Preparation method of alkali-resistant basalt fiber for cement-based cementing material

CN118993596AActive Publication Date: 2024-11-22JIAHUA SPECIAL CEMENT
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411010048.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2024-11-22
Estimated Expiration
2044-07-26

AI Technical Summary

Technical Problem

The reaction of basalt fibers with OH- in an alkaline environment causes its mechanical properties to deteriorate in cement-based cementitious materials, and alkali-resistant basalt fibers need to be developed to improve their alkali-resistant properties.

Method used

By mixing basalt with the additive ball mill, heat treatment is used to form a melt, quench and wire drawing, and then coated with nanoTiO2 and nanoTa2O5-loaded alkali-resistant slurry during the wire drawing process to form alkali-resistant basalt fibers, using zircon and gold The synergistic action of redite and barite enhances the alkali resistance of fibers.

Benefits of technology

The alkali resistance and tensile resistance of basalt fibers are significantly improved, and the protective layer is formed to slow down the erosion of alkali solution, enhance the stability of the fiber, and avoid fiber dissolution and damage.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118993596A_ABST
    Figure CN118993596A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of alkali-resistant basalt fiber for a cement-based cementing material, which comprises the following steps: mixing basalt and an additive through ball milling to obtain a basalt fiber raw material; the preparation method comprises the following steps: gradually heating a basalt fiber raw material to 1350-1600 DEG C, and homogenizing for 5-10 hours to obtain a basalt melt; the basalt melt is quenched, and basalt glass is obtained; basalt glass is subjected to wire drawing under the condition of 1250-1450 DEG C to generate hot fibers, the hot fibers are modified to obtain the alkali-resistant basalt fibers, and the modification is that the hot fibers are coated with the alkali-resistant slurry in the wire drawing process. The alkali resistance of the basalt fiber can be improved, and the effect of long-term performance stability of the basalt fiber reinforced cement-based material is achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of building materials, and in particular to a method for preparing alkali-resistant basalt fiber for cement-based cementitious materials. Background Art

[0002] Continuous basalt fiber is an environmentally friendly material extruded from molten volcanic rock at a temperature of 1400-1500℃. Basalt fiber is considered to be a good reinforcement material for cement matrix due to its advantages such as good modulus, high strength, large failure strain, good stability, and resistance to thermal and chemical corrosion. Basalt fiber has no chemical reaction when in contact with other chemical substances and is an eco-friendly material. However, the main component of the basalt fiber network skeleton is Si-O bond, which can still react with OH- in an alkaline environment. Therefore, it is urgent to develop an alkali-resistant basalt fiber to improve the degradation of the mechanical properties of basalt fiber and its reinforced cement-based cementitious products. Summary of the invention

[0003] The object of the present invention is to provide a method for preparing alkali-resistant basalt fiber for cement-based cementitious materials, so as to improve the alkali resistance of basalt fiber in cement-based cementitious materials.

[0004] To achieve the above purpose, the technical solution adopted by the present invention is as follows:

[0005] A method for preparing alkali-resistant basalt fiber for cement-based cementitious materials comprises the following steps:

[0006] S1, mixing basalt and additives by ball milling to obtain basalt fiber raw material;

[0007] S2, gradually heating the basalt fiber raw material to 1350-1600°C, and then homogenizing for 5-10 hours to obtain basalt melt;

[0008] S3, quenching the basalt melt to obtain basalt glass;

[0009] S4, drawing the basalt glass at 1250-1450° C. to produce hot fibers, and modifying the hot fibers to obtain alkali-resistant basalt fibers, wherein the modification is to coat the alkali-resistant slurry on the hot fibers during the drawing process.

[0010] In S4, during the drawing process, the alkali-resistant slurry is coated on the hot fiber through a container connected to the liquid funnel on the drawing machine.

[0011] Preferably, in S1, basalt and additives are mixed by ball milling and then separated from the grinding balls by a sieve plate to obtain basalt fiber raw material;

[0012] Preferably, in S3, the basalt melt is quickly poured onto a heat-resistant steel plate and quenched to obtain basalt glass;

[0013] Preferably, in S4, the basalt glass is drawn at 1320° C. using a platinum-rhodium alloy bushing.

[0014] Furthermore, the alkali-resistant slurry is obtained by loading nano-TiO2 and nano-Ta2O5 on montmorillonite, and the preparation method comprises the following steps:

[0015] Step A: Slowly drip 10 mL of 6 mol / L HCl into 2.5 mL of 0.08 mol / L TiCl4 solution to obtain a first solution, then slowly add distilled water to dilute the first solution to a volume of 100 mL, stir thoroughly until the first solution is clear, then add 5 mol / L ammonia water to adjust the pH value of the first solution to 8-9, the volume ratio of ammonia water to the first solution is 1:1, and then age at room temperature for 3 hours to obtain a nano-TiO2 precursor solution;

[0016] Step B: 8 g of tantalum ethoxide is added to 20 mL of ethanol to prepare a tantalum ethoxide-ethanol solution, and then distilled water is slowly added to dilute the volume of the tantalum ethoxide-ethanol solution to 100 mL, and then 5 mol / L ammonia water is added to adjust the pH value of the tantalum ethoxide-ethanol solution to 8-9, and the volume ratio of ammonia water to tantalum ethoxide-ethanol solution is 1:1. The temperature is raised to 80°C-85°C and kept for 30 minutes to obtain a nano-Ta2O5 precursor solution;

[0017] Step C: treating sodium montmorillonite in distilled water with ultrasonic waves to obtain a montmorillonite suspension, wherein the solid content of the montmorillonite suspension is 20 wt %;

[0018] Step D: 5 mmol Ti per 1 g montmorillonite 4+ and 5mmol Ta 5+ The nano-TiO2 precursor solution and the nano-Ta2O5 precursor solution are added dropwise to the montmorillonite suspension and stirred evenly. The pH is adjusted to 5-7 with boric acid to obtain an alkali-resistant slurry. The final concentration of montmorillonite in the alkali-resistant slurry is 4 g / L.

[0019] Furthermore, the additives include rutile, barite and zircon.

[0020] Furthermore, the basalt fiber raw material includes the following components in weight percentage:

[0021]

[0022] Furthermore, the main component of the rutile is TiO2, and the content of TiO2 is ≥95wt%; the main component of the barite is BaSO4, and the content of BaSO4 is 92-98wt%; the zircon contains the following components in weight percentage: ZrO2: 62-67wt%, SiO2: 28-32wt%.

[0023] Furthermore, the basalt contains the following minerals in weight percentage: SiO2: 45-55wt%, Al2O3: 12-15wt%, Fe2O3: 9.5-13wt%, TiO2: 2.0-3.0wt%, CaO: 5.0-8.5wt%, MgO: 5.0-8.5wt%, K2O: 1.5-3.5wt%, Na2O: 3.5-4.5wt%.

[0024] Furthermore, the average particle size of the basalt fiber raw material is 65-80 μm.

[0025] Furthermore, in S2, the basalt fiber raw material is preferably placed in a high-temperature muffle furnace and heated to 1000°C at 250°C / h, and further heated to 1550°C at 30°C / h, and then homogenized at 1550°C for 6h to obtain a basalt melt.

[0026] Compared with the prior art, the present invention has the following beneficial effects:

[0027] 1. The zircon used in the present invention contains Zr element, rutile contains Ti element, and Zr 4+ 、Ti 4+ and Si 4+ The radius of Zr is similar. 4+ 、Ti 4+ Can be in the form of a network [ZrO4] 4+ 、[TiO4] 4+ Replace part of Si in the form of 4+ , to connect the broken silicon-oxygen network. [ZrO4] 4+ 、[TiO4] 4+ and [SiO4] 4+ The titanium silicate mixed skeleton is formed, the network structure is strengthened, and the alkali resistance and tensile strength of basalt fiber are improved. Barite is a barium-containing sulfate mineral, in which BaSO4 is a hardly soluble compound that can resist alkali corrosion. Therefore, the synergistic effect of zircon, rutile and barite can significantly improve the fiber's alkali corrosion resistance.

[0028] 2. When basalt fiber is used in cementitious materials, OH - Slowly diffuse into the fiber, destroying the silicon-aluminum network structure, while Si and Al diffuse into the solution in the form of soluble ions.2+ , Fe 3+ , Ca 2+ 、Zr 4+ and Ti 4+ Slowly diffuse to the surface, generate alkali-resistant compounds, form a protective layer, and slow down the further damage of the fiber in the alkali solution. 4+ and Ti 4+ The co-produced protective layer is better than that of Zr alone. 4+ or Ti 4+ The resulting protective layer has better density and can greatly improve the alkali resistance of basalt fiber.

[0029] 3. Unlike other studies on modified basalt fibers, the present invention uses basalt fibers as a substrate, does not require cumbersome steps, and performs surface modification through a one-step method. Since the temperature is relatively high when the fiber is just pulled out, the montmorillonite loaded with nano-TiO2 and nano-Ta2O5 is easily deposited on the basalt fiber, and the alkali-resistant slurry has good dispersibility and can be evenly coated on the surface of the basalt fiber. The basalt fiber reacts with the silanol of the montmorillonite to form a new Si-O-Si bond, thereby improving the alkali resistance and tensile properties of the basalt fiber.

[0030] TiO2 and Ta2O5 are very stable under acidic and alkaline conditions, and can prevent the invasion of alkaline solutions, thereby inhibiting the dissolution and destruction of fibers. At the same time, the montmorillonite coated with nano-TiO2 and nano-Ta2O5 has a large specific surface area, and the addition of Ta2O5 increases the -OH groups on the surface of the TiO2 coating, which react with the OH groups in the cement-based cementitious materials. - React and form negative charge on the coating surface, increasing the adsorption capacity of montmorillonite and making Ca 2+ , Ba 2+ etc. are deposited on the coating surface, forming a denser surface protective layer, which limits the corrosive alkaline medium from entering the fiber. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 This is a microstructure diagram of the alkali-resistant basalt fiber of Example 1 of the present invention.

[0032] Figure 2 This is a microstructure diagram of ordinary basalt fiber in comparative example 1 of the present invention. DETAILED DESCRIPTION

[0033] In order to make the purpose, technical scheme and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments and drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0034] In each embodiment of the present invention, the method for preparing alkali-resistant basalt fiber for cement-based cementitious material comprises the following steps:

[0035] S1, mixing basalt and additives by ball milling, and then separating them from the grinding balls through a sieve plate to obtain basalt fiber raw materials;

[0036] S2, placing the basalt fiber raw material in a high-temperature muffle furnace and heating it to 1000°C at 250°C / h, and further heating it to 1550°C at 30°C / h, and then homogenizing it at 1550°C for 6h to obtain a basalt melt;

[0037] S3, quickly pouring the basalt melt onto a heat-resistant steel plate for quenching to obtain basalt glass;

[0038] S4. Drawing basalt glass at 1320° C. using a platinum-rhodium alloy bushing to produce hot fibers, and coating the hot fibers with an alkali-resistant slurry during the drawing process to obtain alkali-resistant basalt fibers.

[0039] Example 1

[0040] As a preferred embodiment of the present invention, this embodiment provides an alkali-resistant basalt fiber for cement-based cementitious materials. In this embodiment, the basalt fiber raw material includes the following components in weight percentage:

[0041]

[0042] Example 2

[0043] As a preferred embodiment of the present invention, this embodiment provides an alkali-resistant basalt fiber for cement-based cementitious materials. In this embodiment, the basalt fiber raw material includes the following components in weight percentage:

[0044]

[0045] Example 3

[0046] As a preferred embodiment of the present invention, this embodiment provides an alkali-resistant basalt fiber for cement-based cementitious materials. In this embodiment, the basalt fiber raw material includes the following components in weight percentage:

[0047]

[0048] Example 4

[0049] As a preferred embodiment of the present invention, this embodiment provides an alkali-resistant basalt fiber for cement-based cementitious materials. In this embodiment, the basalt fiber raw material includes the following components in weight percentage:

[0050]

[0051] Comparative Example 1

[0052] The basalt fiber in this comparative example adopts ordinary basalt fiber, which comes from Sichuan Aerospace Tuoxin Basalt Industry Co., Ltd.

[0053] Comparative Example 2

[0054] The basalt fiber of this comparative example has the same basalt fiber raw material as that of Example 1, but in the preparation method, no alkali-resistant slurry is added during drawing.

[0055] The basalt fibers of the embodiments and comparative examples were placed in a NaOH solution with a temperature of 80°C and a mass fraction of 5wt% for accelerated aging, and were rinsed with deionized water after 6h, 24h, and 96h, and then kept at 105°C in a drying oven for 1h. The fibers were taken out and placed in a desiccator to cool to room temperature to measure their weight loss and tensile strength at break. The test results are shown in Table 1 below.

[0056] Table 1

[0057]

[0058] According to Table 1, after being immersed in 5wt% NaOH solution for 24h, the ordinary basalt fiber in Comparative Example 1 has been completely corroded and the fiber is broken. The strength retention rate of each time period of Examples 1-4 is significantly greater than that of Comparative Example 1-2, and after 96h of accelerated aging, Examples 1-4 and Comparative Example 2 still retain a certain residual strength. Compared with Comparative Example 1, Examples 1-4 show that the alkali-resistant basalt fiber of the present invention can effectively improve the alkali resistance strength of basalt fiber and reduce alkali resistance loss. Compared with Comparative Example 2, Example 1 shows that the alkali-resistant slurry can further improve the alkali resistance of basalt fiber.

[0059] Figure 1 and Figure 2 The microstructure diagrams are respectively of the alkali-resistant basalt fiber of Example 1 accelerated aging for 6 hours and the ordinary basalt fiber of Comparative Example 1 accelerated aging for 6 hours. After 6 hours of accelerated aging, a few pits appeared on the fiber surface of Example 1, while serious damage occurred on the fiber surface of Comparative Example 1. Therefore, the alkali-resistant basalt fiber of the present invention can effectively improve the alkali resistance of basalt fiber.

[0060] Finally, it should be noted that the above embodiments are only preferred embodiments of the present invention to illustrate the technical solutions of the present invention, rather than limiting them, and certainly not limiting the patent scope of the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions recorded in the aforementioned embodiments, or replace some or all of the technical features therein by equivalents. These modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present invention. In other words, any changes or modifications made to the main design concept and spirit of the present invention that have no substantive significance, and the technical problems they solve are still consistent with the present invention, should be included in the protection scope of the present invention. In addition, the direct or indirect application of the technical solutions of the present invention in other related technical fields is also included in the patent protection scope of the present invention.

Claims

1. A method for preparing alkali-resistant basalt fiber for cement-based cementitious materials, It is characterized in that The following steps are involved: S1, mixing basalt and additives by ball milling to obtain basalt fiber raw material; S2, gradually heating the basalt fiber raw material to 1350-1600°C, and then homogenizing for 5-10 hours to obtain basalt melt; S3, quenching the basalt melt to obtain basalt glass; S4, drawing the basalt glass at 1250-1450° C. to produce hot fibers, and modifying the hot fibers to obtain alkali-resistant basalt fibers, wherein the modification is to coat the alkali-resistant slurry on the hot fibers during the drawing process.

2. The method for preparing an alkali-resistant basalt fiber for cement-based cementitious materials according to claim 1, It is characterized in that The alkali-resistant slurry is nano-TiO 2 With nano-Ta 2 O 5 The preparation method of the obtained product is carried out by loading on montmorillonite, and comprises the following steps: Step A: 10 mL of 6 mol / L HCl was slowly dripped into 2.5 mL of 0.08 mol / L TiCl4 solution to obtain a first solution, and then distilled water was slowly added to dilute the first solution to a volume of 100 mL, and the solution was stirred until the first solution was clear, and then 5 mol / L ammonia water was added to adjust the pH value of the first solution to 8-9, and the volume ratio of ammonia water to the first solution was 1:1, and the solution was aged at room temperature for 3 h to obtain nano-TiO 2 Precursor solution; Step B: 8 g of tantalum ethoxide was added to 20 mL of ethanol to prepare tantalum ethoxide-ethanol solution, and then distilled water was slowly added to dilute the volume of the tantalum ethoxide-ethanol solution to 100 mL, and then ammonia water with a concentration of 5 mol / L was added to adjust the pH value of the tantalum ethoxide-ethanol solution to 8-9, and the volume ratio of ammonia water to tantalum ethoxide-ethanol solution was 1:

1. The temperature was raised to 80°C-85°C and kept for 30 minutes to obtain nano-Ta. 2 O 5 Precursor solution; Step C: treating sodium montmorillonite in distilled water with ultrasonic waves to obtain a montmorillonite suspension, wherein the solid content of the montmorillonite suspension is 20 wt %; Step D: 5 mmol Ti per 1 g montmorillonite 4+ and 5mmol Ta 5+ The amount of nano-TiO 2 Precursor solution and nano-Ta 2 O 5 The precursor solution is added dropwise to the montmorillonite suspension and stirred evenly. Boric acid is used to adjust the pH to 5-7 to obtain an alkali-resistant slurry. The final concentration of montmorillonite in the alkali-resistant slurry is 4 g / L.

3. The method for preparing an alkali-resistant basalt fiber for cement-based cementitious materials according to claim 1, It is characterized in that The additives include rutile, barite and zircon.

4. The method for preparing an alkali-resistant basalt fiber for cement-based cementitious materials according to claim 3, It is characterized in that The basalt fiber raw material includes the following components in weight percentage:

5. The method for preparing the alkali-resistant basalt fiber for cement-based cementitious materials according to claim 3, It is characterized in that The main component of rutile is TiO 2 , TiO 2 The content of ≥95wt%; the main component of the barite is BaSO 4 ,BaSO 4 The content is 92-98wt%; the zircon contains the following components in weight percentage: ZrO 2 :62-67wt%SiO 2 :28-32wt%.

6. The method for preparing an alkali-resistant basalt fiber for cement-based cementitious materials according to claim 1, It is characterized in that The basalt contains the following minerals in weight percentage: SiO 2 :45-55wt%Al 2 O 3 :12~15wt%Fe 2 O 3 :9.5~13wt%TiO 2 :2.0~3.0wt%, CaO: 5.0~8.5wt%, MgO: 5.0~8.5wt%, K 2 O: 1.5~3.5wt%Na 2 O: 3.5~4.5wt%.

7. The method for preparing the alkali-resistant basalt fiber for cement-based cementitious materials according to claim 1, It is characterized in that The average particle size of the basalt fiber raw material is 65-80 μm.

8. The method for preparing the alkali-resistant basalt fiber for cement-based cementitious materials according to claim 1, It is characterized in that Preferably, in S2, the basalt fiber raw material is placed in a high-temperature muffle furnace and heated to 1000°C at 250°C / h, and further heated to 1550°C at 30°C / h, and then homogenized at 1550°C for 6h to obtain a basalt melt.

Citation Information

Patent Citations

  • High alkali-resistant basalt fiber and preparation method thereof

    CN113121120A

  • High-strength alkali-resistant basalt fiber and preparation method thereof

    CN115959834A

  • Multi-mineral combined alkali-resistant basalt fiber raw material formula and preparation method

    CN116354608A

  • Alkali-resistant basalt continuous fibre and its production method

    CN1272561A