Preparation method of glass mold for manufacturing cosmetic bottle

By adopting austenitic stainless steel materials and solid solution treatment technology, the problem of insufficient antioxidant performance and short service life of cosmetic glass bottle molds is solved, and high-precision and high-stability glass bottle molding is achieved, which improves product quality and production efficiency.

CN118993502APending Publication Date: 2024-11-22SUZHOU DONGHAI GLASS MOLD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411022452.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-29
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The existing cosmetic glass bottle molds have insufficient antioxidant performance, short service life, and complex spray welding process and high uncertainty, resulting in low yield and short market response cycle.

Method used

Austenitic stainless steel is used as the mold material, and through solid solution treatment and stress-removing annealing process, combined with high-precision processing and polishing treatment, molds with excellent oxidation resistance and high temperature resistance are formed.

Benefits of technology

It significantly improves the service life and production efficiency of the mold, improves product quality, reduces process complexity and defect rate, and achieves high precision and high stability glass bottle molding.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

According to the preparation method of the glass mold for manufacturing the cosmetic bottle, austenitic stainless steel with excellent oxidation resistance, high temperature resistance and corrosion resistance is selected, and after a blank material is subjected to solution treatment and destressing treatment, the durability of the mold is greatly improved, and the service life of the mold is greatly prolonged; and a heat preservation structure does not need to be designed and complicated spray welding treatment does not need to be carried out when the mold is prepared. The problems that in the prior art, a glass mold for manufacturing cosmetic bottles is not high in yield and short in service life, and manufactured cosmetic glass packaging bottles are poor in appearance quality yield are solved, the service life of the mold is remarkably prolonged, the production efficiency is remarkably improved, the product quality is remarkably improved, and the mold has wide application prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of glass mold manufacturing, in particular to a method for preparing a glass mold for manufacturing a cosmetic bottle. Background Art

[0002] Compared with other daily glass packaging bottles, cosmetic glass bottles are relatively smaller, lighter, and use less glass material per bottle. Therefore, the manufacturing process requirements are different from those of ordinary glass bottles. For example, the manufacturing process of ordinary beer bottles emphasizes mass production and cost-effectiveness; while the manufacturing process of cosmetic glass bottles focuses more on refinement and high quality. Therefore, for the same unit weight (for example, 1 ton) of glass material, the added value of cosmetic glass bottles is much higher than that of other ordinary daily glass packaging bottles.

[0003] Due to the characteristics of cosmetic glass bottles, there are significant differences in the molding process between cosmetic glass bottles and large glass (such as beer bottles) with relatively heavy glass drops. Since the mass of the glass drops is small and a very beautiful appearance is required, the molding temperature of cosmetic glass bottles must be increased, otherwise the molding appearance quality and yield rate of cosmetic glass bottles will be very poor; this leads to a significant increase in the requirements for the anti-oxidation performance of the mold.

[0004] The molds for cosmetic glass bottles have gradually transitioned from ordinary gray cast iron in the early days to ductile iron, and now to composite materials with gray cast iron as the base material and nickel-based alloy powder welding hardening treatment on the inner cavity glass contact surface. The above materials all have some problems in the production process. Gray cast iron can barely be used as a large glass bottle with a relatively low temperature due to its slightly poor high-temperature oxidation resistance. It is very unsuitable for cosmetic bottles with a higher production process temperature than large glass, and the service life of the mold is extremely short. Ductile iron has better oxidation resistance than gray cast iron, but it still cannot meet the production requirements of cosmetic glass bottles, because the market demand for cosmetic glass bottles is increasingly tending to carry out deep processing such as spraying, baking paint, and hot stamping to improve the beauty and added value of the bottles. After the deep processing of these cosmetic glass bottles, the original tiny defects are significantly magnified, making it increasingly difficult for the market to accept the original non-deeply processed bottles that meet the requirements. Under this circumstance, a composite mold with gray cast iron as the base material and nickel-based alloy spray welding surface hardening on the mold inner cavity glass contact surface has been developed. The cosmetic glass bottle mold produced by this process does have greatly improved anti-oxidation performance. However, because cosmetic glass bottles need to have exquisite and diversified appearance, various shapes and colors, they usually need unique appearance designs to highlight the brand image and attract consumers. As a result, due to the grotesque shape of the glass bottle, it is impossible to complete the spray welding of the mold cavity through automated nickel-based spray welding. The current nickel-based alloy process of this composite material process must be realized by artificial oxyacetylene spray welding. This leads to many problems. First, the working environment of the spray welding process is harsh, with high temperature and strong light, which requires very high experience of the operating staff and the cost of training employees is huge. Second, the process yield is relatively low. From the perspective of industry experience, there is at least 10% of the spray welding defect rate. And many spray welding defects, such as cracking, sand holes, etc., must be discovered after the production of the array machine. When they are discovered, it is too late and basically impossible to repair. The process uncertainty of nickel-based alloy surfacing poses a huge challenge to the production of cosmetic glass bottles with a very short market response cycle.

[0005] Therefore, it is of great significance to develop a cosmetic glass mold with strong durability and high stability. Summary of the invention

[0006] The main technical problem solved by the present invention is to provide a method for preparing a glass mold for manufacturing a cosmetic bottle, which has a long service life, high molding accuracy and production stability.

[0007] In order to solve the above technical problems, a technical solution adopted by the present invention is: to provide a method for preparing a glass mold for manufacturing a cosmetic bottle, the specific steps comprising:

[0008] (100) Selecting mold blank material: Selecting austenitic stainless steel as the mold blank material;

[0009] (200) Cutting: Cut the mold blank according to the drawing;

[0010] (300), solution treatment process;

[0011] (301) Heating: heating the mold blank material to a temperature range of 1040°C to 1150°C;

[0012] (302) Insulation: Insulate for 2-3 hours within the above temperature range according to the wall thickness of the mold;

[0013] (303) Rapid cooling: Rapidly cool the material to room temperature;

[0014] (400), stress relief annealing process: heating the material in the low temperature range of 200℃ to 400℃, and then slowly cooling it to room temperature to eliminate residual stress;

[0015] (500) Mold processing: Process the mold blank to ensure that the size and shape of each mold component meet the design requirements;

[0016] (600) Polishing: Polishing the mold surface.

[0017] In a preferred embodiment of the present invention, the austenitic stainless steel has the following properties: thermal conductivity is less than 20 W / m·K at 500°C.

[0018] In a preferred embodiment of the present invention, the chemical composition of the austenitic stainless steel is:

[0019] Carbon (C): ≤ 0.08%

[0020] Manganese (Mn): ≤2.00%

[0021] Silicon (Si): ≤1.50%

[0022] Phosphorus (P): ≤ 0.045%

[0023] Sulfur (S): ≤ 0.030%

[0024] Chromium (Cr): 24.00%-26.00%

[0025] Nickel (Ni):19.00%-22.00%

[0026] Molybdenum (Mo): ≤0.75%

[0027] Nitrogen (N): ≤ 0.10%

[0028] Iron (Fe): Balance.

[0029] In a preferred embodiment of the present invention, after the mold material is treated by the solid solution process and the stress relief process, the mold performance reaches:

[0030] At 600℃, creep strength, stress at 100,000 hours, is 50-70MPa; after exposure to 600℃ environment for 100 hours, the mass increase does not exceed 0.5mg / cm 2 .

[0031] In a preferred embodiment of the present invention, the rapid cooling step is performed by water quenching or rapid air cooling.

[0032] In a preferred embodiment of the present invention, after the polishing step, the mold surface achieves a mirror effect.

[0033] The beneficial effects of the present invention are as follows: the present invention provides a method for preparing a glass mold for manufacturing a cosmetic bottle, which solves the problems in the prior art of low mold yield, short mold service life, and poor appearance quality yield of the manufactured cosmetic glass packaging bottles, significantly improves the mold service life, production efficiency and product quality, and has broad application prospects. DETAILED DESCRIPTION

[0034] The preferred embodiments of the present invention are described in detail below so that the advantages and features of the present invention can be more easily understood by those skilled in the art, thereby making a clearer and more definite definition of the protection scope of the present invention.

[0035] The present invention discloses a method for preparing a glass mold for manufacturing a cosmetic bottle, and the specific steps include:

[0036] First: Select the mold blank: Select austenitic stainless steel with excellent oxidation resistance, high temperature resistance and corrosion resistance as the mold blank; the preferred austenitic stainless steel is SUS310S stainless steel, and the chemical composition is as follows:

[0037] Carbon (C): ≤0.08%, manganese (Mn): ≤2.00%, silicon (Si): ≤1.50%, phosphorus (P): ≤0.045%, sulfur (S): ≤0.030%, chromium (Cr): 24.00%-26.00%, nickel (Ni): 19.00%-22.00%, molybdenum (Mo): ≤0.75%, nitrogen (N): ≤0.10%, iron (Fe): balance.

[0038] The main elements and their functions are:

[0039] Chromium (Cr): Improves oxidation resistance and corrosion resistance. The 24-26% chromium content enables SUS310S to form a dense chromium oxide protective layer in high temperature environments.

[0040] Nickel (Ni): Improves high temperature strength and oxidation resistance. 19-22% nickel content helps maintain the stability of the austenite structure.

[0041] Carbon (C): Low carbon content (≤0.08%) helps reduce carbide precipitation, thereby improving intergranular corrosion resistance.

[0042] Manganese (Mn), Silicon (Si): Improve oxidation resistance and high temperature strength, but the content is low to prevent adverse effects on weldability and mechanical properties.

[0043] Silicon (Si) increases the oxidation resistance of steel and assists in deoxidation during the casting process.

[0044] Nitrogen (N), as an interstitial alloying element, significantly improves the strength of austenitic stainless steel through interstitial solid solution strengthening.

[0045] It is also an austenite stabilizing element, particularly beneficial in preventing the formation of martensite or ferrite phases. Nitrogen improves resistance to pitting and crevice corrosion. Nitrogen combines with chromium to form chromium nitride, which helps to increase the overall hardness and wear resistance of the steel. However, excessive nitrogen can lead to the formation of chromium nitride. This depletes the amount of free chromium available to form the protective chromium oxide layer, reducing the overall corrosion resistance of the steel. Excessive nitrogen reduces the ductility of the steel, making the material more brittle and more susceptible to cracking.

[0046] Molybdenum (Mo) significantly improves resistance to pitting and crevice corrosion and contributes to high temperature strength. It also improves the creep resistance of the steel, i.e. the ability to withstand deformation under high temperatures and long-term stress. Too much Mo can lead to the formation of brittle phases, such as sigma phase, especially at high temperatures. This can significantly reduce the toughness and ductility of the steel. Molybdenum is an expensive alloying element. It will increase the overall cost of stainless steel, making it less economical in some applications.

[0047] Phosphorus (P) and sulfur (S): As impurity elements, their content should be reduced as much as possible to improve the toughness and corrosion resistance of the material.

[0048] Second: Cut the mold blank according to the drawing;

[0049] Then, a solution treatment process and a stress relief annealing process are performed;

[0050] 1. Heating: Heat SUS310S stainless steel to a temperature range of 1040°C to 1150°C. Ensure that all carbides and other phases can be fully dissolved into the austenite matrix.

[0051] 2. Insulation: In the above temperature range, according to the wall thickness of the mold, keep warm for about 2-3 hours to ensure that the alloy elements are evenly distributed in the austenite matrix.

[0052] 3. Rapid cooling: Rapidly cool the material to room temperature, usually by water quenching or rapid air cooling. Prevent carbides from re-precipitating, so that the alloy elements are evenly distributed in the matrix, forming a stable austenite structure. Thus, the oxidation resistance and corrosion resistance of the material are improved.

[0053] 4. Heat the material at a low temperature range of 200°C to 400°C, and then slowly cool it to room temperature to eliminate residual stress.

[0054] Third: Mold processing: Precision machining of mold blanks to ensure that the size and shape of each mold component meet the design requirements. In particular, the mold surface and cavity parts need to be processed with high precision.

[0055] Fourth, the mold surface is polished with high precision. Due to the use of SUS310S austenitic stainless steel, the polishing can achieve a mirror effect, which is significantly improved compared with the polishing effect of existing materials, so as to reduce the surface defects of the glass bottle and improve the finish of the finished product.

[0056] In the daily glass packaging industry, there is an unwritten rule that within the tolerance of the mold material and without affecting the glass bottle molding process, the higher the molding temperature, the better the appearance quality of the glass bottle, whether it is a large-capacity glass bottle or a small-capacity glass bottle. In particular, small-capacity cosmetic glass bottles have particularly stringent requirements on appearance quality; since the droplets of cosmetic glass bottles are small and harden easily, the molding temperature of this type of glass bottle is about 100°C higher than that of ordinary beer bottles, liquor bottles and other glass bottles. In addition, when designing the mold, it is necessary to add a heat preservation groove or hole structure to the mold; however, the thermal conductivity of SUS310S stainless steel is not that high, so there is no need to design a heat preservation structure, which is also more advantageous for processing;

[0057] At 500°C, the thermal conductivity of SUS310S austenitic stainless steel is about 16-20W / m·K, while the thermal conductivity of ferritic ductile iron currently used as cosmetic glass molds is about 25-30W / m·K; the thermal conductivity of gray iron is about 35-45W / m·K.

[0058] Cosmetic mold materials: SUS310S austenitic stainless steel with excellent oxidation resistance, high temperature resistance and corrosion resistance is selected, and the blank material is subjected to solid solution treatment and then quenching and tempering treatment to improve the durability and service life of the mold. The creep strength of SUS310S austenitic stainless steel (at 600℃, near the mold working temperature) and the stress under 100,000 hours are about 50-70MPa, while according to available information, the creep strength of ductile iron at 350℃ is about 10-20MPa. Gray cast iron is even worse. This has a direct impact on the precision and life of the mold at high temperatures; compared with the composite mold of gray iron base material nickel-based alloy spray welding, SUS310S austenitic stainless steel does not require complex spray welding treatment, and the yield rate of mold materials is almost 100%. After being exposed to a 600℃ environment for 100 hours, the mass increase of SUS310S does not exceed 0.5mg / cm 2 . It has excellent high temperature oxidation resistance, which is unmatched by other materials.

[0059] The present invention discloses a method for preparing a glass mold for manufacturing a cosmetic bottle. Austenitic stainless steel with excellent oxidation resistance, high temperature resistance and corrosion resistance is selected, and the rough material is subjected to solid solution treatment and stress relief treatment, so that the durability and service life of the mold are greatly improved. The mold preparation does not require the design of a heat preservation structure, and does not require complex spray welding treatment.

[0060] The above descriptions are merely embodiments of the present invention and are not intended to limit the patent scope of the present invention. Any equivalent structure or equivalent process transformation made using the contents of the present invention specification, or directly or indirectly applied in other related technical fields, are also included in the patent protection scope of the present invention.

Claims

1. A method for preparing a glass mold for manufacturing a cosmetic bottle, characterized in that: The specific steps include: (100) Selecting mold blank material: Selecting austenitic stainless steel as the mold blank material; (200) Cutting: Cut the mold blank according to the drawing; (300), solution treatment process; (301) Heating: heating the mold blank material to a temperature range of 1040°C to 1150°C; (302) Insulation: Insulate for 2-3 hours within the above temperature range according to the wall thickness of the mold; (303) Rapid cooling: Rapidly cool the material to room temperature; (400), stress relief annealing process: heating the material in the low temperature range of 200℃ to 400℃, and then slowly cooling it to room temperature to eliminate residual stress; (500) Mold processing: Process the mold blank to ensure that the size and shape of each mold component meet the design requirements; (600) Polishing: Polishing the mold surface.

2. The method for preparing a glass mold for manufacturing a cosmetic bottle according to claim 1, characterized in that: The austenitic stainless steel has the following properties: at 500° C., the thermal conductivity is less than 20 W / m·K.

3. The method for preparing a glass mold for manufacturing a cosmetic bottle according to claim 1, characterized in that: The chemical composition of the austenitic stainless steel is: Carbon (C): ≤ 0.08% Manganese (Mn): ≤2.00% Silicon (Si): ≤1.50% Phosphorus (P): ≤ 0.045% Sulfur (S): ≤ 0.030% Chromium (Cr): 24.00%-26.00% Nickel (Ni):19.00%-22.00% Molybdenum (Mo): ≤0.75% Nitrogen (N): ≤0.10% Iron (Fe): Balance.

4. The method for preparing a glass mold for manufacturing a cosmetic bottle according to claim 1, characterized in that: After the mold material has been treated with the solid solution process and stress relief process, the mold performance reaches: At 600℃, creep strength, stress at 100,000 hours, is 50-70MPa; after exposure to 600℃ environment for 100 hours, the mass increase does not exceed 0.5mg / cm 2 .

5. The method for preparing a glass mold for manufacturing a cosmetic bottle according to claim 1, characterized in that: In the rapid cooling step, water quenching or rapid air cooling is performed.

6. The method for preparing a glass mold for manufacturing a cosmetic bottle according to claim 1, characterized in that: After the polishing step, the mold surface reaches a mirror effect.

Citation Information

Patent Citations

  • Novel austenitic heat-resistance stainless steel

    CN101921967A

  • Technology for producing hot melt glass die

    CN104058579A

  • High-strength heat-resisting steel plate and preparation method thereof

    CN109440012A

  • Processing method for glass mold

    CN109822304A

  • Method for cleaning mold for press-molding optical glass element

    JP1989119534A