Sulfide solid electrolyte and preparation method and application thereof
By premixing in a protective atmosphere and performing high-pressure solid phase reaction to prepare an oxygen-containing solid electrolyte, the problem of unstable traditional sulfur-silver germanium ore type electrolyte in the air is solved, and its stability and battery performance are improved.
Patent Information
- Application Number
- CN202411255052.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-09
- Publication Date
- 2024-12-03
AI Technical Summary
The traditional sulfur-silver germanium ore solid electrolyte is unstable in the air, and produces the toxic gas H2S when exposed, and the ionic conductivity is attenuated. The ionic conductivity of the oxygen-containing sulfur-silver germanium ore solid electrolyte is significantly attenuated when prepared by ball milling + sintering process.
The chemical formula of the solid electrolyte containing oxygen sulfide is Li6PSaObX, where X is selected from F, Cl, Br, I. The lithium source, P source, S source and halogen source are premixed in a protective atmosphere and high-pressure solidification is performed. Phase reaction preparation, combined with high-pressure torsion treatment, a sulfide solid electrolyte with non-thermodynamic stability was prepared.
It improves the air and water stability of the sulfide solid electrolyte, increases its contact with the positive and negative electrode interface, reduces the internal resistance of the battery, and improves the battery performance.
Smart Images

Figure CN119069780A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of solid electrolytes, and in particular relates to a sulfide solid electrolyte and a preparation method and application thereof. Background Art
[0002] Traditional argyrodite-type solid electrolytes have high ionic conductivity, but they are difficult to exist stably in an air atmosphere and will produce toxic gas H when exposed to air. 2 S, and the ionic conductivity decays at the same time; the argyrodite-type solid electrolyte containing O can improve the air stability, but the ionic conductivity of the argyrodite-type solid electrolyte prepared by ball milling + sintering process is significantly attenuated compared with that without O doping. Summary of the invention
[0003] The main purpose of the present invention is to provide a sulfide solid electrolyte and a preparation method and application thereof, so as to overcome the deficiencies of the prior art.
[0004] In order to achieve the above-mentioned invention object, the technical solution adopted by the present invention includes: The embodiment of the present invention provides a sulfide solid electrolyte, wherein the sulfide solid electrolyte is an oxygen-containing solid electrolyte, and the chemical formula of the sulfide solid electrolyte is Li 6 PS a O b X, wherein X is selected from any one of F, Cl, Br, and I, and satisfies a+b=5, a / b≥4, and b>0.
[0005] The present invention also provides a method for preparing the aforementioned sulfide solid electrolyte, which comprises: In a protective atmosphere, a lithium source, a P source, a S source, an O source and a halogen source are premixed, and then a high-pressure solid-phase reaction is carried out to obtain a sulfide solid electrolyte.
[0006] The embodiment of the present invention also provides the use of the aforementioned sulfide solid electrolyte in preparing a lithium battery positive electrode or a lithium ion battery.
[0007] An embodiment of the present invention further provides a lithium battery positive electrode, which includes a positive electrode active material and a solid electrolyte; wherein the solid electrolyte includes the aforementioned sulfide solid electrolyte.
[0008] An embodiment of the present invention further provides a lithium-ion battery, which includes a positive electrode, a negative electrode and an intermediate layer; wherein the intermediate layer includes the aforementioned sulfide solid electrolyte, and the positive electrode includes the aforementioned lithium battery positive electrode.
[0009] Compared with the prior art, the present invention has the following beneficial effects: (1) The sulfide solid electrolyte provided by the present invention uses O element to replace S element, which increases the polarity and 5+ , Li + Stronger binding ability stabilizes the sulfide solid electrolyte and prevents decomposition, thereby improving its air and water stability; (2) Traditional oxygen substitution will increase the elastic modulus of the sulfide solid electrolyte and reduce the electronic conductivity. The former is not conducive to the contact between the sulfide solid electrolyte and the positive and negative electrode interfaces, and the latter will increase the internal resistance of the battery. The traditional ball milling and sintering process allows the sulfide particles to grow to a thermally stable state. The high-pressure torsion treatment adopted in this application achieves a sample in a non-thermodynamically stable state through high shear and large plastic deformation, which improves the problem of battery performance degradation caused by the increase in elastic modulus and the decrease in electronic conductivity. BRIEF DESCRIPTION OF THE DRAWINGS
[0010] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0011] Figure 1 is a SEM image of the LiPSCl solid electrolyte sample prepared in Example 4 of the present invention; Figure 2 It is the XRD spectrum of the LiPSCl solid electrolyte sample prepared in Example 4 of the present invention. DETAILED DESCRIPTION
[0012] In view of the defects of the prior art, the inventor of this case has proposed the technical solution of the present invention after long-term research and extensive practice. The technical solution of the present invention will be described clearly and completely below. Obviously, the described embodiments are part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0013] Specifically, as one aspect of the technical solution of the present invention, a sulfide solid electrolyte involved is an oxygen-containing solid electrolyte, and the chemical formula of the sulfide solid electrolyte is Li 6 PS a O b X (denoted as: LiPSOX), wherein X is selected from any one of F, Cl, Br, and I, and satisfies a+b=5, a / b≥4, and b>0.
[0014] In some preferred embodiments, the sulfide solid electrolyte has a spherical or quasi-spherical structure.
[0015] In some preferred embodiments, the average particle size D of the sulfide solid electrolyte is 50 <1 μm.
[0016] In some preferred embodiments, the room temperature ionic conductivity of the sulfide solid electrolyte is 1.0E-4~1.0E-2 S / cm.
[0017] Another aspect of the embodiments of the present invention further provides a method for preparing the aforementioned sulfide solid electrolyte, which comprises: In a protective atmosphere, a lithium source, a P source, a S source, an O source and a halogen source are premixed, and then a high-pressure solid-phase reaction is carried out to obtain a sulfide solid electrolyte.
[0018] In some preferred embodiments, the preparation method specifically includes: in a protective atmosphere, using a three-dimensional mixing device to premix a lithium source, a P source, a S source, an O source and a halogen source to obtain a premix; wherein the three-dimensional mixing device uses a rotation speed of 500~5000rpm and a time of 5~10h.
[0019] In some preferred embodiments, the preparation method specifically includes: in a protective atmosphere, placing the premixed material in a high-pressure torsion device for high-pressure torsion treatment, thereby obtaining the sulfide solid electrolyte; wherein the pressure used in the high-pressure torsion treatment is 50~200MPa, the rotation frequency is 10~100Hz, and the time is 1~3h.
[0020] In some preferred embodiments, the lithium source includes Li 2 O, LiX, Li 2 S, LiOH, Li 2 CO 3 Any one or more combinations of the foregoing, and not limited to these.
[0021] In some preferred embodiments, the P source includes P 2 O 5 and / or P 2 S 5 , but not limited to this.
[0022] In some preferred embodiments, the S source includes Li 2 S and / or P 2 S 5 , but not limited to this.
[0023] In some preferred embodiments, the O source includes Li 2 O, LiOH, Li 2 CO3 , P 2 O 5 Any one or more combinations of the foregoing, and not limited to these.
[0024] In some preferred embodiments, the halogen source includes LiX, but is not limited thereto.
[0025] In some preferred embodiments, the molar ratio of the S source to the O source is 4-19:1.
[0026] Another aspect of the embodiments of the present invention further provides the use of the aforementioned sulfide solid electrolyte in preparing a lithium battery positive electrode or a lithium ion battery.
[0027] Another aspect of an embodiment of the present invention further provides a lithium battery positive electrode, which includes a positive electrode active material and a solid electrolyte; wherein the solid electrolyte includes the aforementioned sulfide solid electrolyte.
[0028] Another aspect of an embodiment of the present invention further provides a lithium-ion battery, which includes a positive electrode, a negative electrode and an intermediate layer; wherein the intermediate layer includes the aforementioned sulfide solid electrolyte, and the positive electrode includes the aforementioned lithium battery positive electrode.
[0029] Further, the negative electrode includes a lithium metal negative electrode, but is not limited thereto.
[0030] The technical solution of the present invention is further described in detail below in conjunction with several preferred embodiments. This embodiment is implemented on the premise of the technical solution of the invention, and provides a detailed implementation method and a specific operation process, but the protection scope of the present invention is not limited to the following embodiments.
[0031] The experimental materials used in the following examples can be purchased from conventional biochemical reagent companies unless otherwise specified. Unless otherwise specified, "room temperature" used in this application refers to the temperature measured by a Celsius thermometer in an ordinary laboratory, generally 20-30°C, preferably 25°C (Kelvin temperature is 298.15K) ± 2°C.
[0032] Example 1 1) Use a three-dimensional mixer to premix, and then use high-pressure solid phase reaction to prepare Li 6 PS 0.25 O 4.75 The specific preparation steps of the solid electrolyte powder of Cl include: adding LiCl into a three-dimensional mixer according to a molar ratio of 5:0.9:0.1:2 under an inert protective atmosphere. 2 O.P 2 O 5 , P 2 S 5, LiCl, the rotation speed is set to 1000rpm, the time is 8h. Then, the mixture is subjected to high-pressure torsion using a high-pressure torsion device under a protective atmosphere, the pressure is set to 100MPa, the rotation frequency is 50Hz, the time is 2h, and LPSOCl material is obtained, which is then ground in a mortar to obtain LPSOCl powder.
[0033] 2) The solid electrolyte powder was placed under different humidity conditions for different periods of time to test the ionic conductivity; the solid electrolyte material after the above-mentioned placement was used to assemble a Li||Li symmetrical battery. 2 The cycle test was carried out under the conditions. The above different humidity conditions include relative humidity of 40%; the above different standing times include 0h, 1h, 2h, 5h; the results are shown in Table 1.
[0034] 3) The above electrolyte materials were subjected to electronic conductivity test and elastic modulus test; the results are shown in Table 2.
[0035] 4) In a -40°C dew point dry room, the solid electrolyte was mixed with lithium iron phosphate active material, conductive agent and binder in a mass ratio of 2:5:2:1, and prepared into a positive electrode by dry rolling; the solid electrolyte was prepared into an electrolyte layer by dry rolling; lithium metal was used as the negative electrode, and assembled into a solid-state battery with the positive electrode and the solid electrolyte layer, and the number of room temperature cycles at 90% capacity retention was recorded under a pressure of 5 MPa; the results are shown in Table 2. Example 2
[0036] The difference between this embodiment and embodiment 1 is that the preparation chemical formula is Li 6 PS 0.5 O 4.5 The solid electrolyte powder of Cl was added into the ball mill according to the molar ratio of 12.5:2:0.5:5. 2 O.P 2 O 5 , P 2 S 5 , LiCl.
[0037] The remaining preparation methods and parameters were consistent with those in Example 1. The characterization results are shown in Tables 1 and 2. Example 3
[0038] The difference between this embodiment and embodiment 1 is that the preparation chemical formula is Li 6 PS 1 O 4 The solid electrolyte powder of Cl was added into the ball mill according to the molar ratio of 12.5:1.5:1:5. 2 O.P 2 O 5 , P 2 S5 , LiCl.
[0039] The remaining preparation methods and parameters were consistent with those in Example 1. The characterization results are shown in Tables 1 and 2. Example 4
[0040] The difference between this embodiment and embodiment 1 is that the preparation chemical formula is Li 6 PS 2.5 O 2.5 The solid electrolyte powder of Cl was added into the ball mill at a molar ratio of 2.5:0.5:1. 2 O.P 2 S 5 、LiCl. Prepared Li 6 PS 2.5 O 2.5 The SEM image of the solid electrolyte powder of Cl is shown in Figure 1 As shown in Figure 2, it can be seen that the sample particles are spherical and nanoscale; the XRD spectrum is shown in Figure 2 Figure 2 As shown, the results show that the main phase is argyrodite, with no obvious impurity phase.
[0041] The remaining preparation methods and parameters were consistent with those in Example 1. The characterization results are shown in Tables 1 and 2. Example 5
[0042] The difference between this embodiment and embodiment 1 is that the preparation chemical formula is Li 6 PS 4 O 1 The solid electrolyte powder of Cl was added into the ball mill according to the molar ratio of 1.5:1:0.5:1. 2 S. Li 2 O.P 2 S 5 , LiCl.
[0043] The remaining preparation methods and parameters were consistent with those in Example 1. The characterization results are shown in Tables 1 and 2. Example 6
[0044] The difference between this embodiment and embodiment 1 is that the preparation chemical formula is Li 6 PS 4.5 O 0.5 The solid electrolyte powder of Cl was added into the ball mill according to the molar ratio of 2:0.5:0.5:1. 2 S. Li 2 O.P 2 S 5 、LiCl The remaining preparation methods and parameters were consistent with those in Example 1. The characterization results are shown in Tables 1 and 2. Example 7
[0045] The difference between this embodiment and embodiment 1 is that the preparation chemical formula is Li 6 PS 4.75 O 0.25 The solid electrolyte powder of Cl was added into the ball mill according to the molar ratio of 2.25:0.25:0.5:1. 2 S. Li 2 O.P 2 S 5 、LiCl The remaining preparation methods and parameters were consistent with those in Example 1. The characterization results are shown in Tables 1 and 2. Example 8
[0046] The difference between this embodiment and embodiment 4 is that LiOH and P are added into the ball mill according to the molar ratio of 5:0.5:1. 2 S 5 、LiCl The remaining preparation methods and parameters were consistent with those in Example 4. The characterization results are shown in Tables 1 and 2. Example 9
[0047] The difference between this embodiment and embodiment 4 is that Li is added into the ball mill according to the molar ratio of 2.5:0.5:1. 2 CO 3 , P 2 S 5 、LiCl The remaining preparation methods and parameters were consistent with those in Example 4. The characterization results are shown in Tables 1 and 2.
[0048] Comparative Example 1 The method is the same as in Example 4, except that Li 2 S replaces Li 2 O, the chemical formula of the prepared product is Li 6 PS 5 Cl solid electrolyte powder.
[0049] The remaining preparation methods and parameters were consistent with those in Example 4. The characterization results are shown in Tables 1 and 2.
[0050] Comparative Example 2 The method is the same as in Example 4, except that: P is added to the ball mill. 2 O 5 Replace P 2 S 5 The product formula is Li 6 PO 5 Cl solid electrolyte powder.
[0051] The remaining preparation methods and parameters were consistent with those in Example 4. The characterization results are shown in Tables 1 and 2.
[0052] Comparative Example 3 The method is the same as that of Example 4, except that Li is added to the ball mill in a molar ratio of 2.5:0.5:2.5:1. 2 O.P 2 O 5 , CS 2 , LiCl, the chemical formula of the prepared product is Li 6 PS 5 Cl solid electrolyte powder.
[0053] The remaining preparation methods and parameters were consistent with those in Example 4. The characterization results are shown in Tables 1 and 2.
[0054] Comparative Example 4 The method is the same as in Example 4, except that Li is added to the ball mill at a molar ratio of 2.5:0.5:1. 2 S.P. 2 S 3 , LiCl, the chemical formula of the prepared product is Li 6 PS 4 Cl solid electrolyte powder.
[0055] The remaining preparation methods and parameters were consistent with those in Example 4. The characterization results are shown in Tables 1 and 2.
[0056] Comparative Example 5 The method is the same as that of Example 4, except that Li is added to the ball mill at a molar ratio of 2.5:0.5:0.5:1. 2 S. Li 2 O.P 2 S 3 , LiCl, the chemical formula of the prepared product is Li 6 PS 3.5 O 0.5 Cl solid electrolyte powder.
[0057] The remaining preparation methods and parameters were consistent with those in Example 4. The characterization results are shown in Tables 1 and 2.
[0058] Comparative Example 6 The method is the same as in Example 3, except that high pressure torsion is not used, and ordinary solid phase reaction is used instead. Specifically, Li is added into the ball mill in a molar ratio of 2.5:0.5:1. 2 O.P 2 S 5, LiCl, add 3 mm zirconium balls to the ball mill according to the ball-to-material mass ratio of 10:1, and seal the ball mill. Use a high-speed planetary ball mill to ball mill the above precursor powders, set the speed to 2000rpm, and the time is 8 hours. Then keep it at 300℃ for 10 hours, the heating rate is 3℃ / min, and cool it with the furnace when cooling.
[0059] Comparative Example 7 The method is the same as that of Example 3, except that the pressure used in the high-pressure torsion treatment is 10 MPa.
[0060] Comparative Example 8 The method is the same as that of Example 3, except that the pressure used in the high-pressure torsion treatment is 250 MPa.
[0061] Comparative Example 9 The method is the same as that of Example 3, except that the rotation frequency used in the high-pressure torsion treatment is 2 Hz.
[0062] Comparative Example 10 The method is the same as that of Example 3, except that the rotation frequency used in the high-pressure torsion treatment is 150 Hz.
[0063] Table 1 Ionic conductivity of Examples 1-9 and Comparative Examples 1-10 after standing in an air atmosphere with a relative humidity of 40%
[0064] Table 1 shows the ionic conductivity data of the electrolytes in different embodiments and comparative examples after being stored for different time periods in an air atmosphere with a relative humidity of 40%. Embodiments 1-5 show that as the O content increases, the initial ionic conductivity of the solid electrolyte decreases, but the air stability improves; the ionic conductivity of Embodiments 1-5 at 0h is similar to or slightly lower than that of Comparative Example 1, but after 1h, 2h, and 5h, the ionic conductivity of Embodiments 1-5 is significantly improved compared to Comparative Example 1; while the ionic conductivity of Comparative Example 2 is relatively low and is not affected by the standing time.
[0065] Table 2 Elastic modulus, electronic conductivity, cycle number and discharge retention rate in Examples 1-9 and Comparative Examples 1-10
[0066] Table 2 shows the elastic modulus, electronic conductivity of the sulfide solid electrolytes of different embodiments and comparative examples, and the cycle performance of the assembled solid-state batteries. The elastic modulus increases with the increase of O content, and the electronic conductivity decreases with the increase of O content. The combination of the two plays a role in inhibiting lithium dendrites, thereby helping to improve the cycle performance.
[0067] In addition, the inventors of this case also referred to the aforementioned embodiments and conducted experiments with other raw materials, process operations, and process conditions described in this specification, and obtained relatively ideal results.
[0068] It should be understood that the technical solution of the present invention is not limited to the above-mentioned specific implementation cases. Any technical deformation made according to the technical solution of the present invention without departing from the scope of protection of the purpose of the present invention and the claims shall fall within the protection scope of the present invention.
Claims
1. A sulfide solid electrolyte, Features: The sulfide solid electrolyte is an oxygen-containing solid electrolyte, and the chemical formula of the sulfide solid electrolyte is Li 6 PS a O b X, wherein X is selected from any one of F, Cl, Br, and I, and satisfies a+b=5, a / b≥4, and b>0.
2. The sulfide solid electrolyte according to claim 1, Features: The sulfide solid electrolyte has a spherical or quasi-spherical structure.
3. The sulfide solid electrolyte according to claim 1, Features: The average particle size D of the sulfide solid electrolyte 50 <1 μm; And / or, the room temperature ionic conductivity of the sulfide solid electrolyte is 1.0E-4~1.0E-2 S / cm.
4. A method for preparing the sulfide solid electrolyte according to any one of claims 1 to 3, It is characterized in that include: In a protective atmosphere, a lithium source, a P source, a S source, an O source and a halogen source are premixed, and then a high-pressure solid-phase reaction is carried out to obtain a sulfide solid electrolyte.
5. The preparation method according to claim 4, It is characterized in that Specifically include: In a protective atmosphere, a three-dimensional mixing device is used to premix a lithium source, a P source, a S source, an O source and a halogen source to obtain a premix; wherein the three-dimensional mixing device uses a rotation speed of 500-5000 rpm and a time of 5-10 hours.
6. The preparation method according to claim 4, It is characterized in that Specifically include: In a protective atmosphere, the premixed material is placed in a high-pressure torsion device for high-pressure torsion treatment, thereby obtaining the sulfide solid electrolyte; wherein the pressure used in the high-pressure torsion treatment is 50-200 MPa, the rotation frequency is 10-100 Hz, and the time is 1-3 hours.
7. The preparation method according to claim 4, Features: The lithium source includes Li 2 O, LiX, Li 2 S, LiOH, Li 2 CO 3 Any one or more combinations of; And / or, the P source includes P 2 O 5 and / or P 2 S 5 ; And / or, the S source includes Li 2 S and / or P 2 S 5 ; And / or, the O source includes Li 2 O, LiOH, Li 2 CO 3 , P 2 O 5 Any one or more combinations of; and / or, the halogen source comprises LiX; And / or, the molar ratio of the S source to the O source is 4-19:
1.
8. Use of the sulfide solid electrolyte according to any one of claims 1 to 3 in preparing a lithium battery positive electrode or a lithium ion battery.
9. A lithium battery positive electrode, It is characterized in that It comprises a positive electrode active material and a solid electrolyte; wherein the solid electrolyte comprises the sulfide solid electrolyte according to any one of claims 1 to 3.
10. A lithium ion battery, It is characterized in that It comprises a positive electrode, a negative electrode and an intermediate layer; wherein the intermediate layer comprises the sulfide solid electrolyte according to any one of claims 1 to 3, and the positive electrode comprises the lithium battery positive electrode according to claim 9.