Layered oxide positive electrode material, preparation method thereof, positive electrode slurry, positive electrode plate and sodium ion battery

By coordinating cyanide, the precursor material of the cubic structure is formed and sintered to generate pore layered oxide positive electrode material, which solves the problems of impedance increase and volume strain of the materials in the circulating and storage process of sodium ion batteries, and achieves low internal resistance and High-speed performance improvement.

CN118993173APending Publication Date: 2024-11-22JIANGSU TIANHE ENERGY STORAGE CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411125434.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-16
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The layered oxide positive electrode material in existing sodium ion batteries is prone to gas production during circulation and storage, resulting in increased impedance, reduced rate performance, cycle failure and expansion force, and the sheet structure of the single crystal material is de-lacked in Na+ During the embedding process, we face the problems of volume strain and electrochemical contact deterioration.

Method used

M-CN bond is formed by cyanide coordination metal bonds, and the precursor substance with a cube structure is induced to synthesize and sinter it with sodium source to generate a layered oxide positive electrode material with pores, reducing the volume strain during charge and discharge de-embedding process , ensure the penetration of the electrolyte and the rapid deintercalation of Na+, and reduce internal resistance.

Benefits of technology

The low internal resistance, long cycle, high magnification and low expansion characteristics of sodium ion batteries are achieved, and the electrochemical performance of the material is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118993173A_ABST
    Figure CN118993173A_ABST
Patent Text Reader

Abstract

The invention discloses a layered oxide positive electrode material, a preparation method thereof, a positive electrode slurry, a positive electrode plate and a sodium ion battery, the preparation method comprises the following steps: (1) performing coordination precipitation on a metal salt and a substance containing a cyano group in the presence of an acidic substance, a complexing agent and a surfactant to prepare a precursor substance; (2) sintering the precursor substance and a sodium source to prepare a layered oxide positive electrode material; metal elements in the metal salt are selected from one or more of Ni, Fe, Mn, Cu, Zn, Ti and Co. The layered oxide positive electrode material prepared by the invention is beneficial to reduction of direct-current internal resistance of the sodium-ion battery, improvement of cycle performance, increase of multiplying power and reduction of expansive force.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of sodium ion batteries, and in particular relates to a layered oxide positive electrode material, a preparation method thereof, a positive electrode slurry, a positive electrode sheet and a sodium ion battery. Background Art

[0002] In the context of the fact that the cost of raw materials for lithium-ion batteries is not rising, sodium-ion batteries, which have similar electrochemical working principles to lithium-ion batteries, have attracted widespread attention due to their low cost and wide sources. Among sodium-ion batteries, layered oxide cathode materials have the most advantages in energy density, cycle performance and large-scale production. They have relatively high gram capacity and are expected to further improve energy density, becoming a substitute or supplement for lithium iron phosphate batteries. In the future, they are expected to be widely used in start-stop power supplies, A00-class vehicles, home energy storage, industrial and commercial energy storage, and large-scale energy storage.

[0003] Layered oxide materials for sodium ion batteries can be subdivided into polycrystalline materials and single crystal materials. Polycrystalline materials have lower impedance, but are prone to gassing during circulation and storage. Single crystal materials have relatively small particle size and low surface residual alkali. Single crystals sintered by conventional methods often show a large amount of growth along the (003) inert surface, presenting a flaky structure, which is not conducive to Na + The rapid deintercalation and flake-structured single crystals in Na + The process of embedding and de-embedding often faces large volume strain. The volume strain along the c-axis direction often leads to the rupture of particles along this direction and the deterioration of electrochemical contact. These properties lead to increased impedance of sodium-ion batteries, reduced rate performance, cycle failure and increased expansion force.

[0004] Therefore, there is an urgent need to develop a layered oxide positive electrode material that can improve the internal resistance, rate performance, cycle performance and expansion force performance of sodium ion batteries. BRIEF DESCRIPTION OF THE DRAWINGS

[0005] Figure 1 This is an electron microscope image of the precursor material prepared in Example 1 of the present invention.

[0006] Figure 2 This is an electron microscope image of the layered oxide positive electrode material prepared in Example 1 of the present invention.

[0007] Figure 3 This is an electron microscope image of the layered oxide positive electrode material prepared in Comparative Example 2 of the present invention.

[0008] Figure 4 This is an electron microscope image of the precursor material prepared in Comparative Example 6 of the present invention.

[0009] Figure 5 This is an electron microscope image of the layered oxide positive electrode material prepared in Comparative Example 6 of the present invention.

[0010] Figure 6 This is an electron microscope image of the precursor material prepared in Comparative Example 7 of the present invention.

[0011] Figure 7 This is an electron microscope image of the layered oxide positive electrode material prepared in Comparative Example 7 of the present invention. Summary of the invention

[0012] In order to solve the problems existing in the prior art, the present invention provides a layered oxide positive electrode material and a preparation method thereof. The present invention forms an M-CN bond by coordinating a cyanide metal bond, inducing the synthesis of a precursor material having a cubic structure, and the precursor material has a relatively high active surface exposure; then the precursor material is sintered with a sodium source, and the cyanide group of the precursor material is thermally decomposed to generate CO2 and NO during the synthesis and calcination process. x The layered oxide cathode material has pores inside, and the layered oxide cathode material retains the cubic morphology of the precursor material to a certain extent after calcination, and the active surface is increased. The layered oxide cathode material with this structure can reduce the volume strain generated during the charge and discharge process of sodium insertion and removal, and fully ensure the penetration of the electrolyte and Na + The rapid deintercalation and reduction of impedance make the sodium ion battery containing the layered oxide positive electrode material of the present invention have the characteristics of low internal resistance, long cycle, high rate and low expansion.

[0013] Specifically, the present invention provides a method for preparing a layered oxide positive electrode material, the preparation method comprising the following steps:

[0014] (1) Coordinating and precipitating a metal salt and a substance containing a cyano group in the presence of an acidic substance, a complexing agent and a surfactant to obtain a precursor substance;

[0015] (2) sintering the precursor material with a sodium source to obtain a layered oxide positive electrode material;

[0016] The metal element in the metal salt is selected from one or more of Ni, Fe, Mn, Cu, Zn, Ti and Co.

[0017] In one or more embodiments, the metal elements in the metal salt include Ni and Mn, and optionally also include one or more of Fe, Cu, Zn, Ti and Co.

[0018] In one or more embodiments, in step (1), the metal salt is selected from one or more of sulfates, chlorides, acetates and oxalates.

[0019] In one or more embodiments, in step (1), the substance containing a cyano group is selected from one or more of sodium ferrocyanide, potassium ferrocyanide and potassium cobalt cyanide.

[0020] In one or more embodiments, in step (1), the acidic substance is selected from one or more of hydrochloric acid, sulfuric acid, acetic acid, oxalic acid and acetic acid.

[0021] In one or more embodiments, in step (1), the complexing agent is selected from one or more of sodium citrate, sodium ascorbate, sodium pyrophosphate, sodium oxalate and ethylenediamine sodium oxalate.

[0022] In one or more embodiments, in step (1), the surfactant is polyvinyl pyrrolidone and / or sodium dodecylbenzene sulfonate.

[0023] In one or more embodiments, in step (1), the ratio of the sum of the amount of the cyano group in the cyano group-containing substance and the total amount of the metal element in the metal salt is 9:(1-3).

[0024] In one or more embodiments, in step (1), the ratio of the amount of the complexing agent to the sum of the total amount of the metal elements in the metal salt is 1:(1-10).

[0025] In one or more embodiments, in step (1), the ratio of the amount of the surfactant to the sum of the total amount of the metal elements in the metal salt is 1:(1-10).

[0026] In one or more embodiments, in step (1), the ratio of the sum of the amount of hydrogen ions in the acidic substance and the total amount of metal elements in the metal salt is 1:(1-5).

[0027] In one or more embodiments, in step (1), the temperature of the coordination precipitation is 10-70°C.

[0028] In one or more embodiments, in step (1), the coordination precipitation time is 4-8 hours.

[0029] In one or more embodiments, in step (1), a mixed solution comprising a metal salt, an acidic substance, a complexing agent and a surfactant is added to a solution comprising a substance containing a cyano group to perform a precipitation reaction to obtain a precursor substance; preferably, a peristaltic pump is used to drop the mixed solution of the metal salt, the acidic substance, the complexing agent and the surfactant; more preferably, the dropping speed is 0.5-1.5 mL·min -1 .

[0030] In one or more embodiments, in step (1), a mixed solution comprising a metal salt and an acidic substance is added to a solution comprising a cyano group-containing substance, a complexing agent and a surfactant to perform a precipitation reaction to obtain a precursor substance; preferably, a peristaltic pump is used to dropwise add the mixed solution of the metal salt and the acidic substance; more preferably, the dropping speed is 0.5-1.5 mL·min -1 .

[0031] In one or more embodiments, the method further comprises: after step (1) coordination precipitation, aging, separation, washing and drying to obtain a precursor material; preferably, the aging time is 20-28 hours; separation is performed by a centrifuge; washing is performed by water and / or ethanol; drying is performed by vacuum drying; and the drying temperature is 80-120°C.

[0032] In one or more embodiments, in step (2), the sodium source is sodium carbonate and / or sodium hydroxide.

[0033] In one or more embodiments, in step (2), the ratio of the amount of sodium element in the sodium source to the sum of the total amount of metal elements in the precursor material is (0.6-1.2):1.

[0034] In one or more embodiments, in step (2), the sintering temperature is 700-900°C;

[0035] In one or more embodiments, in step (2), the sintering time is 8-12 hours.

[0036] The invention provides a layered oxide positive electrode material prepared by the preparation method of the invention.

[0037] The present invention provides a positive electrode slurry, wherein the positive electrode slurry comprises a layered oxide positive electrode material prepared by the preparation method of the present invention or the layered oxide positive electrode material of the present invention.

[0038] The present invention provides a positive electrode plate, which comprises a current collector and an active material layer located on the surface of the current collector, wherein the active material layer is made of the positive electrode slurry of the present invention.

[0039] The present invention provides a sodium ion battery comprising the positive electrode plate of the present invention. DETAILED DESCRIPTION

[0040] In order to enable those skilled in the art to understand the characteristics and effects of the present invention, the following is a general description and definition of the terms and expressions mentioned in the specification and claims. Unless otherwise specified, all technical and scientific terms used in the text are the common meanings understood by those skilled in the art for the present invention. In the event of a conflict, the definition in this specification shall prevail.

[0041] The theories or mechanisms described and disclosed herein, whether correct or incorrect, should not limit the scope of the present invention in any way, that is, the present invention can be implemented without being limited by any specific theory or mechanism.

[0042] Herein, “comprising”, “including”, “containing” and similar terms encompass the meanings of “consisting essentially of” and “consisting of”. For example, when “A comprises B and C” is disclosed herein, “A consists essentially of B and C” and “A consists of B and C” should be deemed to be disclosed herein.

[0043] In this article, all features such as values, quantities, contents and concentrations defined in the form of numerical ranges or percentage ranges are only for brevity and convenience. Accordingly, the description of numerical ranges or percentage ranges should be considered to have included and specifically disclosed all possible secondary ranges and individual values ​​within the range (including integers and fractions).

[0044] In this document, unless otherwise specified, percentage refers to mass percentage and ratio refers to mass ratio.

[0045] Herein, when describing embodiments or examples, it should be understood that they are not used to limit the present invention to these embodiments or examples. On the contrary, all substitutes, improvements and equivalents of the methods and materials described in the present invention can be included in the scope limited by the claims.

[0046] In this document, in order to make the description concise, not all possible combinations of various technical features in various embodiments or examples are described. Therefore, as long as there is no contradiction in the combination of these technical features, the various technical features in various embodiments or examples can be combined arbitrarily, and all possible combinations should be considered to be within the scope of this specification.

[0047] In the present invention, the molar ratio is the ratio of the amounts of substances.

[0048] The present invention provides a method for preparing a layered oxide positive electrode material, the preparation method comprising the following steps:

[0049] (1) Coordinating and precipitating a metal salt and a substance containing a cyano group in the presence of an acidic substance, a complexing agent and a surfactant to obtain a precursor substance;

[0050] (2) sintering the precursor material with a sodium source to obtain a layered oxide positive electrode material;

[0051] In the present invention, the metal element in the metal salt may be one or more selected from Ni, Fe, Mn, Cu, Zn, Ti and Co, and the metal element in the metal salt may be represented by M.

[0052] In the present invention, the metal elements in the metal salt include Ni and Mn, and optionally include one or more of Fe, Cu, Zn, Ti and Co. In some embodiments, the metal elements in the metal salt include Ni, Mn and one or two selected from Cu and Zn, for example, the metal elements in the metal salt are Ni, Mn and Cu, and the metal elements in the metal salt are Ni, Mn and Zn.

[0053] The present invention prepares a precursor substance by coordinating and precipitating a metal salt and a substance containing a cyano group in the presence of an acidic substance, a complexing agent and a surfactant, that is, by forming an M-CN bond through the coordination of a cyanide metal bond, inducing the synthesis of a precursor substance having a cubic structure (such as Figure 1 The precursor material has a relatively high active surface exposure; the precursor material is then sintered with a sodium source to obtain a layered oxide positive electrode material. During the synthesis and calcination process, the cyanide group of the precursor material is thermally decomposed to generate CO2 and NO x etc., so that pores are formed inside the generated layered oxide cathode material, and the layered oxide cathode material retains the cubic morphology of the precursor material to a certain extent after calcination (such as Figure 2 As shown in Figure 2, the active surface increases, such as the ratio of (100), (010) and (110) surfaces. The layered oxide positive electrode material with this structure can reduce the volume strain generated during the charge and discharge process of sodium insertion and deintercalation, and fully ensure the penetration of the electrolyte and Na + The rapid deintercalation and reduction of impedance make the sodium ion battery containing the layered oxide positive electrode material of the present invention have the characteristics of low internal resistance, long cycle, high rate and low expansion.

[0054] In step (1), the metal salt may be one or more selected from sulfate, chloride, acetate and oxalate.

[0055] In step (1), the substance containing a cyano group may be one or more selected from sodium ferrocyanide, potassium ferrocyanide and potassium cobalt cyanide. In the present invention, cyanide and metal bonds coordinate to form M-CN bonds, inducing the synthesis of a precursor substance having a cubic structure, and after calcination, the layered oxide positive electrode material retains the cubic morphology of the precursor substance, so that the sodium ion battery containing the layered oxide positive electrode material of the present invention has the characteristics of low internal resistance, long cycle, high rate and low expansion.

[0056] In step (1), the acidic substance may be one or more selected from hydrochloric acid, sulfuric acid, acetic acid, oxalic acid and acetic acid. In the present invention, the acidic substance can provide a good reaction environment for metal ion complexation, avoid metal ion hydrolysis to form flocculent substances, and thus fail to combine well with the coordination group. Therefore, in some embodiments, the use of the above-mentioned acidic substance is conducive to the synthesis of a precursor substance with a cubic structure, forming a layered oxide positive electrode material with a cubic morphology, thereby promoting the reduction of the DC internal resistance of the sodium ion battery assembled with the layered oxide positive electrode material, the improvement of the cycle performance, the increase of the rate and the decrease of the expansion force.

[0057] In step (1), the complexing agent may be one or more selected from the group consisting of sodium citrate, sodium ascorbate, sodium pyrophosphate, sodium oxalate and ethylenediamine sodium oxalate.

[0058] In step (1), the surfactant is polyvinyl pyrrolidone and / or sodium dodecylbenzene sulfonate. In the present invention, the surfactant can make the metal ions react uniformly and avoid agglomeration. Therefore, in some embodiments, the use of the above-mentioned surfactant is conducive to the synthesis of a precursor material with a cubic structure, forming a layered oxide positive electrode material with a cubic morphology, thereby promoting the reduction of the DC internal resistance, the improvement of the cycle performance, the increase of the rate and the decrease of the expansion force of the sodium ion battery assembled with the layered oxide positive electrode material.

[0059] In step (1), the ratio of the amount of the substance of the cyano group in the substance containing the cyano group to the sum of the total amount of the metal in the metal salt can be 9: (1-3), for example, 9: 1, 9: 1.5, 9: 2, 9: 2.5, 9: 3. In the present invention, the ratio of the amount of the substance of the cyano group in the substance containing the cyano group to the sum of the total amount of the metal in the metal salt is controlled within the above range, which is beneficial to the reduction of the DC internal resistance, the improvement of the cycle performance, the increase of the rate and the decrease of the expansion force of the sodium ion battery assembled with the prepared layered oxide positive electrode material.

[0060] In step (1), the ratio of the amount of the complexing agent to the sum of the total amount of the metal elements in the metal salt can be 1: (1-10), such as 1: 2, 1: 4, 1: 6, 1: 8, 1: 10. In the present invention, the ratio of the amount of the complexing agent to the sum of the total amount of the metal elements in the metal salt is controlled within the above range, which is beneficial to the reduction of the DC internal resistance, the improvement of the cycle performance, the increase of the rate and the decrease of the expansion force of the sodium ion battery assembled with the prepared layered oxide positive electrode material.

[0061] In step (1), the ratio of the amount of the surfactant to the sum of the total amount of the metal elements in the metal salt can be 1: (1-10), for example, 1: 2, 1: 4, 1: 6, 1: 8, 1: 10. In the present invention, the sum of the amount of the surfactant and the total amount of the metal elements in the metal salt is controlled within the above range, which is beneficial to the reduction of the DC internal resistance, the improvement of the cycle performance, the increase of the rate and the decrease of the expansion force of the sodium ion battery assembled with the prepared layered oxide positive electrode material.

[0062] In step (1), the ratio of the amount of hydrogen ions in the acidic substance to the total amount of metal elements in the metal salt can be 1: (1-5), such as 1: 1, 1: 2, 1: 3, 1: 4, 1: 5. In the present invention, the sum of the amount of hydrogen ions in the acidic substance and the total amount of metal elements in the metal salt is controlled within the above range, which is beneficial to the reduction of the DC internal resistance, the improvement of the cycle performance, the increase of the rate and the decrease of the expansion force of the sodium ion battery assembled with the prepared layered oxide positive electrode material.

[0063] In step (1), the temperature of the coordination precipitation can be 10-70°C, for example, 10°C, 20°C, 30°C, 40°C, 50°C, 60°C, 70°C.

[0064] In step (1), the coordination precipitation time can be 4-8 hours, for example, 4 hours, 5 hours, 6 hours, 7 hours, 8 hours.

[0065] In step (1), a mixed solution comprising a metal salt, an acidic substance, a complexing agent and a surfactant is added to a solution comprising a substance containing a cyano group to perform a precipitation reaction to obtain a precursor substance; preferably, a peristaltic pump is used to dropwise add the mixed solution of the metal salt, the acidic substance, the complexing agent and the surfactant; more preferably, the dropping speed can be 0.5-1.5 mL·min -1 , for example 0.5 mL min -1 、0.7mL·min -1 、0.9mL·min -1 、1.1mL·min -1 、1.3mL·min -1 、1.5mL·min -1 .

[0066] In step (1), a mixed solution containing a metal salt and an acidic substance is added to a solution containing a cyano group-containing substance, a complexing agent and a surfactant to perform a precipitation reaction to obtain a precursor substance; preferably, a peristaltic pump is used to dropwise add the mixed solution of the metal salt and the acidic substance; more preferably, the dropping speed can be 0.5-1.5 mL·min -1 , for example 0.5 mL min -1 、0.7mL·min-1 、0.9mL·min -1 、1.1mL·min -1 、1.3mL·min -1 、1.5mL·min -1 .

[0067] The preparation method of the present invention further comprises: step (1) after coordination precipitation, aging, separation, washing and drying are performed to obtain a precursor substance.

[0068] In the present invention, the aging time can be 20-28 hours, for example 20 hours, 22 hours, 24 hours, 26 hours, 28 hours.

[0069] In the present invention, a centrifuge can be used to separate the aged product.

[0070] In the present invention, water and / or ethanol may be used to wash the separated product.

[0071] In the present invention, the drying may be vacuum drying.

[0072] In the present invention, the drying temperature may be 80-120°C, for example 80°C, 90°C, 100°C, 110°C, 120°C.

[0073] In step (2), the sodium source may be sodium carbonate and / or sodium hydroxide.

[0074] In step (2), the ratio of the amount of the sodium element in the sodium source to the total amount of the metal elements in the precursor material can be (0.6-1.2): 1, for example 0.6: 1, 0.7: 1, 0.8: 1, 0.9: 1, 1: 1, 1.1: 1, 1.2: 1. In the present invention, the ratio of the amount of the sodium element in the sodium source to the total amount of the metal elements in the precursor material is controlled within the above range, which is beneficial to the reduction of the DC internal resistance of the sodium ion battery assembled with the prepared layered oxide positive electrode material, the improvement of the cycle performance, the increase of the rate and the decrease of the expansion force.

[0075] In step (2), the sintering temperature may be 700-900° C., for example, 700° C., 750° C., 800° C., 850° C., 900° C. In the present invention, controlling the sintering temperature within the above range is beneficial to reducing the DC internal resistance, improving the cycle performance, increasing the rate, and reducing the expansion force of the sodium ion battery assembled with the prepared layered oxide positive electrode material.

[0076] In step (2), the sintering time can be 8-12 hours, for example 8 hours, 9 hours, 10 hours, 11 hours, 12 hours.

[0077] The invention provides a layered oxide positive electrode material prepared by the preparation method of the invention.

[0078] The invention provides a positive electrode slurry comprising a layered oxide positive electrode material prepared by the preparation method of the invention.

[0079] The present invention provides a positive electrode sheet comprising a current collector and an active material layer located on the surface of the current collector.

[0080] In the present invention, the positive electrode current collector may be aluminum foil, copper foil, titanium foil, nickel foil, iron foil, zinc foil, etc.

[0081] In the present invention, the active material layer is made of positive electrode slurry. The positive electrode slurry is coated on the current collector, and then dried and pressed to obtain a positive electrode sheet.

[0082] The sodium ion battery of the present invention comprises a positive electrode sheet, a negative electrode sheet, a separator and an electrolyte. The separator can be arranged between the positive and negative electrode sheets.

[0083] The negative electrode sheet includes a negative electrode current collector and a negative electrode active material layer disposed on the negative electrode current collector. The negative electrode current collector may be aluminum foil, copper foil, titanium foil, nickel foil, iron foil, zinc foil, etc. The negative electrode active material layer includes a negative electrode active material. The negative electrode active material may include a material capable of reversibly embedding / de-embedding sodium ions, a carbon-based material, a titanium-based material, an alloy material, a metal compound, etc. Examples of negative electrode active materials include hard carbon, soft carbon, Na2Ti3O7, Na 0.6 [Cr 0.6 Ti 0.4 ]O2、Li4Ti5O 12 , NaTi2(PO4)3, etc.

[0084] The negative electrode active material layer may also include one or two selected from a conductive agent and a binder. The conductive agent is used to improve the conductivity of the electrode. Examples of negative electrode conductive agents include conductive carbon black, conductive graphite, vapor deposited carbon fiber (VGCF), carbon nanotubes, graphene, etc. The negative electrode binder improves the bonding performance between the negative electrode active material particles and between the negative electrode active material particles and the current collector. Examples of negative electrode binders include polyvinylidene fluoride (PVDF), styrene-butadiene rubber (SBR), sodium carboxymethyl cellulose (CMC-Na), cyclodextrin, gelatin, polyvinyl alcohol, polyacrylate, acrylonitrile multipolymer, etc. The mass ratio of each component in the negative electrode material layer can be conventional.

[0085] The negative electrode active material layer is obtained by coating a negative electrode slurry containing various components of the negative electrode active material layer and a solvent onto a negative electrode current collector, followed by drying and pressing. The solvent of the negative electrode slurry may be water.

[0086] In some embodiments, the preparation method of the negative electrode sheet includes the following steps: dispersing the negative electrode active material, the binder and the conductive agent in water to obtain a uniform negative electrode slurry; evenly coating the negative electrode slurry on both surfaces of the negative electrode collector, such as copper foil, and after drying, compacting with a roller press to obtain a negative electrode sheet.

[0087] The separator can be a polymer porous separator, an inorganic porous separator or a polymer-inorganic composite porous separator. The polymer porous separator includes a single-layer polymer porous separator and a multi-layer polymer porous separator.

[0088] The electrolyte solution includes an organic solvent and an electrolyte salt.

[0089] Organic solvents suitable for the electrolyte of the present invention may include carbonate solvents, carboxylate solvents, ether solvents or other aprotic solvents. In some embodiments, the electrolyte includes carbonate solvents. In the electrolyte of the present invention, the mass of carbonate solvents can be 80%-100% of the total mass of the organic solvent, such as 85%, 90%, 95%. Examples of carbonate solvents include ethylene carbonate (EC), propylene carbonate (PC), dimethyl carbonate (DMC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), γ-butyrolactone, methyl acetate, ethyl acetate, propyl acetate, butyl acetate, ethyl propionate, propyl propionate, butyl propionate, etc. In some embodiments, the organic solvent is selected from at least two of ethylene carbonate, propylene carbonate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, γ-butyrolactone, methyl acetate, ethyl acetate, propyl acetate, butyl acetate, ethyl propionate, propyl propionate and butyl propionate. In some embodiments, the organic solvent comprises at least one cyclic carbonate and at least one linear carbonate. Examples of cyclic carbonates include ethylene carbonate, propylene carbonate, butylene carbonate, gamma-butyrolactone, etc. Examples of linear carbonates include dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, etc.

[0090] The electrolyte of the present invention may include an electrolyte salt. The electrolyte salt may include or be selected from a sodium salt. The sodium salt may be selected from one or more of an organic sodium salt and an inorganic sodium salt. In some embodiments, the electrolyte salt is selected from one or more of sodium perchlorate, sodium hexafluorophosphate, sodium hexafluoroaluminate, NaTFSI, NaFSI, NaBOB, NaODFB, NaPO2F2, etc. In some embodiments, the concentration of the electrolyte salt in the electrolyte is 0.5 to 2 mol / L, for example, 1 mol / L, 1.5 mol / L.

[0091] The electrolyte of the present invention may optionally contain various additives that can be used in the electrolyte, such as desolvating agents, cosolvents, film-forming additives, etc. The mass fraction of each type of additive in the electrolyte may be 0.1% to 10%, such as 1%, 2%, 3%, 4%, 5%.

[0092] The positive electrode sheet, the negative electrode sheet and the separator are stacked and / or wound, encapsulated in a shell, and dried, injected (electrolyte is injected), sealed, left to stand, formed, and divided to obtain a sodium ion battery. The form of the sodium ion battery of the present invention is not particularly limited, and can be a cylindrical sodium ion battery, a soft-pack sodium ion battery or an aluminum shell sodium ion battery.

[0093] Compared with the prior art, the present invention has the following beneficial effects: the layered oxide positive electrode material prepared by the present invention has pores inside and a cubic appearance outside, and its active surface is increased; this structure reduces the volume strain generated by the sodium ion battery during the process of charging and discharging sodium, fully ensures the contact between the material and the electrolyte, and ensures that Na + The rapid deintercalation can effectively reduce the impedance, thereby making the sodium ion battery containing the layered oxide positive electrode material of the present invention have low DC internal resistance, excellent cycle performance, high rate performance and low expansion force performance.

[0094] The present invention will be described below in the form of specific examples. It should be understood that these examples are merely illustrative and are not intended to limit the scope of the present invention. The methods, reagents and materials used in the examples are, unless otherwise stated, conventional methods, reagents and materials in the art. The raw material compounds in the examples can all be purchased through commercial routes.

[0095] Example 1

[0096] This embodiment prepares the layered oxide positive electrode material according to the following steps:

[0097] (1) NiCl2·6H2O and MnCl2·4H2O were dissolved in deionized water at a molar ratio of 1:1. Sodium citrate, polyvinyl pyrrolidone and hydrochloric acid were added at a ratio of 8:1:1:2 to the total molar amount of metal elements in M ​​salt (M salt is NiCl2·6H2O and MnCl2·4H2O), the molar amount of sodium citrate, the molar amount of polyvinyl pyrrolidone and the molar amount of hydrogen ions in hydrochloric acid. The mixture was stirred to obtain a mixed solution. The concentration of metal elements in M ​​salt in the mixed solution was 1 mol / L. The mixed solution was added to Na4Fe(CN)6·10H2O solution through a peristaltic pump at a ratio of 1:9 to the total molar amount of metal elements in M ​​salt and the molar amount of cyano groups in Na4Fe(CN)6·10H2O solution. The concentration of Na4Fe(CN)6·10H2O in the Na4Fe(CN)6·10H2O solution was 1 mol / L. The dripping rate was controlled to 1 mL·min -1, stirring was continued at 60°C for 6 hours, and then aged for 24 hours to obtain a precipitate, which was separated by a high-speed centrifuge, repeatedly washed with deionized water and anhydrous ethanol, and finally placed at 100°C for 48 hours in a vacuum dryer to obtain a precursor material NiMn[Fe(CN)6]3. The morphology of the precursor material prepared in this embodiment is as follows Figure 1 As shown;

[0098] (2) Sodium carbonate and the precursor material obtained in step (1) were mixed in a ratio of 0.8:1 between the molar amount of sodium element in sodium carbonate and the total molar amount of metal elements in the precursor material, and sintered in an O2 atmosphere at 700°C for 10 h to obtain a layered oxide positive electrode material Na 0.8 Ni 0.2 Mn 0.2 Fe 0.6 O2, the morphology of the layered oxide positive electrode material prepared in this embodiment is as follows Figure 2 shown.

[0099] Example 2

[0100] The other conditions are the same as those in Example 1, except that in this example, the NiCl2·6H2O and MnCl2·4H2O in a molar ratio of 1:1 in step (1) are replaced by NiCl2·6H2O, MnCl2·4H2O and CuCl2·2H2O in a molar ratio of 3:4:1, and the M salt is NiCl2·6H2O, MnCl2·4H2O and CuCl2·2H2O.

[0101] Example 3

[0102] The other conditions are the same as those in Example 1, except that in this example, the NiCl2·6H2O and MnCl2·4H2O in a molar ratio of 1:1 in step (1) are replaced by MnCl2·4H2O, NiCl2·6H2O and ZnCl2 in a molar ratio of 4:3:1. In this case, the M salt is MnCl2·4H2O, NiCl2·6H2O and ZnCl2.

[0103] Example 4

[0104] This embodiment prepares the layered oxide positive electrode material according to the following steps:

[0105] (1) K3Co(CN)6, sodium dodecylbenzene sulfonate and sodium ascorbate were dissolved in deionized water at a molar ratio of 2:1:1, and stirred to form an A1 solution, in which the concentration of sodium ascorbate was 1 mol / L; Ni(CH3COO)2, Mn(CH3COO)2 and hydrogen ions in acetic acid were added to deionized water at a molar ratio of 4:4:2, and stirred to form an A2 solution, in which the concentration of Ni(CH3COO)2 was 1 mol / L; A2 solution was added to A1 solution by a peristaltic pump in a ratio of 1:9 of the total molar amount of metal elements in M ​​salt (M salt is Ni(CH3COO)2 and Mn(CH3COO)2) and the molar amount of cyano groups in K3Co(CN)6 solution, and the dripping rate was controlled to 1 mL min -1 , stirring continuously for 6 h at 60 °C, then aging for 24 h to obtain a precipitate, separating the precipitate by high-speed centrifuge, repeatedly washing with deionized water and anhydrous ethanol, and finally drying under vacuum at 100 °C for 48 h to obtain the precursor material NiMn[Co(CN)6]3;

[0106] (2) Sodium carbonate and the precursor material obtained in step (1) were mixed in a ratio of 0.8:1 of the molar amount of sodium element in sodium carbonate to the total molar amount of metal elements in the precursor material, and sintered in an O2 atmosphere at 700°C for 10 h to obtain a layered oxide positive electrode material Na 0.8 Ni 0.2 Mn 0.2 Co 0.6 O2.

[0107] Example 5

[0108] The other conditions are the same as those in Example 3, except that the sintering temperature in step (2) is replaced from 700° C. to 800° C. in this example.

[0109] Example 6

[0110] The other conditions are the same as those in Example 3, except that the sintering temperature in step (2) is replaced from 700° C. to 900° C. in this example.

[0111] Comparative Example 1

[0112] This comparative example prepares the layered oxide positive electrode material according to the following steps:

[0113] (1) dissolving NaCH3COO·3H2O, Ni(CH3COO)2, Mn(CH3COO)2, Fe(CH3COO)2 and citric acid in deionized water at a molar ratio of 8:2:2:6:10 to obtain a mixed solution, and drying the mixed solution at 70° C. to obtain a precursor material;

[0114] (2) The precursor material obtained in step (1) is subjected to a first sintering in an air atmosphere at 400° C. for 2 h, and then subjected to a second sintering in an air atmosphere at 700° C. for 10 h, to obtain a layered oxide positive electrode material.

[0115] Comparative Example 2

[0116] The other conditions are the same as those in Comparative Example 1, except that in this comparative example, the molar ratio of NaCH3COO·3H2O, Ni(CH3COO)2, Mn(CH3COO)2, Fe(CH3COO)2 and citric acid in step (1) is replaced by the molar ratio of NaCH3COO·3H2O, Ni(CH3COO)2, Mn(CH3COO)2, Cu(CH3COO)2, Fe(CH3COO)2 and citric acid in step (1) is replaced by the molar ratio of NaCH3COO·3H2O, Ni(CH3COO)2, Mn(CH3COO)2, Cu(CH3COO)2, Fe(CH3COO)2 and citric acid in step (1). The morphology of the layered oxide positive electrode material obtained in this comparative example is as follows: Figure 3 shown.

[0117] Comparative Example 3

[0118] The other conditions are the same as those in Comparative Example 1, except that in this Comparative Example, the molar ratio of NaCH3COO·3H2O, Ni(CH3COO)2, Mn(CH3COO)2, Fe(CH3COO)2 and citric acid in step (1) is replaced by a molar ratio of NaCH3COO·3H2O, Ni(CH3COO)2, Mn(CH3COO)2, Zn(CH3COO)2, Fe(CH3COO)2 and citric acid in 8:1.5:2:0.5:6:10.

[0119] Comparative Example 4

[0120] The other conditions are the same as those of Comparative Example 3, except that the sintering temperature of the second sintering in step (2) is replaced from 700° C. to 800° C.

[0121] Comparative Example 5

[0122] The other conditions are the same as those of Comparative Example 1, except that the sintering temperature of the second sintering in step (2) is replaced from 700° C. to 900° C.

[0123] Comparative Example 6

[0124] The other conditions are the same as those in Example 1, except that polyvinyl pyrrolidone is not added in step (1) of this comparative example. The morphology of the precursor material prepared in this comparative example is as follows: Figure 4 As shown, the morphology of the layered oxide cathode material is Figure 5 shown.

[0125] Comparative Example 7

[0126] The other conditions are the same as those in Example 1, except that hydrochloric acid is not added in step (1) of this comparative example. The morphology of the precursor material prepared in this comparative example is as follows: Figure 6 As shown, the morphology of the layered oxide cathode material is Figure 7 shown.

[0127] Test Case

[0128] (1) Preparing a positive electrode sheet: The layered oxide positive electrode materials, conductive carbon black, conductive carbon tubes, polyvinylidene fluoride and nitrogen methyl pyrrolidone prepared in Examples 1-6 and Comparative Examples 1-7 were mixed in a mass ratio of 97.5:1:0.5:1:40 to prepare a mixture, and the mixture was stirred at 500 rpm for 4 h to obtain a positive electrode slurry; the positive electrode slurry was evenly coated on an aluminum foil using a scraper, and the mixture was placed in a forced air drying oven and dried at 120° C. for 20 min. Finally, the dried electrode sheet was rolled and cut to obtain a positive electrode sheet.

[0129] (2) Preparing a negative electrode sheet: A negative electrode hard carbon material, conductive carbon black (Super P), sodium carboxymethyl cellulose (CMC-Na) and styrene-butadiene rubber (SBR) are mixed in a mass ratio of 85:10:4:1 to prepare a mixture, which is dissolved in deionized water and stirred evenly to obtain a negative electrode slurry. The negative electrode slurry is coated on an aluminum foil, and the mixture is dried and cut into sheets to obtain a negative electrode sheet.

[0130] (3) Preparation of electrolyte: Sodium hexafluorophosphate was dissolved in a mixed solvent of ethylene carbonate (EC) and dimethyl carbonate (DEC) in a volume ratio of 1:1, and then fluoroethylene carbonate (FEC) was added in an amount of 5% by mass of the mixed solvent to obtain an electrolyte, wherein the concentration of sodium hexafluorophosphate in the electrolyte was 1 mol / L.

[0131] (4) Assembling sodium ion soft-pack cells: The negative electrode sheets and the positive electrode sheets are matched according to an NP ratio of 1.2, and a polyacrylonitrile / graphene oxide (PG) separator is added in between. After winding, baking, injecting electrolyte, packaging, forming, and capacity division, a 1.5Ah soft-pack cell is assembled.

[0132] (5) DC internal resistance test: Charge to 3.95 V at 0.5 C, discharge to 50% of the initial capacity at 0.5 C, and then discharge at a rate of 4 C for 10 s. The DC internal resistance of the sodium ion soft-pack cells of the layered oxide positive electrode materials prepared in Examples 1-6 and Comparative Examples 1-7 was calculated by the ratio of the voltage drop value to the current.

[0133] (6) Rate performance test: In a constant temperature box, the sodium ion soft-pack cells containing the layered oxide positive electrode materials prepared in Examples 1-6 and Comparative Examples 1-7 were charged and discharged at the same rate, that is, the charge and discharge tests were carried out at rates of 0.33C, 1C, 5C and 10C, respectively. Specifically, the cells were charged to 3.95V at 0.33C and discharged to 1.5V at 0.33C; charged to 3.95V at 1C and discharged to 1.5V at 1C; charged to 3.95V at 5C and discharged to 1.5V at 5C; charged to 3.95V at 10C and discharged to 1.5V at 10C.

[0134] (7) Cyclic performance test: In a constant temperature chamber, the sodium ion soft-pack cells containing the layered oxide positive electrode materials prepared in Examples 1-6 and Comparative Examples 1-7 were subjected to a cyclic charge and discharge test at a rate of 1C, i.e., the steps of charging at 1C to 3.95V and discharging at 1C to 1.5V were cycled 500 times.

[0135] (8) Expansion force performance test: The sodium ion soft-pack battery cells containing the layered oxide positive electrode materials prepared in Examples 1-6 and Comparative Examples 1-7 were placed in a customized expansion force test fixture, connected to a pressure monitoring device, fixed the initial pressure at 1000N, and recorded the pressure changes during the cycle.

[0136] Table 1: DC internal resistance, rate performance, cycle performance and expansion force performance of sodium ion batteries containing layered oxide positive electrode materials of Examples 1-6 and Comparative Examples 1-7

[0137]

[0138] As shown in Table 1, compared with the layered oxide positive electrode material prepared by the common sol-gel method in Comparative Example 1, the layered oxide positive electrode material prepared by the preparation method of the present invention in Example 1 or Example 4 has lower DC internal resistance, higher rate performance, lower expansion force and better cycle performance. The comparison between Example 2 and Comparative Example 2 and the comparison between Example 3 and Comparative Example 3 further verified this conclusion.

[0139] Figure 1 This is an electron microscope image of the precursor material prepared in Example 1 of the present invention. Figure 1 It can be seen that the precursor material prepared by adding polyvinyl pyrrolidone has a cubic morphology. Figure 4 This is an electron microscope image of the precursor material prepared in Comparative Example 6 of the present invention. Figure 4It can be seen that the precursor material prepared without adding polyvinyl pyrrolidone has no cubic morphology. Therefore, it can be concluded that the addition of surfactant is conducive to the formation of a cubic morphology of the precursor material. On the basis that the precursor material has a cubic morphology, the layered oxide positive electrode material formed by sintering also has a cubic morphology, so the addition of surfactant is conducive to the formation of a cubic morphology of the layered oxide positive electrode material.

[0140] Further, Figure 2 This is an electron microscope image of the layered oxide positive electrode material prepared in Example 1 of the present invention. Figure 2 It can be seen that the layered oxide cathode material prepared by adding polyvinyl pyrrolidone has a cubic morphology. Figure 5 This is an electron microscope image of the layered oxide positive electrode material prepared in Comparative Example 6 of the present invention. The layered oxide positive electrode material prepared without adding polyvinyl pyrrolidone has no cubic morphology. Therefore, it can be verified that adding a surfactant is conducive to the formation of a cubic morphology of the layered oxide positive electrode material.

[0141] Furthermore, it can be seen from Table 1 that the layered oxide positive electrode material prepared by adding polyvinyl pyrrolidone in Example 1 has lower DC internal resistance, higher rate performance, lower expansion force and better cycle performance, compared with the layered oxide positive electrode material prepared without adding polyvinyl pyrrolidone in Comparative Example 6. This shows that the layered oxide positive electrode material with a cubic morphology can promote the reduction of DC internal resistance, improvement of cycle performance, increase of rate and decrease of expansion force of the sodium ion battery assembled with the layered oxide positive electrode material.

[0142] Figure 1 This is an electron microscope image of the precursor material prepared in Example 1 of the present invention. Figure 1 It can be seen that the precursor material prepared by adding hydrochloric acid has a cubic morphology. Figure 6 This is an electron microscope image of the precursor material prepared in Comparative Example 7 of the present invention. Figure 6 It can be seen that the precursor material prepared without adding hydrochloric acid has no cubic morphology. Therefore, it can be concluded that adding an acidic substance is conducive to the formation of a cubic morphology of the precursor material. On the basis that the precursor material has a cubic morphology, the layered oxide positive electrode material formed by sintering also has a cubic morphology, so adding an acidic substance is conducive to the formation of a cubic morphology of the layered oxide positive electrode material.

[0143] Further, Figure 2 This is an electron microscope image of the layered oxide positive electrode material prepared in Example 1 of the present invention. Figure 2 It can be seen that the layered oxide cathode material prepared by adding hydrochloric acid has a cubic morphology. Figure 7This is an electron microscope image of the layered oxide positive electrode material prepared in Comparative Example 7 of the present invention. The layered oxide positive electrode material prepared without adding hydrochloric acid has no cubic morphology. Therefore, it can be verified that adding an acidic substance is conducive to the formation of a cubic morphology of the layered oxide positive electrode material.

[0144] Furthermore, it can be seen from Table 1 that the layered oxide positive electrode material prepared by adding hydrochloric acid in Example 1 has lower DC internal resistance, higher rate performance, lower expansion force and better cycle performance, compared with the layered oxide positive electrode material prepared without adding hydrochloric acid in Comparative Example 7. This shows that the layered oxide positive electrode material with a cubic morphology can further promote the reduction of DC internal resistance, improvement of cycle performance, increase of rate and decrease of expansion force of the sodium ion battery assembled with the layered oxide positive electrode material.

Claims

1. A method for preparing a layered oxide positive electrode material, characterized in that: The preparation method comprises the following steps: (1) Coordinating and precipitating a metal salt and a substance containing a cyano group in the presence of an acidic substance, a complexing agent and a surfactant to obtain a precursor substance; (2) sintering the precursor material with a sodium source to obtain a layered oxide positive electrode material; The metal element in the metal salt is selected from one or more of Ni, Fe, Mn, Cu, Zn, Ti and Co.

2. The preparation method according to claim 1, characterized in that The preparation method has one or more of the following characteristics: The metal elements in the metal salt include Ni and Mn, and optionally include one or more of Fe, Cu, Zn, Ti and Co; In step (1), the metal salt is selected from one or more of sulfate, chloride, acetate and oxalate; In step (1), the cyano group-containing substance is selected from one or more of sodium ferrocyanide, potassium ferrocyanide and potassium cobalt cyanide; In step (1), the acidic substance is selected from one or more of hydrochloric acid, sulfuric acid, acetic acid, oxalic acid and acetic acid; In step (1), the complexing agent is selected from one or more of sodium citrate, sodium ascorbate, sodium pyrophosphate, sodium oxalate and ethylenediamine sodium oxalate; In step (1), the surfactant is polyvinyl pyrrolidone and / or sodium dodecylbenzene sulfonate.

3. The preparation method according to claim 1, characterized in that: The preparation method has one or more of the following characteristics: In step (1), the ratio of the amount of the cyano group in the cyano group-containing substance to the total amount of the metal element in the metal salt is 9:(1-3); In step (1), the amount of the complexing agent is 244792 of the total amount of the metal element in the metal salt. The ratio of the sum of the quantities is 1:(1-10); In step (1), the ratio of the amount of the surfactant to the total amount of the metal element in the metal salt is 1:(1-10); In step (1), the ratio of the amount of hydrogen ions in the acidic substance to the total amount of metal elements in the metal salt is 1:(1-5); In step (1), the temperature of the coordination precipitation is 10-70°C; In step (1), the coordination precipitation time is 4-8 hours.

4. The preparation method according to claim 1, characterized in that: In step (1), a mixed solution comprising a metal salt, an acidic substance, a complexing agent and a surfactant is added to a solution comprising a substance containing a cyano group to perform a precipitation reaction to obtain a precursor substance; preferably, a peristaltic pump is used to dropwise add the mixed solution of the metal salt, the acidic substance, the complexing agent and the surfactant; more preferably, the dropping speed is 0.5-1.5 mL·min -1 ; or In step (1), a mixed solution containing a metal salt and an acidic substance is added to a solution containing a cyano group-containing substance, a complexing agent and a surfactant to perform a precipitation reaction to obtain a precursor substance; preferably, a peristaltic pump is used to dropwise add the mixed solution of the metal salt and the acidic substance; more preferably, the dropping speed is 0.5-1.5 mL·min -1 .

5. The preparation method according to claim 1, characterized in that: The method further comprises: after step (1) coordination precipitation, aging, separation, washing and drying to obtain a precursor material; preferably, the aging time is 20-28 hours; separation is performed by a centrifuge; washing is performed by water and / or ethanol; drying is performed by vacuum drying; and the drying temperature is 80-120°C.

6. The preparation method according to claim 1, characterized in that: The preparation method has one or more of the following characteristics: In step (2), the sodium source is sodium carbonate and / or sodium hydroxide; In step (2), the ratio of the amount of the sodium element in the sodium source to the total amount of the metal elements in the precursor material is (0.6-1.2):1; In step (2), the sintering temperature is 700-900° C.; In step (2), the sintering time is 8-12 hours.

7. A layered oxide prepared by the preparation method according to any one of claims 1 to 6 Extreme material.

8. A positive electrode slurry, characterized in that: The positive electrode slurry comprises a layered oxide positive electrode material prepared by the preparation method according to any one of claims 1 to 6 or a layered oxide positive electrode material according to claim 7.

9. A positive electrode sheet, characterized in that: The positive electrode sheet comprises a current collector and an active material layer located on a surface of the current collector, wherein the active material layer is made of the positive electrode slurry according to claim 8.

10. A sodium ion battery, characterized in that: The sodium ion battery comprises the positive electrode sheet according to claim 9.