Single-crystal positive electrode active material and preparation method and application thereof

Through two combined calcination and grinding processes, a single crystal positive electrode active material was successfully prepared, which solved the problem of insufficient air stability and circulation performance of O3-type layered oxides in sodium ion batteries, and achieved a single-dimensional with low cost and excellent performance The preparation of crystal positive electrode material improves the overall performance of sodium ion batteries.

CN118993169APending Publication Date: 2024-11-22INSTITUTE OF PROCESS ENGINEERING CHINESE ACADEMY OF SCIENCES
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411063609.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-05
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The prior art is difficult to effectively improve the air stability and circulation performance of O3-type layered oxides in sodium ion batteries, and high-temperature sintering method cannot prepare high-performance single-crystal positive electrode active materials, and the preparation cost is relatively high.

Method used

Two combined calcination processes are adopted, and the prefixed material obtained from the first calcination is ground and then refired by the second calcination process to induce single crystal growth of grains. Combined with the grinding process, single crystal positive electrode active material is prepared, reducing costs and increasing Air stability and circulation properties of the material.

Benefits of technology

The effective preparation of single-crystal positive electrode active material is achieved, the air stability and electrochemical cycling performance of the material are improved, the preparation cost is reduced, and the stress concentration and side reaction problems of the material are alleviated under high voltage, which is improved. Cyclic stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118993169A_ABST
    Figure CN118993169A_ABST
Patent Text Reader

Abstract

The invention relates to a single-crystal positive electrode active material and a preparation method and application thereof, the preparation method comprises the following steps: (1) carrying out first calcination on a sodium source and a precursor material to obtain a pre-sintered material; and (2) grinding the pre-sintered material, and performing secondary calcination to obtain the single-crystal positive electrode active material. In the preparation method disclosed by the invention, the re-sintering process of performing second calcination on the pre-sintered material obtained by the first calcination induces the single crystal growth of crystal grains, and the re-sintering process is combined with the grinding process between the two times of calcination, so that the effective preparation of the single crystal positive electrode active material is realized, the air stability of the positive electrode active material is improved, and the service life of the positive electrode active material is prolonged. And the electrochemical cycle performance of the positive electrode active material is improved. In addition, the preparation process adopting two-time combined calcination has the advantages of low preparation cost and simplicity in operation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of batteries, and in particular to a single crystal positive electrode active material and a preparation method and application thereof. Background Art

[0002] As a technology with high energy conversion efficiency, electrochemical energy storage has attracted widespread attention. In particular, the development of lithium-ion batteries has greatly changed people's daily lives. They are used in 3C products, new energy vehicles, and energy storage systems that have rapidly emerged in recent years. However, the uneven distribution of raw material resources and high prices of lithium-ion batteries have limited their further development. Sodium-ion batteries have similar performance and abundant sodium resources in the earth's crust, which can greatly reduce costs and have potential application prospects in the field of energy storage.

[0003] Positive electrode materials are considered to be the key to developing high-performance sodium-ion batteries. O3-type layered oxides are considered to be highly promising positive electrode materials due to their high theoretical capacity and high sodium content. However, their actual capacity, cycle stability and air stability are still far below the requirements of energy storage devices. Currently, various strategies have been adopted to improve the performance of O3-type layered oxides, among which specific strategies include ion doping / substitution and coating.

[0004] Prior art CN117223124A discloses a high entropy oxide doped, coated and co-modified positive electrode material and its preparation method and application. High entropy oxide is a single-phase solid solution material in which multiple metal elements share the same atomic site and cations are randomly distributed. Due to the disorder of the metal layer, the metal elements tend to undergo random redox reactions, which can inhibit Na + / Vacancy order and charge order delay or inhibit phase change and improve the rate performance and cycle stability of electrode materials.

[0005] Prior art CN116031395A discloses a fluorine ion and / or vacancy doped sodium ion battery positive electrode material and its preparation method and application, in which a small amount of fluorine ions and / or vacancies are used to replace oxygen ions in the material to significantly improve the structural stability of the material as well as the sodium ion conductivity and electronic conductivity.

[0006] However, the O3-type layered oxides given in the above-mentioned prior art still need to be further improved in terms of air stability and cycle performance. In view of the problems of cycle performance and air stability of O3-type layered oxides, drawing on the commercial success of single-crystal positive electrodes of lithium-ion batteries, the strategy of using single-crystal positive electrode materials is introduced into the positive electrode of sodium-ion batteries, which can effectively alleviate the side reactions caused by material intercrystalline particle cracking and new interface exposure and electrolyte erosion caused by stress concentration under high voltage. At present, the main methods for preparing single-crystal positive electrodes are molten salt method, hydrothermal method and high-temperature sintering method. However, the first two methods require additional washing processes. Due to the large specific heat capacity of water, evaporating water undoubtedly increases the actual cost. The currently used high-temperature sintering process cannot effectively prepare single-crystal positive electrode active materials for high-performance sodium-ion batteries.

[0007] Therefore, providing a method for preparing positive electrode active materials, which can effectively achieve the preparation of single crystal positive electrode active materials with good air stability and excellent cycle performance while reducing the preparation cost, is an urgent problem to be solved. Summary of the invention

[0008] In order to solve the above technical problems, the purpose of the present invention is to provide a single crystal positive electrode active material and a preparation method and application thereof. In the preparation method of the present invention, the pre-calcined material obtained by the first calcination is subjected to a re-firing process of a second calcination, which induces the single crystal growth of the grains, and the re-firing process is combined with the grinding process between the two calcinations, so as to realize the effective preparation of the single crystal positive electrode active material, improve the air stability of the positive electrode active material, and improve the electrochemical cycle performance of the positive electrode active material. In addition, the preparation process of the two combined calcinations adopted by the present invention has the advantages of low preparation cost and simple operation.

[0009] To achieve this object, the present invention adopts the following technical solutions:

[0010] In a first aspect, the present invention provides a method for preparing a single crystal positive electrode active material, the preparation method comprising:

[0011] (1) calcining the sodium source and the precursor material to obtain a pre-calcined material;

[0012] (2) Grinding the pre-sintered material and subjecting it to a second calcination to obtain the single crystal positive electrode active material.

[0013] The preparation method provided by the present invention performs a second calcination re-firing process on the polycrystalline pre-fired material obtained by the first calcination after grinding. By re-firing the obtained pre-fired material, the single crystal growth of the grains is induced, and the effective preparation of the single crystal positive electrode active material is achieved, the air stability of the positive electrode active material is improved, and the electrochemical cycle performance of the positive electrode active material is improved. At the same time, a grinding process is also performed between the first calcination and the second calcination process in the present invention, which can improve the uniformity of the product, thereby ensuring the preparation of the single crystal positive electrode active material and improving the electrochemical performance of the material. In addition, the preparation process of the two combined calcinations adopted by the present invention has the advantages of low preparation cost and simple operation.

[0014] Preferably, the chemical formula of the precursor material in step (1) is Ni a Fe b Mn c M d (OH) e ;

[0015] Wherein, 0≤a≤0.6, 0≤b≤0.4, 0≤c≤0.6, 0≤d≤0.4, a+b+c+d=1, a, b and c are not 0 at the same time, and e satisfies the Ni a Fe b Mn c M d (OH) e The algebraic sum of the positive and negative valences of is 0;

[0016] The M includes M1 and / or M2, the M1 includes any one of Li, K, Cu, Ca or Mg or a combination of at least two thereof, and the M2 includes any one of Ti, Zr, Nb, Y or Al or a combination of at least two thereof.

[0017] Specifically, in the chemical formula of the precursor of the present invention, a can be 0.01, 0.03, 0.05, 0.1, 0.15, 0.2, 0.25, 0.3, 0.35, 0.4, 0.45, 0.5, 0.55 or 0.6, etc.; b can be 0.01, 0.03, 0.05, 0.1, 0.15, 0.2, 0.25, 0.3, 0.35 or 0.4, etc.; c can be 0. 0.1, 0.15, 0.2, 0.25, 0.3, 0.35, 0.4, 0.45, 0.5, 0.55 or 0.6, etc.; d can be 0.01, 0.03, 0.05, 0.1, 0.15, 0.2, 0.25, 0.3, 0.35 or 0.4, etc.; but it is not limited to the listed values, and other values ​​not listed within the above numerical range are also applicable.

[0018] In the precursor material of the present invention, M1 is doped at the Ni position of the precursor material, and M2 is doped at the Mn position.

[0019] In one embodiment, the precursor material used in the present invention is an undoped hydroxide, and a single crystal positive electrode active material can be prepared by the preparation method provided by the present invention, thereby improving the air stability of the positive electrode active material and improving the electrochemical cycle performance of the positive electrode active material.

[0020] In one embodiment, the present invention uses an element-doped precursor material, which can introduce doping elements into the obtained single-crystal positive electrode active material, which is beneficial to alleviate the lattice strain phenomenon of the material under high voltage and inhibit the migration and dissolution of transition metals, and prevent the occurrence of intercrystalline cracks and surface side reactions during the cycle, thereby further improving the cycle stability of the battery. In the preparation method provided by the present invention, the element-doped precursor and the re-firing process used in the preparation work together to achieve the successful preparation of the single-crystal positive electrode active material, and at the same time, further improve the air stability and electrochemical cycle performance of the single-crystal positive electrode active material.

[0021] Preferably, the M includes M1 and M2, and the molar ratio of M1 to M2 is 1:(0.01-10), for example, 1:0.01, 1:0.02, 1:0.05, 1:0.1, 1:0.3, 1:0.5, 1:1, 1:2, 1:3, 1:4, 1:5, 1:6, 1:7, 1:8, 1:9 or 1:10, etc.

[0022] Preferably, the M1 includes Cu.

[0023] Preferably, the M2 includes Ti and / or Zr.

[0024] Preferably, M2 comprises Ti and Zr, and the molar ratio of Ti to Zr is (0.01-10): 1. For example, 0.01: 1, 0.02: 1, 0.05: 1, 0.1: 1, 0.3: 1, 0.5: 1, 1: 1, 2: 1, 3: 1, 4: 1, 5: 1, 6: 1, 7: 1, 8: 1, 9: 1 or 10: 1, etc.

[0025] Preferably, the sodium source in step (1) comprises any one of sodium carbonate, sodium hydroxide, sodium bicarbonate, sodium oxide, sodium nitrate or organic acid sodium salt, or a combination of at least two thereof.

[0026] Preferably, the sodium source comprises any one of sodium carbonate, sodium hydroxide or sodium bicarbonate or a combination of at least two thereof, preferably sodium carbonate and / or sodium hydroxide.

[0027] Preferably, the molar ratio of the precursor material to the sodium source in step (1) is 1:(0.8-1.1), for example, 1:0.8, 1:0.9, 1:1.0 or 1:1.1, etc.

[0028] The present invention regulates the amount of sodium source, and cooperates with the re-firing process in the preparation process, which can effectively solve the problem of impurity generation in the preparation process, reduce the collapse of the crystal structure, and help to obtain high-purity single crystal particles, thereby avoiding the low discharge capacity of the battery in the first week caused by the presence of impurities in the positive electrode active material. At the same time, regulating the amount of sodium source and the re-firing process can jointly improve the electrochemical properties of the material, especially the cycle performance and air stability.

[0029] In addition, if the molar ratio of the precursor material to the sodium source in the present invention is too high, it will make it difficult for the material to form an O3 stacking state; if the molar ratio of the two is too low, a large amount of surface residual alkali will remain on the surface of the material, forming a higher overpotential, which will deteriorate the electrochemical performance of the material.

[0030] In the preparation method of the present invention, by adopting the re-firing process, selecting the type of doping elements in the precursor material and regulating the amount of the sodium source, the three are compounded with each other, so that the effective preparation of the single crystal positive electrode active material can be achieved, thereby improving the air stability of the positive electrode active material, and jointly promoting the improvement of the comprehensive performance of the sodium ion battery in terms of the first week discharge capacity, cycle stability and electrochemical stability under air storage.

[0031] Preferably, before the first calcination in step (1), the sodium source and the precursor material are further mixed.

[0032] In the present invention, the mixing method is not limited, and it can be ball milling mixing, oscillation mixing or stirring mixing, and those skilled in the art can select according to their needs.

[0033] Preferably, the first calcination heating rate in step (1) is 1-15°C / min, for example, 1°C / min, 3°C / min, 5°C / min, 7°C / min, 9°C / min, 11°C / min, 13°C / min or 15°C / min, etc.

[0034] Preferably, the first calcination in step (1) includes a first insulation stage and a second insulation stage.

[0035] Preferably, the temperature of the first insulation stage is 400-500°C, for example, 400°C, 410°C, 420°C, 430°C, 440°C, 450°C, 460°C, 470°C, 480°C, 490°C or 500°C.

[0036] Preferably, the first insulation stage lasts for 4-6 hours, such as 4 hours, 4.5 hours, 5 hours, 5.5 hours or 6 hours.

[0037] The first heat preservation stage in the first calcination process of the present invention is to eliminate the crystal water in the precursor. Under a specific temperature range and a suitable time range, the crystal water can be eliminated as much as possible, thereby improving the performance of the material.

[0038] Preferably, the temperature of the second insulation stage is 850-950°C, for example, 850°C, 860°C, 870°C, 880°C, 890°C, 900°C, 910°C, 920°C, 930°C, 940°C or 950°C.

[0039] The second heat preservation stage in the first calcination process of the present invention adopts a specific temperature, which can make the sodium source and the precursor solution fully react to obtain a polycrystalline positive electrode active material. If the temperature of the second heat preservation stage in the first calcination process of the present invention is too high, the transition metal ions will precipitate into phases separately, and the active electrode pairs will decrease, resulting in a decrease in the first-week discharge capacity of the battery; if the temperature of the second heat preservation stage is too low, the crystallinity of the polycrystalline material will be poor, which is not conducive to the release of performance.

[0040] Preferably, the second insulation stage lasts for 10-20 hours, such as 10 hours, 11 hours, 12 hours, 13 hours, 14 hours, 15 hours, 16 hours, 17 hours, 18 hours, 19 hours or 20 hours, etc., preferably 15-20 hours.

[0041] Preferably, the first calcination in step (1) is carried out in an oxygen-containing atmosphere.

[0042] Preferably, the gas in the oxygen-containing atmosphere includes any one of air or oxygen.

[0043] Preferably, the gas in the oxygen-containing atmosphere further includes any one of nitrogen or inert gas.

[0044] Optionally, the pre-sintered material obtained by natural cooling after the first calcination in the present invention is then subjected to a grinding process and a second calcination process in sequence.

[0045] Preferably, the second calcination heating rate in step (2) is 1-15°C / min, for example, 1°C / min, 3°C / min, 5°C / min, 7°C / min, 9°C / min, 11°C / min, 13°C / min or 15°C / min, etc.

[0046] Preferably, the temperature of the second calcination in step (2) is 1000°C-1100°C, for example, 1000°C, 1010°C, 1020°C, 1030°C, 1040°C, 1050°C, 1060°C, 1070°C, 1080°C, 1090°C or 1100°C, etc., preferably 1025°C-1075°C.

[0047] The present invention adopts a second calcination process to re-sinter the pre-sintered material obtained by the first calcination, which can promote the complete conversion of the polycrystalline pre-sintered material obtained by the first calcination into a single crystal positive electrode active material, thereby improving the performance of the positive electrode active material. In the present invention, if the temperature of the second calcination is too high, the sodium in the bulk phase of the material will volatilize severely, forming too many sodium vacancies, resulting in a decrease in the first-week discharge capacity of the battery; if the temperature of the second calcination is too low, the primary particles cannot grow, which is not conducive to the formation of a micron-level single crystal morphology.

[0048] Preferably, the second calcination time in step (2) is 10-20 h, for example 10 h, 11 h, 12 h, 13 h, 14 h, 15 h, 16 h, 17 h, 18 h, 19 h or 20 h, etc., preferably 15-20 h.

[0049] Preferably, the second calcination in step (2) is carried out in an oxygen-containing atmosphere.

[0050] Preferably, the gas in the oxygen-containing atmosphere includes any one of air or oxygen.

[0051] Preferably, the gas in the oxygen-containing atmosphere further includes any one of nitrogen or inert gas.

[0052] In a second aspect, a single crystal positive electrode active material is prepared by the preparation method described in the first aspect.

[0053] The single crystal positive electrode active material provided by the present invention has excellent air stability, excellent cycle performance, less impurities, high purity, and can effectively improve the first cycle discharge specific capacity of the battery.

[0054] Preferably, the chemical formula of the single crystal positive electrode active material is Na x Ni a Fe b Mn c M d O2;

[0055] Among them, 0.8≤x≤1, 0≤a≤0.6, 0≤b≤0.4, 0≤c≤0.6, 0≤d≤0.4, a+b+c+d=1, a, b and c are not 0 at the same time;

[0056] M includes M1 and / or M2, M1 includes any one or a combination of at least two of Li, K, Cu, Ca or Mg, and M2 includes any one or a combination of at least two of Ti, Zr, Nb, Y or Al.

[0057] Specifically, in the chemical formula of the single crystal positive electrode active material of the present invention, x may be 0.8, 0.82, 0.84, 0.86, 0.88, 0.9, 0.92, 0.94, 0.96, 0.98 or 1, etc.; a may be 0.01, 0.03, 0.05, 0.1, 0.15, 0.2, 0.25, 0.3, 0.35, 0.4, 0.45, 0.5, 0.55 or 0.6, etc.; b may be 0.01, 0.03, 0.05, 0.1, 0.15 , 0.2, 0.25, 0.3, 0.35 or 0.4, etc.; c can be 0.01, 0.03, 0.05, 0.1, 0.15, 0.2, 0.25, 0.3, 0.35, 0.4, 0.45, 0.5, 0.55 or 0.6, etc.; d can be 0.01, 0.03, 0.05, 0.1, 0.15, 0.2, 0.25, 0.3, 0.35 or 0.4, etc.; but it is not limited to the listed values, and other values ​​not listed within the above numerical range are also applicable.

[0058] The introduction of doping elements into the single crystal positive electrode active material of the present invention can effectively alleviate the stress concentration phenomenon of the material under high pressure and inhibit the migration and dissolution of transition metals, prevent the occurrence of intercrystalline cracks and surface side reactions during the cycle process, thereby further improving the cycle stability of the battery.

[0059] Preferably, the M includes M1 and M2, and the molar ratio of M1 to M2 is 1:(0.01-10), for example, 1:0.01, 1:0.02, 1:0.05, 1:0.1, 1:0.3, 1:0.5, 1:1, 1:2, 1:3, 1:4, 1:5, 1:6, 1:7, 1:8, 1:9 or 1:10, etc.

[0060] Preferably, the M1 includes Cu.

[0061] Preferably, the M2 includes Ti and / or Zr.

[0062] Preferably, M2 includes Ti and Zr, and the molar ratio of Ti to Zr is (0.01-10):1, for example, 0.01:1, 0.02:1, 0.05:1, 0.1:1, 0.3:1, 0.5:1, 1:1, 2:1, 3:1, 4:1, 5:1, 6:1, 7:1, 8:1, 9:1 or 10:1, etc.

[0063] Preferably, the D50 of the single crystal positive active material is 3 μm or more, for example, 3 μm, 3.2 μm, 3.4 μm, 3.6 μm, 3.8 μm, 4 μm, 4.2 μm, 4.4 μm, 4.6 μm, 4.8 μm or 5 μm.

[0064] The single crystal positive electrode active material of the present invention is a large-sized particle structure.

[0065] Optionally, the single crystal positive electrode active material of the present invention is a layered structure.

[0066] In a third aspect, the present invention provides a positive electrode, which includes the positive electrode active material as described in the second aspect.

[0067] In a fourth aspect, the present invention provides a sodium ion battery, comprising the positive electrode as described in the third aspect.

[0068] Compared with the prior art, the present invention has at least the following beneficial effects:

[0069] (1) In the preparation method provided by the present invention, the pre-calcined material obtained by the first calcination is subjected to a second calcination process, which induces the single crystal growth of the grains, and the combination of the calcination process and the grinding process between the two calcinations realizes the effective preparation of the single crystal positive electrode active material, improves the air stability of the positive electrode active material, and improves the electrochemical cycle performance of the positive electrode active material. In addition, the preparation process of the two combined calcinations adopted by the present invention has the advantages of low preparation cost and simple operation.

[0070] (2) In the preparation method of the present invention, by adopting the re-firing process, and regulating the type of doping elements in the precursor material and the amount of sodium source, the three are compounded with each other, which can achieve the effective preparation of single crystal positive electrode active materials, thereby improving the air stability of the positive electrode active materials, and jointly promoting the improvement of the first week discharge capacity, cycle stability and comprehensive performance of the electrochemical stability of the sodium ion battery under air storage.

[0071] (3) The single crystal positive electrode active material provided by the present invention has excellent air stability, excellent cycle performance, less impurities, high purity, and can effectively improve the first cycle discharge capacity of the battery. Furthermore, the introduction of doping elements into the single crystal positive electrode active material of the present invention can effectively alleviate the stress concentration phenomenon of the material under high pressure and inhibit the migration and dissolution of transition metals, prevent the occurrence of intercrystalline cracks and surface side reactions during the cycle, thereby further improving the cycle stability of the battery. BRIEF DESCRIPTION OF THE DRAWINGS

[0072] Figure 1 This is a SEM image of the positive electrode active material prepared in Example 1 of the present invention.

[0073] Figure 2 This is a first-week charge-discharge curve diagram of a type A battery assembled with the positive electrode active materials prepared in Examples 1 and 2 of the present invention.

[0074] Figure 3 This is a cross-sectional SEM image of a type A battery assembled with a pole piece made of the positive electrode active material prepared in Example 9 of the present invention after cycling for 100 cycles at 2.0-4.2V.

[0075] Figure 4 This is a charge and discharge curve diagram of the first week of a type A battery assembled with the positive electrode active material prepared in Example 9 of the present invention.

[0076] Figure 5 This is an XRD comparison chart of the positive electrode active materials prepared in Example 1, Example 10, Example 11 and Example 12 of the present invention.

[0077] Figure 6 The cycle curves of type A batteries assembled with the positive electrode active materials prepared in Example 1 and Comparative Example 1 of the present invention at 2.0-4.2V are shown.

[0078] Figure 7 This is a SEM image of the positive electrode active material prepared in Comparative Example 1 of the present invention.

[0079] Figure 8 This is a SEM image of the positive electrode active material prepared in Comparative Example 2 of the present invention.

[0080] Fig. 9 This is a SEM image of the positive electrode active material prepared in Comparative Example 4 of the present invention. DETAILED DESCRIPTION

[0081] The technical solution of the present invention is further described below in conjunction with the accompanying drawings and through specific implementation methods. However, the following examples are only simplified examples of the present invention and do not represent or limit the scope of protection of the present invention. The scope of protection of the present invention shall be subject to the claims.

[0082] The hydroxide precursor materials used in the following examples are obtained by the preparation method in Example 1 of CN116969521A, with the only difference being that the types and proportions of the raw materials are regulated according to the types of elements in the precursor materials and the molar amounts of the elements.

[0083] Example 1

[0084] This embodiment provides a method for preparing a positive electrode active material, the preparation method comprising the following steps:

[0085] (1) Spherical Ni 0.3 Fe 0.2 Mn0.25 Cu 0.1 Ti 0.1 Zr 0.05 (OH) 2.3 The mixture was mixed with sodium carbonate at a molar ratio of 1:1.05 for 10 min, heated to 450°C at a heating rate of 5°C / min in an air atmosphere, kept warm for 5 h, then heated to 900°C at a heating rate of 5°C / min, kept warm for 15 h, and naturally cooled to 150°C to obtain a pre-sintered material;

[0086] (2) The pre-sintered material was fully ground, and then the ground product was heated to 1050°C at a heating rate of 10°C / min in an air atmosphere and kept at that temperature for 15 h, and then naturally cooled to 150°C to obtain Na 0.95 Ni 0.3 Fe 0.2 Mn 0.25 Cu 0.1 Ti 0.1 Zr 0.05 O2 single crystal positive electrode active material.

[0087] This embodiment also provides a positive electrode active material obtained by the above preparation method, which is a single crystal material with a layered structure and a chemical formula of Na 0.95 Ni 0.3 Fe 0.2 Mn 0.25 Cu 0.1 Ti 0.1 Zr 0.05 O2, particle size D50 is 5μm.

[0088] Example 2

[0089] This embodiment provides a method for preparing a positive electrode active material, the preparation method comprising the following steps:

[0090] (1) Spherical Ni 0.35 Fe 0.1 Mn 0.35 Cu 0.1 Ti 0.05 Zr 0.05 (OH) 2.2 The mixture was mixed with sodium hydroxide at a molar ratio of 1:1.08 for 10 minutes, heated to 400°C at a heating rate of 3°C / min in an air atmosphere, kept warm for 6 hours, then heated to 950°C at a heating rate of 3°C / min, kept warm for 18 hours, and naturally cooled to 150°C to obtain a pre-sintered material;

[0091] (2) The pre-sintered material was fully ground, and then the ground product was heated to 1025°C at a heating rate of 5°C / min in an air atmosphere and kept at that temperature for 20 h, and then naturally cooled to 150°C to obtain Na 0.98 Ni 0.35 Fe 0.1 Mn 0.35 Cu 0.1 Ti 0.05 Zr 0.05 O2 single crystal positive electrode active material.

[0092] This embodiment also provides an extremely active material obtained by the above preparation method, which is a single crystal material with a layered structure and a chemical formula of Na 0.98 Ni 0.35 Fe 0.1 Mn 0.35 Cu 0.1 Ti 0.05 Zr 0.05 O2, particle size D50 is 4μm.

[0093] Example 3

[0094] This embodiment provides a method for preparing a positive electrode active material, the preparation method comprising the following steps:

[0095] (1) Spherical Ni 0.4 Fe 0.1 Mn 0.25 Cu 0.05 Ti 0.15 Zr 0.05 (OH) 2.4 The mixture was mixed with sodium carbonate at a molar ratio of 1:1.05 for 10 min, heated to 500°C at a heating rate of 15°C / min in an air atmosphere, kept warm for 4 h, then heated to 850°C at a heating rate of 15°C / min, kept warm for 20 h, and naturally cooled to 150°C to obtain a pre-sintered material;

[0096] (2) The pre-sintered material was fully ground, and then the ground product was heated to 1075°C at a heating rate of 15°C / min in an air atmosphere and kept at that temperature for 18 hours, and then naturally cooled to 150°C to obtain NaNi 0.4 Fe 0.1 Mn 0.25 Cu 0.05 Ti 0.15 Zr 0.05 O2 single crystal positive electrode material.

[0097] This embodiment also provides a positive electrode active material obtained by the above preparation method, which is a single crystal material with a layered structure and a chemical formula of NaNi 0.4 Fe0.1 Mn 0.25 Cu 0.05 Ti 0.15 Zr 0.05 O2, particle size D50 is 5μm.

[0098] Example 4

[0099] The preparation method provided in this embodiment is different from that in embodiment 1 only in that the precursor material in step (1) is replaced by Ni 0.3 Fe 0.2 Mn 0.25 Cu 0.1 Ti 0.15 (OH) 2.3 The rest of the contents are the same as those in Example 1.

[0100] Example 5

[0101] The preparation method provided in this embodiment is different from that in embodiment 1 only in that the precursor material in step (1) is replaced by Ni 0.3 Fe 0.2 Mn 0.35 Cu 0.1 Zr 0.05 (OH) 2.1 The rest of the contents are the same as those in Example 1.

[0102] Example 6

[0103] The preparation method provided in this comparative example is different from that in Example 1 only in that the precursor material in step (1) is replaced by Ni 0.3 Fe 0.2 Mn 0.4 Cu 0.1 (OH)2. The rest of the contents are the same as those in Example 1.

[0104] Example 7

[0105] The preparation method provided in this comparative example is different from that in Example 1 only in that the precursor material in step (1) is replaced by Ni 0.4 Fe 0.2 Mn 0.2 Ti 0.2 (OH) 2.4 The rest of the contents are the same as those in Example 1.

[0106] Example 8

[0107] The preparation method provided in this comparative example is different from that in Example 1 only in that the precursor material in step (1) is replaced by Ni 0.4 Fe 0.2 Mn 0.25 Zr 0.15 (OH)2.3 The rest of the contents are the same as those in Example 1.

[0108] Example 9

[0109] The preparation method provided in this embodiment is different from that in embodiment 1 only in that the precursor material in step (1) is replaced by Ni 0.4 Fe 0.2 Mn 0.4 (OH)2. The rest of the contents are the same as those in Example 1.

[0110] Example 10

[0111] The preparation method provided in this embodiment differs from that in embodiment 1 only in that: the spherical Ni 0.3 Fe 0. 2Mn 0.25 Cu 0.1 Ti 0.1 Zr 0.05 (OH) 2.3 The molar ratio of sodium carbonate is 1:1.3. The rest of the contents are the same as those in Example 1.

[0112] Embodiment 11

[0113] The preparation method provided in this embodiment differs from that in embodiment 1 only in that: the spherical Ni 0.3 Fe 0. 2Mn 0.25 Cu 0.1 Ti 0.1 Zr 0.05 (OH) 2.3 The molar ratio of sodium carbonate is 1:0.7. The rest of the contents are the same as those in Example 1.

[0114] Example 12

[0115] The preparation method provided in this embodiment differs from that in embodiment 1 only in that: the spherical Ni 0.3 Fe 0. 2Mn 0.25 Cu 0.1 Ti 0.1 Zr 0.05 (OH) 2.3 The molar ratio of sodium carbonate is 1:0.4. The rest of the contents are the same as those in Example 1.

[0116] Example 13

[0117] The preparation method provided in this embodiment is different from that in embodiment 1 only in that the temperature of the second heat preservation stage in the first calcination process in step (1) is replaced by 1000° C. The rest of the contents are the same as those in embodiment 1.

[0118] Embodiment 14

[0119] The preparation method provided in this embodiment is different from that in embodiment 1 only in that the temperature of the second heat preservation stage in the first calcination process in step (1) is replaced by 800° C. The rest of the contents are the same as those in embodiment 1.

[0120] Embodiment 15

[0121] The preparation method provided in this embodiment is different from that in embodiment 1 only in that the temperature of the second calcination process in step (2) is replaced by 1100° C. The rest of the contents are the same as those in embodiment 1.

[0122] Example 16

[0123] The preparation method provided in this embodiment is different from that in embodiment 1 only in that the temperature of the second calcination process in step (2) is replaced by 1000° C. The rest of the contents are the same as those in embodiment 1.

[0124] Embodiment 17

[0125] The preparation method provided in this embodiment is different from that in embodiment 1 only in that the temperature of the second calcination process in step (2) is replaced by 1150° C. The rest of the contents are the same as those in embodiment 1.

[0126] Embodiment 18

[0127] The preparation method provided in this embodiment is different from that in embodiment 1 only in that the temperature of the second calcination process in step (2) is replaced by 950° C. The rest of the contents are the same as those in embodiment 1.

[0128] Comparative Example 1

[0129] The preparation method provided in this comparative example is different from that in Example 1 only in that the spherical Ni 0.3 Fe 0.2 Mn 0.25 Cu 0.1 Ti 0.1 Zr 0.05 (OH) 2.3 The precursor material is replaced with a mixture of nickel monoxide (NiO), ferric oxide (Fe2O3), manganese dioxide (MnO2), copper oxide (CuO), zirconium oxide (ZrO) and titanium oxide (Ti2O3) in the same stoichiometric ratio. The rest of the contents are the same as those in Example 1.

[0130] Comparative Example 2

[0131] The preparation method provided in this comparative example is different from that in Example 1 only in that the second calcination process in step (2) is omitted, that is, the process of heating the ground product to 1050°C at a heating rate of 10°C / min in an air atmosphere for 15 hours and then naturally cooling it to 150°C is omitted, and the pre-sintered material obtained in step (1) is directly ground and used as the positive electrode active material. The rest of the contents are the same as in Example 1.

[0132] Comparative Example 3

[0133] The preparation method provided in this comparative example is different from that in Example 1 only in that the first calcination process in step (1) is omitted, that is, the spherical Ni 0.3 Fe 0.2 Mn 0.25 Cu 0.1 Ti 0.1 Zr 0.05 (OH) 2.3 The hydroxide precursor and sodium carbonate were shaken and mixed at a molar ratio of 1:1.05 for 10 minutes and fully ground. Then, the ground product was heated to 1050° C. at a heating rate of 10° C. / min in an air atmosphere for 15 hours, and then naturally cooled to 150° C. to obtain a positive electrode active material. The rest of the contents are the same as in Example 1.

[0134] Comparative Example 4

[0135] The preparation method provided in this comparative example is different from that in Example 1 only in that the grinding process of the pre-sintered material in step (2) is omitted. The rest of the contents are the same as those in Example 1.

[0136] Assembly of sodium-ion batteries:

[0137] (1) Preparation of positive electrode sheets: The positive electrode active materials in the above-mentioned embodiments and comparative examples were directly ground and mixed with carbon nanotubes and polytetrafluoroethylene binder in a mass ratio of 8:1:1, and then cut into 10 mm square electrode sheets. After accurately weighing their masses, the mass of the active material in the positive electrode sheets was calculated based on the formula composition ratio.

[0138] (2) Battery assembly:

[0139] The above-obtained square positive electrode sheet, a 16 mm diameter separator (glass fiber), a 15 mm diameter sodium sheet, a spring sheet, a gasket, etc. were assembled into a 2032 type testable button cell in a glove box (oxygen content less than 0.01 ppm, water content less than 0.01 ppm). Among them, the A-type battery is the positive electrode sheet prepared directly from the positive electrode active materials prepared in Examples 1-18 and Comparative Examples 1-4 and the button cell assembled; the B-type battery is the positive electrode sheet prepared from the positive electrode active materials prepared in Examples 1-18 and Comparative Examples 1-4 and the button cell assembled after being placed in the air for one week.

[0140] Performance testing method:

[0141] The Wuhan Blue Electric high-performance battery test system was used to test the electrochemical performance of the prepared positive electrode active material under high voltage conditions of 2.0-4.2V. The results are shown in Table 1:

[0142] Table 1

[0143]

[0144]

[0145] The test results show that:

[0146] (1) It can be seen from Examples 1 to 9 that in the preparation method provided by the present invention, the pre-calcined material obtained by the first calcination is subjected to a second calcination process, which induces the single crystal growth of the grains, and the calcination process is combined with the grinding process between the two calcinations to achieve the effective preparation of the single crystal positive electrode active material, improve the air stability of the positive electrode active material, and improve the electrochemical cycle performance of the positive electrode active material. Furthermore, the present invention also uses the element-doped precursor and the calcination process used to prepare the positive electrode active material to cooperate with each other and work together to achieve the successful preparation of the single crystal positive electrode active material, and at the same time, further improve the air stability of the single crystal positive electrode active material and the electrochemical cycle performance under high voltage.

[0147] Figure 1 This is a SEM image of the positive electrode active material obtained in Example 1. It can be seen from the image that the preparation method provided by the present invention can successfully prepare a single crystal material.

[0148] Figure 2 The first-week charge-discharge curves of the type A battery of the positive electrode active materials prepared in Example 1 and Example 2 show that the single-crystal positive electrode active material obtained in the present invention has a higher first-week discharge specific capacity.

[0149] Figure 3This is a cross-sectional SEM image of a Type A battery assembled with a pole piece directly made from the positive electrode active material prepared in Example 9 after 100 cycles at 2.0-4.2V. It can be seen from the figure that the single crystal positive electrode active material provided in Example 9 can still maintain a good single crystal morphology after 100 cycles at high voltage.

[0150] Figure 4 This is a first-week charge-discharge curve diagram of a type A battery assembled from a single crystal positive electrode active material prepared in Example 9. As can be seen from the diagram, the single crystal positive electrode active material obtained in the present invention has a higher first-week discharge specific capacity when used in a battery.

[0151] (2) By comparing Example 1 with Examples 10-12, it can be seen that the present invention can improve the first-week discharge capacity of the battery by further regulating the molar ratio of the precursor material to the sodium source and controlling the amount of the sodium source, and can improve the electrochemical properties of the material together with the re-firing process, especially the cycle performance and air stability. In the present invention, if the molar ratio of the precursor material to the sodium source is too high, it is difficult for the material to form an O3 stacking mode; if the molar ratio of the two is too low, a large amount of surface residual alkali will remain on the surface of the material, resulting in a higher overpotential and a lower first-week discharge capacity.

[0152] Figure 5 3 are XRD diagrams of the positive electrode active materials in Example 1, Example 10, Example 11 and Example 12. It can be seen from the figure that the present invention controls the amount of sodium source in combination with the re-firing process in the preparation process, which can effectively solve the problem of impure phase generation in the preparation process, reduce the collapse of the crystal structure, and help to obtain high-purity single crystal particles. Compared with Examples 10-12, the impure peak phase of NiO on the XRD curve of the positive electrode active material prepared in Example 1 is weaker.

[0153] (3) By comparing Example 1 with Examples 13-14, it can be seen that the temperature of the second insulation stage in the first calcination process of the present invention is too high, the transition metal ions are precipitated into phases separately, the active electrode pairs are reduced, and the discharge specific capacity is reduced; if the temperature of the second insulation stage is too low, the crystallinity of the polycrystalline material is poor, which is not conducive to the release of performance.

[0154] (4) By comparing Example 1 with Examples 15-18, it can be seen that the second calcination process of the present invention is to convert the polycrystalline pre-sintered material into a single crystal positive electrode active material as completely as possible, thereby improving the performance of the positive electrode active material. In the present invention, if the temperature of the second calcination is too high, the sodium in the bulk phase of the material will volatilize severely, forming too many sodium vacancies, thereby reducing the discharge specific capacity; if the temperature of the second calcination is too low, the primary particles cannot grow, which is not conducive to the formation of a micron-sized single crystal morphology.

[0155] (5) By comparing Example 1 with Comparative Example 1, it can be seen that if the positive electrode material is not fired using a hydroxide spherical precursor, the electrochemical performance of the prepared positive electrode material is poor and cannot meet the requirements of commercial use.

[0156] Figure 6 The 1C cycle curve diagram of the type A battery assembled with the positive electrode active materials prepared in Example 1 and Comparative Example 1 at 2.0-4.2V. It can be seen from the figure that compared with Example 1, the positive electrode active material prepared in Comparative Example 1 is used in a sodium ion battery, and the capacity retention rate after 400 cycles is poor.

[0157] Figure 7 is the SEM image of the positive electrode active material prepared in Comparative Example 1. Figure 7 It can be seen that the positive electrode active material prepared by the traditional solid phase method cannot obtain a single crystal morphology.

[0158] (6) It can be seen from Example 1 and Comparative Example 2 that if the second calcination process is omitted in the present invention, a single crystal positive electrode active material cannot be formed, and the obtained positive electrode active material has poor stability in air, thereby significantly reducing the cycle performance of the battery.

[0159] Figure 8 is the SEM image of the positive electrode active material prepared in Comparative Example 2. Figure 8 It can be seen that the positive electrode material prepared by omitting the second calcination (re-firing) process has serious agglomeration between the primary particles and cannot form a single crystal morphology.

[0160] (7) It can be seen from Example 1 and Comparative Example 3 that if the first calcination process is omitted in the present invention, the electrochemical performance of the prepared positive electrode material is poor and cannot meet the requirements of commercial use.

[0161] (8) By comparing Example 1 with Comparative Example 4, it can be seen that the grinding process between the first calcination process and the second calcination process in the present invention can appropriately improve the uniformity of the product, thereby ensuring good electrochemical performance. If the grinding process is omitted, the overall performance of the battery will deteriorate.

[0162] Fig. 9 This is the SEM image of the positive electrode active material prepared in Comparative Example 4. Fig. 9 It can be seen that the primary particles of the positive electrode material prepared by omitting the grinding step are severely agglomerated, which is not conducive to the formation of single crystal morphology.

[0163] In the preparation method of the present invention, the pre-calcined material obtained by the first calcination is subjected to a re-sintering process of the second calcination, which induces the single crystal growth of the grains, and the re-sintering process is combined with the grinding process between the two calcinations, so as to realize the effective preparation of the single crystal positive electrode active material, improve the air stability of the positive electrode active material, and improve the electrochemical cycle performance of the positive electrode active material. In addition, the preparation process of the two combined calcinations adopted by the present invention has the advantages of low preparation cost and simple operation.

[0164] The applicant declares that the above is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention shall fall within the protection scope and disclosure scope of the present invention.

Claims

1. A method for preparing a single crystal positive electrode active material, characterized in that: The preparation method comprises: (1) calcining the sodium source and the precursor material to obtain a pre-calcined material; (2) Grinding the pre-sintered material and subjecting it to a second calcination to obtain the single crystal positive electrode active material.

2. The preparation method according to claim 1, characterized in that: The chemical formula of the precursor material in step (1) is Ni a Fe b Mn c M d (OH) e ; Wherein, 0≤a≤0.6, 0≤b≤0.4, 0≤c≤0.6, 0≤d≤0.4, a+b+c+d=1, a, b and c are not 0 at the same time, and e satisfies the Ni a Fe b Mn c M d (OH) e The algebraic sum of the positive and negative valences of is 0; The M includes M1 and / or M2, the M1 includes any one or a combination of at least two of Li, K, Cu, Ca or Mg, and the M2 includes any one or a combination of at least two of Ti, Zr, Nb, Y or Al; Preferably, the M comprises M1 and M2, and the molar ratio of M1 to M2 is 1:(0.01-10); Preferably, the M1 comprises Cu; Preferably, the M2 comprises Ti and / or Zr; Preferably, the M2 includes Ti and Zr, and the molar ratio of Ti to Zr is (0.01-10):

1.

3. The preparation method according to claim 1 or 2, characterized in that: The sodium source in step (1) includes any one of sodium carbonate, sodium hydroxide, sodium bicarbonate, sodium oxide, sodium nitrate or organic acid sodium salt, or a combination of at least two thereof; Preferably, the sodium source comprises any one of sodium carbonate, sodium hydroxide or sodium bicarbonate or a combination of at least two thereof, preferably sodium carbonate and / or sodium hydroxide.

4. The preparation method according to any one of claims 1 to 3, characterized in that: The molar ratio of the precursor material to the sodium source in step (1) is 1:(0.8-1.1); Preferably, before the first calcination in step (1), the sodium source and the precursor material are further mixed.

5. The preparation method according to any one of claims 1 to 4, characterized in that: Step (1) The heating rate of the first calcination is 1-15°C / min; Preferably, the first calcination in step (1) includes a first insulation stage and a second insulation stage; Preferably, the temperature of the first insulation stage is 400-500°C; Preferably, the first insulation stage lasts for 4-6 hours; Preferably, the temperature of the second insulation stage is 850-950°C; Preferably, the second insulation stage lasts for 10-20 hours, preferably 15-20 hours; Preferably, the first calcination in step (1) is carried out in an oxygen-containing atmosphere; Preferably, the gas in the oxygen-containing atmosphere includes any one of air or oxygen; Preferably, the gas in the oxygen-containing atmosphere further includes any one of nitrogen or inert gas.

6. The preparation method according to any one of claims 1 to 5, characterized in that: Step (2) the second calcination heating rate is 1-15°C / min; Preferably, the temperature of the second calcination in step (2) is 1000°C-1100°C, preferably 1025°C-1075°C; Preferably, the second calcination time in step (2) is 10-20 hours, preferably 15-20 hours; Preferably, the second calcination in step (2) is carried out in an oxygen-containing atmosphere; Preferably, the gas in the oxygen-containing atmosphere includes any one of air or oxygen; Preferably, the gas in the oxygen-containing atmosphere further includes any one of nitrogen or inert gas.

7. A single crystal positive electrode active material, characterized in that: The single crystal positive electrode active material is prepared by the preparation method according to any one of claims 1-6.

8. The single crystal positive electrode active material according to claim 7, characterized in that: The chemical formula of the single crystal positive electrode active material is Na x Ni a Fe b Mn c M d O2; Among them, 0.8≤x≤1, 0≤a≤0.6, 0≤b≤0.4, 0≤c≤0.6, 0≤d≤0.4, a+b+c+d=1, a, b and c are not 0 at the same time; M includes M1 and / or M2, M1 includes any one or a combination of at least two of Li, K, Cu, Ca or Mg, and M2 includes any one or a combination of at least two of Ti, Zr, Nb, Y or Al; Preferably, the M comprises M1 and M2, and the molar ratio of M1 to M2 is 1:(0.01-10); Preferably, the M1 comprises Cu; Preferably, the M2 comprises Ti and / or Zr; Preferably, the M2 comprises Ti and Zr, and the molar ratio of Ti to Zr is (0.01-10):1; Preferably, the particle size D50 of the single crystal positive electrode active material is greater than 3 μm.

9. A positive electrode, characterized in that The positive electrode comprises the single crystal positive electrode active material according to claim 7 or 8.

10. A sodium ion battery, characterized in that: The sodium ion battery comprises the positive electrode according to claim 9.