High-activity auxiliary cementing material as well as preparation method and application thereof

The method of enhancing solid waste through carbonization has improved its hydration activity and safety, solved the problems of low hydration activity and poor stability of solid waste in the prior art, achieved efficient solid waste utilization, and simplified The process flow and reduces energy consumption.

CN118993583APending Publication Date: 2024-11-22BEIJING BUILDING MATERIALS ACADEMY OF SCI RES
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410949841.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-16
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The prior art has constraints on energy consumption and cost when improving the hydration activity of solid waste, and some solid wastes such as steel slag have poor stability, which affects their efficient use in concrete.

Method used

Using the carbonization enhancement method, by premixing solid waste with carbonization additives and passing CO2 gas into powder, forming a highly active auxiliary gelling material, improving the hydration activity and safety of solid waste, simplifying the process flow and Reduce energy consumption.

Benefits of technology

It significantly improves the activity of solid waste at different hydration ages, improves its comprehensive utilization efficiency in concrete, reduces process costs and energy consumption, and enhances safety.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118993583A_ABST
    Figure CN118993583A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of building materials, in particular to a high-activity auxiliary cementing material as well as a preparation method and application thereof. The invention relates to a high-activity auxiliary cementing material which is characterized by comprising 84-80 parts by weight of solid waste and 10-16 parts by weight of a carbonization aid, the carbonization auxiliary agent comprises an auxiliary agent A, an auxiliary agent B, an auxiliary agent C and water. According to the preparation method of the auxiliary cementing material, provided by the invention, through the cooperation of grinding and carbonization, the hydration activity can be remarkably improved, and meanwhile, carbon dioxide is consumed.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of building materials, and in particular to a high-activity auxiliary gelling material and a preparation method and application thereof. Background Art

[0002] Solid wastes such as steel slag, magnesium slag, construction waste, and carbide slag are stored in large quantities, and their comprehensive resource utilization efficiency is low. They will pollute the environment, occupy a large amount of land area, and have adverse effects on the social economy. Therefore, effective methods are urgently needed to improve the technical level.

[0003] Cement concrete is a more effective way to dispose of solid waste, but it requires industrial waste to have good hydration activity. Currently, there are methods such as physical activation, chemical activation, and thermal activation to improve the hydration activity of solid waste. Although the activity has been improved to a certain extent, there are still constraints in terms of energy consumption and cost.

[0004] In view of this, the present invention is proposed. Summary of the invention

[0005] The purpose of the present invention is to provide a high-activity auxiliary cementitious material and a preparation method and application thereof, so as to improve the comprehensive utilization level of solid waste and also absorb part of industrial waste gas. Specifically, since the efficient utilization of solid waste in concrete requires higher hydration activity and safety, but different industrial solid wastes generally have the problem of low activity, and some solid wastes such as steel slag also have the safety problem of poor stability, so the carbonization enhancement method is adopted to improve safety and enhance hydration activity.

[0006] Based on this, the present invention has the following technical solutions: In a first aspect, the present invention provides a high-activity auxiliary cementitious material, comprising 84 to 80 parts by weight of solid waste and 10 to 16 parts by weight of a carbonization aid; the carbonization aid comprises an aid A, an aid B, an aid C and water.

[0007] Preferably, the auxiliary agent A comprises one or more of polycarboxylic acid, formic acid, acetic acid and tartaric acid.

[0008] Preferably, the auxiliary agent B includes one or more of zeolite, activated carbon and carbon molecular sieve.

[0009] Preferably, the auxiliary agent C includes one or more of ethanolamine, diethanolamine, diisopropanolamine and triethanolamine.

[0010] Preferably, the high-activity auxiliary gelling material comprises 84-80 parts by weight of solid waste and 10-16 parts by weight of a carbonization aid; the carbonization aid comprises acetic acid, zeolite, polyol amine and water.

[0011] Preferably, the mass ratio of the auxiliary agent A, auxiliary agent B, auxiliary agent C and water is (1-2): (1-2): (1-3): (93-97); the mass of the auxiliary agent A, auxiliary agent B and auxiliary agent C is the dry basis content.

[0012] In the present invention, the dry basis content can be obtained by drying and weighing.

[0013] Preferably, the solid waste includes one or more of steel slag, magnesium slag, construction waste and carbide slag.

[0014] Preferably, the fineness of the solid waste does not exceed 1 mm.

[0015] In a second aspect, the present invention provides a method for preparing the highly active auxiliary gelling material, comprising: premixing the solid waste with the carbonization aid, sealing the mixture, and introducing a mixture containing CO 2 The gas is fed in and grinding begins at the same time, and the discharge after a certain period of grinding is the high-activity gelling material.

[0016] In the present invention, steel slag, magnesium slag, construction waste, and carbide slag belong to alkaline solid wastes, and the mineral components thereof, such as silicate ore phase, gel product, calcium hydroxide, and calcium oxide, are easily reacted with CO 2 Chemical reactions occur to form calcium carbonate and amorphous silica gel products. Calcium carbonate has a nucleating effect, which can improve the early hydration activity. The formation of amorphous silica gel can improve the activity of volcanic ash, which is beneficial to the formation of later strength. Therefore, after carbonization, the activity of solid waste at different hydration ages can be comprehensively improved, which is beneficial to the comprehensive utilization of solid waste.

[0017] Preferably, the grinding time is 30 to 120 minutes.

[0018] Preferably, the CO 2 In the gas, CO 2 The concentration is greater than 17%.

[0019] The present invention adopts a synergistic method of grinding and carbonization to prepare a high-activity auxiliary gelling material, which can avoid the phenomenon that fine particles adsorbed during the carbonization process cause the particles to increase in size and hinder the carbonization process, and can also avoid secondary grinding, making the process simpler and ready for use. In addition, due to the synergistic method of grinding and carbonization, the requirements for the fineness of solid waste are lower, reducing the energy consumption of front-end processing.

[0020] The present invention provides a method for efficiently preparing auxiliary cementitious materials by synergizing grinding and carbonization, which can significantly improve the hydration activity by optimizing the raw material formula. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] In order to more clearly illustrate the technical solutions in the present invention or the prior art, the following briefly introduces the drawings required for use in the embodiments or the description of the prior art. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0022] Figure 1 The present invention provides a production flow chart of a high-activity auxiliary gelling material. DETAILED DESCRIPTION

[0023] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be clearly and completely described below in conjunction with the drawings of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0024] Unless otherwise specified, all raw materials used in the examples are commercially available conventional raw materials, and the technical means used are conventional means well known to those skilled in the art.

[0025] Example 1

[0026] This embodiment provides a high-activity auxiliary gelling material (production flow chart see Figure 1 ), the preparation method of which comprises the following steps: (1) Crush and screen the steel slag to obtain particles smaller than 1 mm; (2) preparing carbonization aids, including aid A acetic acid, aid B zeolite, aid C ethanolamine and triethanolamine (volume ratio 1 / 1), and water, with a mass ratio of 1:1:1:97; (3) mixing the steel slag particles and the carbonization aid in a mass ratio of 85:15 to obtain a mixture; (4) Grinding the powder, introducing industrial waste gas, CO 2 Concentration 20%,

[0027] (5) Grind for 60 minutes and then discharge the material.

[0028] Example 2

[0029] This embodiment provides a high-activity auxiliary gelling material (production flow chart see Figure 1 ), the preparation method of which comprises the following steps: (1) Crush and screen the steel slag to obtain particles smaller than 1 mm; (2) preparing carbonization aids, including aid A acetic acid, aid B zeolite, aid C ethanolamine and triethanolamine (volume ratio 1 / 1), and water, with a mass ratio of 2:1:1:96; (3) mixing the steel slag particles and the carbonization aid in a mass ratio of 85:15 to obtain a mixture; (4) Grinding the powder, introducing industrial waste gas, CO 2 Concentration 20%,

[0030] (5) Grind for 60 minutes and then discharge the material.

[0031] Example 3

[0032] This embodiment provides a high-activity auxiliary gelling material (production flow chart see Figure 1 ), the preparation method of which comprises the following steps: (1) Crush and screen the steel slag to obtain particles smaller than 1 mm; (2) preparing carbonization aids, including aid A acetic acid, aid B zeolite, aid C ethanolamine and triethanolamine (volume ratio 1 / 1), and water, with a mass ratio of 2:1:3:94; (3) mixing the steel slag particles and the carbonization aid in a mass ratio of 85:15 to obtain a mixture; (4) Grinding the powder, introducing industrial waste gas, CO 2 Concentration 20%,

[0033] (5) Grind for 60 minutes and then discharge the material.

[0034] Example 4

[0035] This embodiment provides a high-activity auxiliary gelling material (production flow chart see Figure 1 ), the preparation method of which comprises the following steps: (1) Crush and screen the steel slag to obtain particles smaller than 1 mm; (2) preparing carbonization aids, including aid A acetic acid, aid B zeolite, aid C ethanolamine and triethanolamine (volume ratio 1 / 1), and water, with a mass ratio of 2:2:3:93; (3) mixing the steel slag particles and the carbonization aid in a mass ratio of 85:15 to obtain a mixture; (4) Grinding the powder, introducing industrial waste gas, CO 2 Concentration 20%,

[0036] (5) Grind for 60 minutes and then discharge the material.

[0037] Example 5

[0038] This embodiment provides a high-activity auxiliary gelling material (production flow chart see Figure 1 ), the preparation method of which comprises the following steps: (1) Crush and screen the steel slag to obtain particles smaller than 1 mm; (2) preparing carbonization aids, including aid A acetic acid, aid B zeolite, aid C ethanolamine and triethanolamine (volume ratio 1 / 1), and water, with a mass ratio of 1:1:3:95; (3) mixing the steel slag particles and the carbonization aid in a mass ratio of 85:15 to obtain a mixture; (4) Grinding the powder, introducing industrial waste gas, CO 2 Concentration 20%,

[0039] (5) Grind for 60 minutes and then discharge the material.

[0040] Example 6

[0041] This embodiment provides a high-activity auxiliary gelling material (production flow chart see Figure 1 ), the preparation method of which comprises the following steps: (1) Crush and screen the steel slag to obtain particles smaller than 1 mm; (2) preparing carbonization aids, including aid A acetic acid, aid B zeolite, aid C triethanolamine, and water, in a mass ratio of 1:1:2:96; (3) mixing the steel slag particles and the carbonization aid in a mass ratio of 85:15 to obtain a mixture; (4) Grinding the powder, introducing industrial waste gas, CO 2 Concentration 20%,

[0042] (5) Grind for 60 minutes and then discharge the material.

[0043] Example 7

[0044] This embodiment provides a high-activity auxiliary gelling material (production flow chart see Figure 1 ), the preparation method of which comprises the following steps: (1) Crush and screen the construction waste to obtain particles smaller than 1 mm; (2) preparing carbonization aids, including aid A acetic acid, aid B zeolite, aid C triethanolamine, and water, in a mass ratio of 1:1:2:96; (3) mixing the steel slag particles and the carbonization aid in a mass ratio of 85:15 to obtain a mixture; (4) Grinding the powder, introducing industrial waste gas, CO 2 Concentration 20%,

[0045] (5) Grind for 60 minutes and then discharge the material.

[0046] Comparative Example 1

[0047] This comparative example provides a steel slag powder, and the preparation method thereof comprises the following steps: (1) Crush and screen the steel slag to obtain particles smaller than 1 mm; (2) Grind for 60 minutes and then discharge the material.

[0048] Comparative Example 2

[0049] This comparative example provides a steel slag powder, and the preparation method thereof comprises the following steps: (1) Crush and screen the steel slag to obtain particles smaller than 1 mm; (2) mixing steel slag particles and water in a mass ratio of 85:15 to obtain a mixture; (3) Grinding the powder, introducing industrial waste gas, CO 2 Concentration 20%; (4) Grind for 60 minutes and then discharge the material.

[0050] Comparative Example 3

[0051] This comparative example provides a steel slag powder, and the preparation method thereof comprises the following steps: (1) Crush and screen the steel slag to obtain particles smaller than 1 mm; (2) mixing steel slag particles and water in a mass ratio of 85:15 to obtain a mixture; (3) Grinding the powder, introducing industrial waste gas, CO 2 Concentration 20%, static carbonization 60min; (4) Grinding after discharge.

[0052] Comparative Example 4

[0053] This comparative example provides a construction waste fine powder, and the preparation method thereof comprises the following steps: (1) Crush and screen the construction waste to obtain particles smaller than 1 mm; (2) Grind for 60 minutes and then discharge the material.

[0054] Comparative Example 5

[0055] This comparative example provides a construction waste fine powder, and the preparation method thereof comprises the following steps: (1) Crush and screen the construction waste to obtain particles smaller than 1 mm; (2) mixing the construction waste particles and water in a mass ratio of 85:15 to obtain a mixture; (3) Grinding the powder, introducing industrial waste gas, CO 2 Concentration 20%; (4) Grind for 60 minutes and then discharge the material.

[0056] Comparative Example 6

[0057] (1) Crush and screen the construction waste to obtain particles smaller than 1 mm; (2) mixing the construction waste particles and water in a mass ratio of 85:15 to obtain a mixture; (3) Grinding the powder, introducing industrial waste gas, CO 2 Concentration 20%, static carbonization 60min; (4) Grinding after discharge.

[0058] It should be noted that the grinding time of the comparative example and the embodiment of the present invention is the same in order to better observe the beneficial effects of the technology of the present invention.

[0059] The present invention further conducts an activity index test on the auxiliary cementitious materials prepared in the embodiments and comparative examples, and the method comprises: using 30% of the auxiliary cementitious materials to replace the reference cement, testing the compressive strength at 7d and 28d, and the ratio of the compressive strength to the compressive strength of 100% of the reference cement at the same age is the activity index.

[0060] The results are shown in Table 1: Table 1 Test results of different cases.

[0061]

[0062] From the test results in Table 1, it can be seen that the activity index of steel slag powder and construction waste powder after simple grinding is at a low level. However, after simple carbonization, although its activity has increased, it is not significant and is still below 80%. After adding carbonization aids, the activity index has been further improved compared with simple carbonization. It can also be seen that the activity is not significantly improved after carbonization and then grinding.

[0063] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A highly active auxiliary gelling material, characterized in that: The method comprises 84 to 80 parts by weight of solid waste and 10 to 16 parts by weight of a carbonization aid; the carbonization aid comprises an aid A, an aid B, an aid C and water.

2. The high-activity auxiliary gelling material according to claim 1, characterized in that: The auxiliary agent A includes one or more of polycarboxylic acid, formic acid, acetic acid and tartaric acid.

3. The high-activity auxiliary gelling material according to claim 1, characterized in that: The auxiliary agent B includes one or more of zeolite, activated carbon and carbon molecular sieve.

4. The high-activity auxiliary gelling material according to claim 1, characterized in that: The auxiliary agent C includes one or more of ethanolamine, diethanolamine, diisopropanolamine and triethanolamine.

5. The high-activity auxiliary gelling material according to claim 1, characterized in that: The invention comprises 84 to 80 parts by weight of solid waste and 10 to 16 parts by weight of a carbonization aid; the carbonization aid comprises acetic acid, zeolite, polyol amine and water.

6. The high-activity auxiliary gelling material according to any one of claims 1 to 5, characterized in that: The mass ratio of the auxiliary agent A, auxiliary agent B, auxiliary agent C and water is (1-2): (1-2): (1-3): (93-97); the mass of the auxiliary agent A, auxiliary agent B and auxiliary agent C is the dry basis content.

7. The high-activity auxiliary gelling material according to any one of claims 1 to 6, characterized in that: The solid waste includes one or more of steel slag, magnesium slag, construction waste and carbide slag; Preferably, the fineness of the solid waste does not exceed 1 mm.

8. The method for preparing the high-activity auxiliary gelling material according to any one of claims 1 to 7, characterized in that: include: The solid waste is premixed with the carbonization aid, and then sealed and introduced with gas containing CO2. The high-activity gelling material is discharged after grinding.

9. The method for preparing a high-activity auxiliary gelling material according to claim 8, characterized in that: The CO2 concentration in the CO2-containing gas is greater than 17%.

10. An admixture for mortar or concrete, characterized in that: It contains the high-activity auxiliary gelling material as claimed in claim 8.