active particles is coated with a W-doped lithium titanate coating layer.
[0049] The positive electrode materials of the above comparative example and Examples 1 to 5 were made into batteries and various key technical indicators such as charge and discharge capacity were tested. The test results are as follows: Figure 5-Figure 7 shown.
[0050] from Figure 5 It can be seen that after the first doping element is doped into the lithium titanate coating layer, the specific capacity at different rates is improved, especially at high rates, the improvement is obvious, among which Example 1 performs the best. Figure 6 It can be seen that the cycle performance of different embodiments is improved compared with the comparative example, among which embodiment 1 performs the best. Figure 7 It can be seen that the resistance values of various embodiments at 20% SOC at -10°C are reduced to varying degrees, among which the reduction in Example 1 is the most obvious. This shows that the present invention can not only stabilize the layered structure of the positive electrode material and inhibit the phase change during the charge and discharge process through the process of doping the lithium titanate coating layer with metal cations, but also improve the conductivity of the coating layer, thereby improving the cycle performance of the battery, improving the safety performance and high temperature performance of the battery material, and effectively improving the problem of high DCR of the positive electrode material at low temperature and low SOC.
[0051] Moreover, the ternary precursor in the present invention is a continuous co-precipitation reaction, the elements are evenly mixed, the reaction is sufficient, it is beneficial to the control of the morphology, and continuous production is implemented, which improves the production efficiency and makes the material particle size more consistent.
[0052] The above description is only an implementation mode of the present invention, and does not limit the patent scope of the present invention. Any equivalent structure or equivalent process transformation made by using the contents of the present invention specification and drawings, or directly or indirectly applied in other related technical fields, are also included in the patent protection scope of the present invention.
Claims
1. A method for preparing a lithium-ion ternary positive electrode material, characterized in that: include: Preparation of single crystal active particles using ternary precursors and lithium source materials; The single crystal active particles and the coating material are mixed in a first preset ratio and subjected to a first sintering to form a coating layer on the surface of the single crystal active particles, wherein the coating material comprises a lithium compound, a titanium compound and a first dopant, and the coating layer comprises lithium titanate and a first doping element, and the first doping element is one or more of Mg, Al, Zr, Er, Sr, Nd, Y and W, and the first preset ratio makes the coating layer account for 0.05% to 5% of the total mass of the positive electrode material.
2. The preparation method according to claim 1, characterized in that: The first dopant is one or more of oxides, halides, hydroxides, metal organics, metal fluorides, nitrates, sulfates, carbonates, phosphates and oxalates of the first doping element, or a composite oxide of the first doping element and other metal elements.
3. The preparation method according to claim 1, characterized in that: The lithium compound included in the coating material is one or more of lithium hydroxide, lithium carbonate and lithium oxalate, and the titanium compound included in the coating material is one or more of titanium dioxide, titanium hydroxide, titanium nitrate, titanium tetrachloride and titanyl sulfate.
4. The preparation method according to any one of claims 1 to 3, characterized in that The first sintering temperature is 300° C. to 800° C., the sintering time is 3 h to 25 h, and air or oxygen is introduced during the sintering process.
5. The preparation method according to claim 4, characterized in that: The first sintering temperature is 700° C. to 800° C., and the sintering time is 15 h to 18 h.
6. The preparation method according to claim 1, characterized in that: The step of preparing single crystal active particles using a ternary precursor and a lithium source material comprises: providing the ternary precursor, wherein the chemical formula of the ternary precursor is Ni x Co y Mn 1-x-y (OH)2, where 0≤x≤1, 0≤y≤1, x+y≤1; The lithium source material, the ternary precursor, and the second dopant are mixed in a second preset ratio, and a second sintering is performed to obtain the single crystal active particle; wherein the second dopant is a compound including a second doping element, and the second preset ratio makes the chemical formula of the single crystal active particle Li n Ni x Co y Mn 1-x-y M m O2 holds true, wherein 0.95≤n≤1.2, M represents the second doping element, and 0.01≤m≤0.
10.
7. The preparation method according to claim 6, characterized in that: The second doping element is one or more of Mg, Al, Zr, Er, Sr, Nd, Y and W, and the second dopant is one or more of oxides, halides, hydroxides, metal organics, metal fluorides, nitrates, sulfates, carbonates, phosphates and oxalates of the second doping element, or a composite oxide of the second doping element and other metal elements.
8. A lithium ion ternary positive electrode material prepared by the preparation method according to any one of claims 1 to 7, characterized in that: The positive electrode material comprises single crystal active particles and a coating layer coating the surface of the single crystal active particles; The coating layer includes lithium titanate and a first doping element, and the first doping element is one or more of Mg, Al, Zr, Er, Sr, Nd, Y and W, and the coating layer accounts for 0.05% to 5% of the total mass of the positive electrode material.
9. The lithium ion ternary positive electrode material according to claim 8, characterized in that: The coating layer accounts for 0.05% to 2% of the total mass of the positive electrode material.
10. A lithium ion battery, characterized in that: It includes a lithium ion ternary positive electrode material prepared according to the preparation method according to any one of claims 1 to 7, or a lithium ion ternary positive electrode material according to claim 8 or 9.
Citation Information
Cited By
Positive electrode active material, and positive electrode and lithium secondary battery comprising same
WO2026142251A1