Flame-retardant glass fiber reinforced polypropylene as well as preparation method and application thereof

The glass fiber is modified by Salen type Schiff base to form a carbon layer to improve the flame retardant performance of polypropylene composite materials, which solves the problem of unsatisfactory flame retardant performance of glass fibers in polymer composite materials in the prior art, and simplifies the preparation process And improves the stability and safety of the material.

CN118993575APending Publication Date: 2024-11-22CHONGQING COPOLYFORCE NEW MATERIALS CO LTD +1
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202411372573.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-29
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

In the prior art, glass fibers have poor flame retardant properties in polymer composite materials, and traditional flame retardant modification methods are complex and unfavorable to industrialization.

Method used

The glass fiber is modified with Salen type Schiff base, and a carbon layer is formed by forming a Salen type Schiff base with self-crosslinking and excellent expansion flame retardant properties on the surface of the glass fiber to enhance the flame retardant properties.

Benefits of technology

The flame retardant and mechanical properties of polypropylene composite materials are significantly improved, the preparation process is simplified, and the stability and safety of the material are achieved at high temperatures.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118993575A_ABST
    Figure CN118993575A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of flame-retardant modified glass fibers, in particular to flame-retardant glass fiber reinforced polypropylene as well as a preparation method and application thereof. The flame-retardant modified glass fiber is Salen type Schiff base modified glass fiber, and raw materials of the Salen type Schiff base comprise a first monomer and a second monomer, the first monomer is an aldehyde substance; the second monomer is a diamine substance. The Schiff base formed in the manner has self-crosslinking and excellent intumescent flame-retardant effects, and coats the surface of the glass fiber, so that the glass fiber composite material quickly forms an intumescent compact and hard carbon layer on the surface of the glass fiber at high temperature, and the candlewick effect is inhibited. According to the technical scheme, the technical problem that in the prior art, when flame-retardant modified glass fibers are applied to preparation of composite materials, the flame-retardant performance is not ideal can be solved. The flame-retardant glass fiber provided by the invention can be applied to preparation of a polypropylene composite material, improves the flame retardance and mechanical properties of the composite material, and has ideal popularization and application prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of flame-retardant modified glass fibers, and in particular to flame-retardant glass fiber reinforced polypropylene and a preparation method and application thereof. Background Art

[0002] Glass fiber (GF) is an inorganic non-metallic material with the advantages of high mechanical strength, strong heat resistance, good chemical resistance, and good insulation performance. It is often used as a polymer reinforcement material, which can significantly improve the mechanical properties of polymer composites. It is widely used in construction, electronics, transportation, aerospace, and national defense. Glass fiber itself is non-flammable, but in order to further improve its flame retardant properties or improve its compatibility with the polymer matrix, it can be flame-retardantly modified on its surface. This treatment is usually to ensure the safety and stability of the material at high temperatures, especially when manufacturing composite materials. The common method for flame-retardant modification of glass fiber surface is to treat the glass fiber surface with a silane coupling agent containing flame retardant elements (such as phosphorus, nitrogen, etc.). This method can not only enhance the interfacial bonding between the fiber and the resin, but also give the material certain flame retardant properties. However, this method has limited effect on increasing the flame retardant effect and cannot meet the needs of further applications for the time being.

[0003] Chinese patent CN117866330A discloses a method for preparing flame-retardant glass fiber reinforced modified polypropylene. The polypropylene is synergistically modified by using terminal olefin hyperbranched flame retardant and KH570 modified glass fiber. The olefin groups contained in the two are melt-grafted with polypropylene under the action of an initiator, which not only improves the interfacial compatibility between the hyperbranched flame retardant, the glass fiber and the polypropylene, but also cross-links to form a three-dimensional hybrid cross-linking system, which enhances the chemical cross-linking degree between the two and the polypropylene molecular chain and improves the thermal decomposition temperature of polypropylene. When using KH570 modified glass fiber to prepare polypropylene composite materials, it is also necessary to introduce terminal olefin hyperbranched flame retardant to ensure the flame retardant performance of the composite material. The preparation method of terminal olefin hyperbranched flame retardant is complicated and the preparation process is cumbersome, which is not conducive to industrialization. Therefore, it is urgent to develop a new method for flame-retardant modification of glass fiber surface and corresponding flame-retardant modified glass fiber. When using the glass fiber to prepare composite materials such as polypropylene, a reinforced polypropylene flame-retardant composite material can be obtained by a simple manufacturing process. Summary of the invention

[0004] The present invention is intended to provide a flame retardant modified glass fiber to solve the technical problem in the prior art that the flame retardant modified glass fiber has unsatisfactory flame retardant performance when applied to the preparation of composite materials.

[0005] In order to achieve the above object, the present invention adopts the following technical scheme:

[0006] A flame retardant modified glass fiber is a glass fiber modified by a Salen-type Schiff base. The raw materials of the Salen-type Schiff base include a first monomer and a second monomer. The first monomer is salicylaldehyde or 2,4-dihydroxybenzaldehyde or 2,5-dihydroxybenzaldehyde or 2,6-dihydroxybenzaldehyde or 2,3-dihydroxybenzaldehyde or 3,4-dihydroxybenzaldehyde. The second monomer is ethylenediamine or o-phenylenediamine or m-phenylenediamine or propylenediamine or butanediamine.

[0007] Furthermore, the molar ratio of the first monomer to the second monomer is 1.5-3:1.

[0008] Furthermore, the first monomer is salicylaldehyde or 2,4-dihydroxybenzaldehyde or 2,5-dihydroxybenzaldehyde; and the second monomer is ethylenediamine or o-phenylenediamine.

[0009] The present technical solution also provides a method for preparing a flame retardant modified glass fiber, comprising the following steps performed in sequence:

[0010] S1: Disperse the amino modified glass fiber in the solvent and add the first monomer to obtain GF-NH 2 dispersion; dissolving the second monomer in a solvent to obtain a diamine solution;

[0011] S2: Add the diamine solution dropwise to the GF-NH 2 In the dispersion, flame retardant modified glass fiber is obtained through reaction.

[0012] Furthermore, in S1, the usage ratio of the amino modified glass fiber and the solvent is 50-500 g: 200-5000 ml; and the total mass of the first monomer and the second monomer is 5-50% of the amino modified glass fiber.

[0013] Further, in S1, the solvent is any one of ethanol, water, DMF, DMSO and acetonitrile.

[0014] Furthermore, in S2, the dropping speed of the diamine solution is 0.5-5 drops / second; and the reaction time after the dropping is completed is 2-12 hours.

[0015] Furthermore, the amino-modified glass fiber is prepared by the following method: 50-500g of glass fiber is dispersed in 200-2000ml of an aqueous solution of 50-99% ethanol by volume, and an amino coupling agent is added at a mass of 0.1-10% of the mass of the glass fiber under stirring at a speed of 500-1500rpm, and then reacted at 60-100°C for 4-8h; after the reaction is completed, the amino-modified glass fiber is obtained by washing and drying.

[0016] The technical solution also provides an application of a flame retardant modified glass fiber in the preparation of a polypropylene composite material. The raw materials of the polypropylene composite material include, by weight, 40-65 parts of polypropylene, 14-22 parts of a flame retardant, 20-30 parts of a flame retardant modified glass fiber, 1-10 parts of a compatibilizer, 0.1-1 parts of an antioxidant, and 0.1-1 parts of white oil.

[0017] Furthermore, the first monomer is 2,4-dihydroxybenzaldehyde, and the second monomer is ethylenediamine.

[0018] Furthermore, the addition amount of the flame retardant modified glass fiber in the polypropylene composite material is 30%.

[0019] In this technical solution, "Salen" is a special Schiff base with self-crosslinking and excellent intumescent flame retardant properties. The "Salen" intumescent flame retardant with excellent carbonization effect is coated on the surface of the glass fiber, so that the polymer / GF composite material quickly forms an intumescent, dense and hard carbon layer on the surface of the glass fiber GF at high temperature, thereby greatly suppressing the "wick effect". The Salen-type Schiff base of this solution is formed on the surface of the glass fiber by a first monomer (aldehyde substance) and a second monomer (diamine substance). The first monomer is selected from at least one of salicylaldehyde, 2,4-dihydroxybenzaldehyde, 2,5-dihydroxybenzaldehyde, 2,6-dihydroxybenzaldehyde, 2,3-dihydroxybenzaldehyde, and 3,4-dihydroxybenzaldehyde, and the second monomer is selected from at least one of ethylenediamine, o-phenylenediamine, m-phenylenediamine, propylenediamine, and butanediamine. The glass fiber modified with the Salen-type Schiff base formed in the above manner can form a carbon layer on the surface of the glass fiber when burning to achieve a flame retardant effect.

[0020] The Salen-type Schiff base modified glass fiber of this scheme can be used in the preparation of composite materials, especially in the preparation of polypropylene composite materials, to increase the flame retardancy and mechanical properties of the composite materials. And for polypropylene composite materials, the Salen-type Schiff base modified glass fiber uses 2,4-dihydroxybenzaldehyde and ethylenediamine as the reaction monomers of the Salen-type Schiff base, which can significantly improve the mechanical properties and flame retardancy of the composite materials. In addition, the addition amount of the Salen-type Schiff base modified glass fiber in polypropylene is preferably 30%. And in polypropylene, the combination of piperazine pyrophosphate and melamine polyphosphate is preferably used as the common flame retardant used in compounding. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 Schematic diagram of the structure of the amino-modified glass fiber and the Salen-type Schiff base of Example 1.

[0022] Figure 2Schematic diagram of the structure of the Salen-type Schiff base modified glass fiber (GF@Salen) of Example 1.

[0023] Figure 3 This is a typical photo of the Salen-type Schiff base-modified long glass fiber of Preparation Example 1 after combustion treatment.

[0024] Figure 4 This is a typical photo of the unburned long glass fiber of Preparation Example 1 after being burned. DETAILED DESCRIPTION

[0025] The present invention is further described in detail below in conjunction with examples, but the embodiments of the present invention are not limited thereto. Unless otherwise specified, the technical means used in the following examples and experimental examples are conventional means well known to those skilled in the art, and the materials, reagents, etc. used can be obtained from commercial sources.

[0026] Example 1: Preparation of GF@Salen

[0027] Amino modification of glass fiber: amino silane coupling agent is used to react in ethanol / water solution at a temperature of about 60-100°C to obtain amino modified glass fiber (GF-NH 2 ). You can also directly purchase amino-modified glass fiber available on the market.

[0028] 50-500g (preferably 100g) of glass fiber (GF) is dispersed in 200-2000ml of an ethanol aqueous solution with a volume percentage of 50-99% (preferably 500ml, 90%, i.e., the volume ratio of ethanol to water is 450:50), and an amino coupling agent (preferably KH550) with a mass of 0.1-10% (preferably 1%) of the mass of GF is added under high-speed stirring at 500-1500rpm (preferably 1000rpm), and the temperature is raised from room temperature to 60-100℃ (preferably 80℃) for reaction for 4-8h (preferably 6h). After the reaction is completed, the mixture is filtered, washed, and dried at 50-120℃ (preferably 80℃) to obtain amino-modified glass fiber GF-NH 2 .

[0029] Synthesis of Salen-type Schiff base modified glass fiber (GF@Salen): GF-NH 2 Dispersed in a solvent, one of the two Salen monomers (such as aldehyde) is first added to the mixed solution, and then the diamine dispersed in the same solvent is dropped into the mixed solution.

[0030] 50-500 g (preferably 100 g) of GF-NH 2The mixture is uniformly dispersed in 200-5000 ml (preferably 400 ml) of solvent, and a first monomer (the first monomer is an aldehyde substance, such as salicylaldehyde or 2,4-dihydroxybenzaldehyde or 2,5-dihydroxybenzaldehyde or 2,6-dihydroxybenzaldehyde or 2,3-dihydroxybenzaldehyde) is added to obtain GF-NH 2 Next, the second monomer (the second monomer is a diamine substance, such as ethylenediamine, o-phenylenediamine, m-phenylenediamine, propylenediamine, butanediamine, etc.) is dissolved in 50-1000 ml of solvent (preferably 100 ml) to obtain a diamine solution. The solvent can be any one of ethanol, water, DMF, DMSO, acetonitrile and other organic solvents; the molar ratio of the first monomer (aldehyde) to the second monomer (diamine) is 1.5-3:1 (preferably 2:1), in the above GF-NH 2 In the case of the amount of dispersion and diamine solution, the total mass of the first monomer and the second monomer is GF-NH 2 The diamine solution is slowly added to GF-NH at a rate of 0.5-5 drops / second (preferably 1 drop / second). 2 After the dropwise addition is completed, the reaction is continued for 2-12 hours (preferably 4 hours). After the reaction is completed, the mixture is filtered, washed, and dried at 50-100°C (preferably 80°C) to obtain GF@Salen.

[0031] See the structural diagram of amino modified glass fiber for details. Figure 1 Left, taking the first monomer (salicylaldehyde) and the second monomer (ethylenediamine) as an example, the structural formula of the Salen-type Schiff base can be found in Figure 1 Right: Schematic diagram of Salen-type Schiff base modified glass fiber (GF@Salen) Figure 2 (Take the Salen-type Schiff base synthesized from 2,4-dihydroxybenzaldehyde and ethylenediamine as an example).

[0032] Example 2: Preparation of flame retardant modified glass fiber (GF@Salen) reinforced composite polypropylene material

[0033] In parts by weight, the raw materials of GF@Salen reinforced composite nylon material include: 40-65 parts of polypropylene, 14-22 parts of flame retardant (piperazine pyrophosphate), 20-30 parts of flame retardant modified glass fiber (GF@Salen), 1-10 parts of compatibilizer (KT-1), 0.1-1 part of antioxidant (antioxidant 1010 and / or antioxidant 168), and 0.1-1 part of white oil.

[0034] The flame retardant may be selected from at least one of piperazine pyrophosphate (QZ10-2, produced by Chongqing Kejufu New Materials Co., Ltd.), melamine polyphosphate (MPP, produced by Chongqing Kejufu New Materials Co., Ltd.), melamine cyanurate (MCA) and ammonium polyphosphate (APP). Polypropylene includes two homopolymers of high melt index polypropylene (e.g., PPT30S) and low melt index polypropylene (e.g., PP Y40) with a mass ratio of 1:1.5-2.5.

[0035] After drying the above raw materials, mix them evenly with a high mixer, and then use a screw extruder to melt and extrude them into granules to obtain pellets of flame-retardant modified glass fiber reinforced composite nylon materials. The obtained pellets are dried at 80°C for 12 hours and then injection molded by an injection molding machine to obtain test samples or other products. The temperatures of each section of the extruder are 180±10°C, 200±10°C, 210±10°C, 210±10°C (in the subsequent specific preparation process, the parameters of 180°C, 200°C, 210°C, 210°C), and the main screw speed is 35±1HZ; the temperatures of each section of the injection molding machine are: 180±10°C, 200±10°C, 210±10°C, 210±10°C (in the subsequent specific preparation process, the parameters of 180°C, 200°C, 210°C, 210°C).

[0036] Preparation Example 1

[0037] 100 g of glass fiber (GF, Taishan glass fiber, T435N, diameter 10 μm; in this specific preparation example, the glass fiber is in the form of chopped glass fiber, and the fiber length is controlled at 3-4 mm) was dispersed in 500 ml of ethanol aqueous solution (the volume ratio of ethanol to water is 450:50), and under high-speed stirring at 800 rpm, 1% of the mass of GF amino coupling agent KH550 was added, and the reaction was heated from room temperature to 80°C for 6 hours. After the reaction was completed, the amino-modified glass fiber (GF-NH 2 ). In actual operation, any type of glass fiber can be selected, and the fiber length can be selected according to actual conditions. The glass fiber mainly provides a substrate with a Salen-type Schiff base surface modification.

[0038] 100g GF-NH 2 Evenly dispersed in 400 ml of ethanol, and added the first monomer (2,4-dihydroxybenzaldehyde) to obtain GF-NH 2 Then the second monomer (ethylenediamine) is dissolved in 100 ml of ethanol to obtain a diamine solution. The molar ratio of 2,4-dihydroxybenzaldehyde to ethylenediamine is 2:1, and the sum of the masses of 2,4-dihydroxybenzaldehyde and ethylenediamine is GF-NH 2 The diamine solution was slowly dripped into GF-NH at a rate of 1 drop / second.2 After the addition was completed, the dispersion was reacted for 4 h. After the reaction was completed, the dispersion was filtered, washed, and dried at 80° C. to obtain the Salen-type Schiff base-modified glass fiber GF@Salen (named GF@Salen1).

[0039] Long glass fibers were modified with a Salen-type Schiff base using the method of this preparation example, and the modified long fibers were then subjected to a combustion treatment. Typical photos of the fibers are shown in FIG. Figure 3 As shown. The long glass fiber is directly burned. Typical photos are as follows Figure 4 As shown. The above experiment is mainly to demonstrate the intuitive effect of Salen-type Schiff base modification. The first monomer is selected from at least one of salicylaldehyde, 2,4-dihydroxybenzaldehyde, 2,5-dihydroxybenzaldehyde, 2,6-dihydroxybenzaldehyde, 2,3-dihydroxybenzaldehyde, and 3,4-dihydroxybenzaldehyde, and the second monomer is selected from at least one of ethylenediamine, o-phenylenediamine, m-phenylenediamine, propylenediamine, and butylene diamine. The glass fiber modified with the Salen-type Schiff base formed in accordance with this scheme can form a dense and hard carbon layer on the surface of the glass fiber when burning to achieve a flame retardant effect.

[0040] Preparation Example 2

[0041] This preparation example is basically the same as Preparation Example 1, except that the first monomer is replaced by 2,5-dihydroxybenzaldehyde in an equal molar amount, and the second monomer is replaced by o-phenylenediamine in an equal molar amount. Other conditions are the same as Preparation Example 1 (named GF@Salen2).

[0042] Preparation Example 3

[0043] This preparation example is basically the same as Preparation Example 1, except that an equal molar amount of the first monomer is replaced by salicylaldehyde, and an equal molar amount of the second monomer is replaced by o-phenylenediamine. Other conditions are the same as Preparation Example 1 (named GF@Salen3).

[0044] The flame retardant modified glass fiber reinforced composite polypropylene material was prepared using the GF@Salen of the above-mentioned preparation examples 1-3. The raw materials are shown in Table 1, and the preparation method is the same as that of Example 2. The synthesized composite material was subjected to performance tests, and the experimental results are shown in Table 1. Among them. The UL-94 (3.2 mm, 1.6 mm, 0.8 mm) detection method refers to the standard GB / T 2408-2008 / IEC; the limiting oxygen index (LOI) test refers to the standard ASTM-D2863. The tensile performance test method refers to the standard GB / T 1040.2-2022, and the cantilever beam impact test test method refers to the standard GB1843-2008.

[0045] Table 1: Raw material composition (parts) and performance test results of flame retardant modified glass fiber reinforced composite polypropylene materials (t1 represents the time of spontaneous combustion of the specimen after the first ignition in the vertical combustion test, t2 represents the time of spontaneous combustion of the specimen after the second ignition in the vertical combustion test, and NR represents no grade)

[0046]

[0047] From the above experimental data, it can be seen that the addition of flame retardant modified glass fiber has a greatly improved effect on the flame retardant properties of polypropylene composites compared to the addition of unmodified glass fiber or amino-modified glass fiber. For details, see the comparison between composite materials 1-3 and composite materials 7 and composite material 9.

[0048] In addition, for polypropylene composites, the modification effect of GF@Salen1 is the most ideal, which can simultaneously ensure the mechanical properties and flame retardant properties of the composites. The first monomer used in GF@Salen1 is 2,4-dihydroxybenzaldehyde, and the second monomer is ethylenediamine (composite material 1); the first monomer used in GF@Salen2 is 2,5-dihydroxybenzaldehyde, and the second monomer is o-phenylenediamine (composite material 2); the first monomer used in GF@Salen3 is salicylaldehyde, and the second monomer is o-phenylenediamine (composite material 3). Comparing composite materials 2 and 3, 2,5-dihydroxybenzaldehyde is used to replace salicylaldehyde. Although there are only two hydroxyl groups between the two, the former has a very significant effect on improving the flame retardant properties of the composite material. In composite material 1, the 2,4-dihydroxybenzaldehyde used is an isomer of 2,5-dihydroxybenzaldehyde. When 2,4-dihydroxybenzaldehyde is combined with ethylenediamine to form a Salen-type Schiff base modification, its effect on improving the flame retardant properties of the composite material is very significant (compared with composite material 2). Therefore, GF@Salen1 modified glass fiber is the best choice. In addition, the flame retardant modified glass fiber is preferably 30 parts in polypropylene to maintain a relatively ideal flame retardant effect, while adding 20 parts of flame retardant modified glass fiber will significantly reduce the flame retardant effect.

[0049] In addition, the flame retardants used in combination with flame retardant modified glass fiber are piperazine pyrophosphate (QZ10-2, produced by Chongqing Kejufu New Materials Co., Ltd.) and melamine polyphosphate (MPP, produced by Chongqing Kejufu New Materials Co., Ltd.). After a large number of experiments, the inventor found that the combination of QZ10-2 and MPP has the most obvious effect on improving the flame retardant properties of polypropylene composite materials added with flame retardant modified glass fiber. The inventor tried to prepare composite material 11. The raw material composition and preparation process of composite material 11 are basically the same as those of composite material 1, except that QZ10-2 and MPP flame retardant are replaced with 17 parts of QZ10-2. The inventor also tried to prepare composite material 12. The raw material composition and preparation process of composite material 12 are basically the same as those of composite material 1, except that QZ10-2 and MPP flame retardant are replaced with 17 parts of MPP. In the UL-94 test of composite materials 11 and 12, only the 3.2 mm specimens passed the V-0 grade, while the 1.6 mm and 0.8 mm specimens did not pass the grade, which was different from the flame retardant performance of composite material 1. This shows that adding a certain proportion of QZ10-2 and MPP flame retardant to the polypropylene composite material with GF@Salen1 can maximize the flame retardant performance of the composite material.

[0050] The inventors also tried to make composite material 13. The raw material composition and preparation process of composite material 13 are basically the same as composite material 9, except that QZ10-2 and MPP flame retardant are replaced by 17 parts of QZ10-2. The inventors also tried to make composite material 14. The raw material composition and preparation process of composite material 14 are basically the same as composite material 9, except that QZ10-2 and MPP flame retardant are replaced by 17 parts of MPP. The test results of 3.2mm, 1.6mm and 0.8 strips of UL-94 test of composite materials 13 and 14 are all NR (no grade). The above experimental results further illustrate that when GF@Salen is applied to polypropylene composite materials, the combined use of QZ10-2 and MPP flame retardant is very critical to improving the flame retardant properties of the composite materials.

[0051] The above is only an embodiment of the present invention, and the common knowledge such as the known specific technical solutions and / or characteristics in the solution is not described in detail here. It should be pointed out that for those skilled in the art, without departing from the technical solution of the present invention, several modifications and improvements can be made, which should also be regarded as the protection scope of the present invention, and these will not affect the effect of the implementation of the present invention and the practicality of the patent. The scope of protection required by this application shall be based on the content of its claims, and the specific implementation methods and other records in the specification can be used to interpret the content of the claims.

Claims

1. A flame retardant modified glass fiber, characterized in that: The glass fiber is modified by a Salen-type Schiff base, and the raw materials of the Salen-type Schiff base include a first monomer and a second monomer; the first monomer is salicylaldehyde or 2,4-dihydroxybenzaldehyde or 2,5-dihydroxybenzaldehyde or 2,6-dihydroxybenzaldehyde or 2,3-dihydroxybenzaldehyde or 3,4-dihydroxybenzaldehyde; the second monomer is ethylenediamine or o-phenylenediamine or m-phenylenediamine or propylenediamine or butylenediamine.

2. The flame retardant modified glass fiber according to claim 1, characterized in that: The molar ratio of the first monomer to the second monomer is 1.5-3:1; the first monomer is salicylaldehyde or 2,4-dihydroxybenzaldehyde or 2,5-dihydroxybenzaldehyde; and the second monomer is ethylenediamine or o-phenylenediamine.

3. The method for preparing a flame retardant modified glass fiber according to claim 1 or 2, characterized in that: The method includes the following steps: S1: dispersing the amino-modified glass fiber in a solvent and adding the first monomer to obtain a GF-NH2 dispersion; dissolving the second monomer in the solvent to obtain a diamine solution; S2: Add the diamine solution dropwise into the GF-NH2 dispersion to obtain flame-retardant modified glass fiber through reaction.

4. The method for preparing a flame retardant modified glass fiber according to claim 3, characterized in that: In S1, the usage ratio of the amino modified glass fiber and the solvent is 50-500g:200-5000ml; the total mass of the first monomer and the second monomer is 5-50% of the amino modified glass fiber.

5. The method for preparing a flame retardant modified glass fiber according to claim 4, characterized in that: In S1, the solvent is any one of ethanol, water, DMF, DMSO and acetonitrile.

6. The method for preparing a flame retardant modified glass fiber according to claim 5, characterized in that: In S2, the diamine solution is added at a rate of 0.5-5 drops / second; and the reaction time after the addition is completed is 2-12 hours.

7. The method for preparing a flame retardant modified glass fiber according to claim 6, characterized in that: The amino modified glass fiber is prepared by the following method: 50-500g of glass fiber is dispersed in 200-2000ml of an ethanol aqueous solution with a volume percentage of 50-99%, and an amino coupling agent is added at a mass of 0.1-10% of the mass of the glass fiber under stirring at a speed of 500-1500rpm, and then reacted at 60-100°C for 4-8h; after the reaction is completed, the amino modified glass fiber is obtained by washing and drying.

8. Use of a flame retardant modified glass fiber according to claim 1 or 2 in the preparation of a polypropylene composite material, characterized in that: The raw materials of the polypropylene composite material include 40-65 parts of polypropylene, 14-22 parts of flame retardant, 20-30 parts of flame retardant modified glass fiber, 1-10 parts of compatibilizer, 0.1-1 parts of antioxidant and 0.1-1 parts of white oil in parts by weight.

9. The use of a flame retardant modified glass fiber in the preparation of a polypropylene composite material according to claim 8, characterized in that: The first monomer is 2,4-dihydroxybenzaldehyde, and the second monomer is ethylenediamine.

10. The use of a flame retardant modified glass fiber in the preparation of a polypropylene composite material according to claim 9, characterized in that: The addition amount of flame retardant modified glass fiber in the polypropylene composite material is 30%.

Citation Information

Patent Citations

  • Halogen-free fiberglass reinforced polypropylene composite material and preparation method thereof

    CN109679203A