Burning-free and steaming-free tailing brick and preparation method thereof
By measuring and adjusting the active silicon-aluminum content of iron tailings sand, fume and bauxite, and using alkali exciters to prepare tailings bricks, the problems of low compressive strength and high energy consumption of tailings bricks are solved, and high efficiency and low energy are achieved The production of tailings bricks consumed to meet the strength and environmental protection goals of national standards.
Patent Information
- Application Number
- CN202411169527.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-24
- Publication Date
- 2024-11-22
AI Technical Summary
In the prior art, the tailings bricks prepared by iron tailings have low compressive strength, high energy consumption during the preparation process, and the active silicon-aluminum content in iron tailings is low, which cannot meet the national standards.
The solid raw materials and alkali exciters are used to prepare sintered and distilled tailings bricks. By measuring the active silicon-aluminum content, the active silicon-aluminum molar ratio in the raw materials is adjusted. Iron tailings sand, silica fume and bauxite are used as raw materials, and silicon is used Sodium acid and sodium hydroxide are alkaline excitants, and inactive substances are dissolved through alkaline solution to form a stable gelling material.
The compressive strength of tailings bricks has been improved to reach 31.32MPa, and the MU20 level that meets the "Non-sintered waste tailings bricks" standard has been reduced, energy consumption has been realized, high-value utilization of iron tailings has been reduced, and resource waste and environment have been reduced. pollute.
Smart Images

Figure BDA0005008811010000031 
Figure BDA0005008811010000061 
Figure BDA0005008811010000062
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of unburned bricks, and in particular to an unburned and steamed tailings brick and a preparation method thereof. Background Art
[0002] Iron tailings formed after iron ore mining is one of the main sources of industrial waste. A large amount of undeveloped iron tailings has caused the piled iron tailings to occupy land resources, pollute the environment, and cause disasters and accidents, resulting in loss of life and property of the people. It is a major problem that needs to be dealt with efficiently. The resource utilization of iron tailings not only reduces resource waste and turns waste into treasure, but also reduces the pollution caused by iron tailings to the environment, and also brings huge economic benefits.
[0003] Since the chemical composition of iron tailings contains Al2O3 and SiO2, in recent years, the use of silicon and aluminum in iron tailings to produce high value-added products such as tailings bricks has become a research focus of comprehensive utilization of solid waste. For example, Chinese patent CN112897955A discloses a non-burning tailings brick with iron tailings as the main raw material, but the tailings utilization rate of this method is low, and the compressive strength of the tailings bricks prepared is low; Chinese patent CN103496933A discloses a method for preparing high-silicon iron tailings pressure-steamed bricks, which requires a large amount of sulfuric acid for pretreatment, and the preparation process requires high temperature and high pressure conditions, high energy consumption, and the compressive strength of the tailings bricks prepared is low; Chinese patent CN109111208A discloses a method for preparing iron tailings sintered bricks, which has high energy consumption and low compressive strength of the tailings bricks.
[0004] The part of silicon and aluminum in iron tailings that can be dissolved by alkali and participate in gel formation is usually called active silicon and aluminum. The content of active silicon and aluminum in the raw material has an important influence on the mechanical strength of the cementitious material. However, the content of active silicon and aluminum in iron tailings is low and the particle size is fine. It cannot meet the national standards when directly used as the raw material for tailings bricks. Therefore, adjusting the content of active silicon and aluminum in the raw material is an important issue that needs to be solved in the preparation of tailings bricks with good mechanical properties. Summary of the invention
[0005] In view of the technical problems existing in the prior art, the purpose of the present invention is to provide a non-burning and non-steaming tailings brick and a preparation method thereof.
[0006] In order to achieve the above object, the present invention adopts the following technical solutions:
[0007] The first aspect of the present invention provides a non-fired and non-steamed tailings brick, which is prepared from solid raw materials and an alkali activator. The solid raw materials include, by weight, 70% to 90% iron tailings sand, 4% silica ash, and 6% to 26% bauxite; the alkali activator is a mixture of sodium silicate, which accounts for 23% to 25% of the solid raw materials, 4% to 6% of sodium hydroxide, and 20% to 22% of water.
[0008] Preferably, the alkaline activator is a mixture of 23% sodium silicate, 4% sodium hydroxide and 22% water, accounting for 23% of the solid raw materials.
[0009] The second aspect of the present invention provides a method for preparing the above-mentioned unburned and unsteamed tailings bricks, comprising the following steps:
[0010] S1. Determine the active silicon and aluminum content to obtain the formula of the unburned and unsteamed tailings brick;
[0011] S11, determining the silicon content and aluminum content in each raw material of iron ore tailings, silica fume and bauxite;
[0012] S12, dissolving the raw materials with an alkaline solution to obtain an inactive substance, and testing the silicon and aluminum content in the obtained inactive substance to obtain the content of inactive silicon and aluminum in each raw material;
[0013] S13, calculating the active silicon and aluminum content in each raw material according to the initial silicon and aluminum content and the inactive silicon and aluminum content of each raw material;
[0014] S14, using silica ash and bauxite as silicon source and aluminum source to adjust the active silicon-aluminum molar ratio of the raw material, the calculation formula of the active silicon-aluminum molar ratio is as follows:
[0015]
[0016] Then, a formula for preparing unburned and unsteamed tailings bricks is obtained;
[0017] S2. Preparation of unburned and unsteamed tailings bricks:
[0018] S21, weighing iron tailings sand, silica fume, and bauxite according to the obtained formula, and mixing them evenly to obtain a dry material;
[0019] S22, preparing an alkali activator according to the obtained formula, and then adding the obtained alkali activator to the dry material, stirring to make the dry material and the alkali activator mix evenly, to obtain a wet mixed material;
[0020] S23, placing the wet mixture in a mold, placing it on a vibrator for shaking, scraping the mold surface flat with a scraper, drying, curing and forming, demolding, and obtaining a brick;
[0021] S24, curing the brick blank to obtain a steaming-free and burning-free tailings brick.
[0022] Preferably, the alkali used for the alkaline dissolution is a 10 mol / L sodium hydroxide solution, the liquid-to-solid ratio of the alkaline solution to the material to be dissolved is 100:1 mL / g, and the alkaline dissolution time is 7 days.
[0023] Preferably, in step S13, the active silicon and aluminum content in the alkali-soluble material is tested, including the steps of: taking the material to be tested and fully stirring it in an alkaline solution to obtain a turbid liquid, filtering it to obtain a filtrate and a filter residue, testing the inactive silicon and aluminum content in the filter residue, and subtracting the inactive silicon and aluminum content from the initial silicon and aluminum content of the raw material to obtain the active silicon and aluminum content of the raw material.
[0024] Preferably, in step S23, the drying temperature is 50-60° C.; and the curing time is 24-32 hours.
[0025] Preferably, in step S22, the stirring and mixing time is 5-12 minutes.
[0026] Preferably, the curing includes two stages: constant temperature curing at 20°C from day 1 to day 7, and natural curing after day 7 until day 28.
[0027] Compared with the prior art, the present invention has the following beneficial effects:
[0028] (1) From the perspective of molecular structure, in a low silicon-aluminum ratio system, free Si(OH)4 and Al(OH)4 - The monomers combine with each other and condense in the form of hydrated ions to form a long-chain (-Si-O-Al-O-)PS type gelling material with an oligomer dimer morphology and low structural strength. The present invention increases the active silicon-to-aluminum ratio, and the continuous increase in Si content increases the content of elemental silicon. The increase in Si(OH)4 monomers will promote the formation of more Si-O-Si bonds, forming a more stable bond structure. As the active silicon-to-aluminum molar ratio increases, the content of elemental silicon dissolved in the system is much higher than that of aluminum. At the same time, part of Si(OH)4 condenses to form a dimer state, and then reacts with Al(OH)4 - The present invention not only effectively alleviates the problem of low active silicon-aluminum components in iron tailings, but also further improves the high-value utilization rate of iron tailings. The unconfined compressive strength of the tailings brick prepared by the present invention can reach up to 31.32MPa, which can reach the MU20 level of the "Non-sintered Garbage Tailings Brick" standard. The preparation process does not require high-temperature sintering and pressure steaming, and has low energy consumption.
[0029] (2) The present invention uses iron tailings as the main raw material, and adjusts the size of the active silicon-aluminum ratio by controlling the proportion of bauxite added to optimize the mechanical properties of the tailings brick. By adjusting the active silicon-aluminum ratio of the raw material, it helps to maximize the application benefits of iron tailings in the production process of tailings bricks, and has certain economic benefits. It not only effectively alleviates the problem of low active silicon-aluminum components in iron tailings, but also further improves the high-value utilization rate of iron tailings, provides technical support for the resource utilization of iron tailings, reduces resource waste, turns waste into treasure, and reduces the pollution caused by iron tailings to the environment. The present invention uses iron tailings, silica fume, and bauxite as raw materials, which are all solid waste-based materials, easy to obtain, low-carbon, and environmentally friendly. It conforms to the concept of "carbon peak and carbon neutrality", and can effectively solve the harm caused to the environment by the above three solid wastes, and provides technical support for the coordinated disposal of large solid wastes such as tailings in the regional environment, and realizes the resource utilization and harmless treatment of solid wastes. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 is the XRD pattern of iron tailings;
[0031] Figure 2 is the particle size distribution diagram of iron tailings;
[0032] Figure 3 is the XRD pattern of bauxite;
[0033] Figure 4 This is the XRD pattern of silica fume. DETAILED DESCRIPTION
[0034] The technical solutions in the embodiments of the present invention will be described clearly and completely below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments.
[0035] Example 1
[0036] A method for preparing a non-burning and non-steaming tailings brick comprises the following steps:
[0037] S1. Determination of active silicon and aluminum content:
[0038] (1) Determine the silicon content and aluminum content in each raw material of iron ore tailings, silica fume and bauxite;
[0039] The iron tailings used in the present invention were taken from the tailings dam of the Dongshan Ore Dressing Plant of Ma Steel in Anhui Province. After drying, crushing and sieving, the iron tailings sand required for the test was obtained and set aside. A small amount of iron tailings was taken and analyzed by X-ray diffraction. Its main mineral composition, chemical composition and particle size distribution were shown in Figures 1-2 and see Table 1.
[0040] Depend on Figure 1It can be seen that the main mineral components of this iron tailings are quartz, calcium feldspar, hematite and albite.
[0041] Table 1
[0042]
[0043] From the results in Table 1, it can be seen that SiO2 is the majority in this iron tailings, reaching 44.72%, followed by Al2O3. These two components are the main substances involved in the formation of gel.
[0044] The particle size distribution of iron tailings is shown in Figure 2 .Depend on Figure 2 It can be seen that the main particles of iron tailings are concentrated around 50μm, a small number of large particles are close to 600μm, and a small number of small particles are around 1μm in size; the total amount of particles smaller than 50μm accounts for 53%.
[0045] The silica ash used in the present invention is taken from a company in Henan Province. Its chemical composition is 98.71% SiO2, which can be used as a silicon source for adjusting active silicon and aluminum. After drying and sieving, samples are taken for XRD analysis. The results are as follows: Figure 3 As shown. Figure 3 It can be seen that the main component of silica fume is quartz.
[0046] The bauxite used in the present invention is taken from a company in Henan Province. Its chemical composition is 85.03% Al2O3, 9.06% SiO2, and a small amount of Fe2O3 and CaO. It can be used as an aluminum source for adjusting active silicon and aluminum. After drying and sieving, samples are taken for XRD analysis. The results are as follows: Figure 4 shown.
[0047] Depend on Figure 4 It can be seen that the main components of this bauxite are mullite, quartz and corundum.
[0048] (2) Each raw material was added to a 10 mol / L sodium hydroxide solution, and the liquid-solid ratio of the sodium hydroxide solution to the material to be dissolved was controlled to be 100:1 mL / g. The mixture was stirred fully and the alkaline dissolution was performed for 7 days. The material to be tested was stirred fully in the sodium hydroxide solution to obtain a turbid liquid. The turbid liquid was filtered to obtain a filtrate and a filter residue. The silicon and aluminum content in the inactive substance in the filter residue was tested by XRF fluorescence to obtain the inactive silicon and aluminum content in each raw material. The initial silicon and aluminum content of the raw material was subtracted from the inactive silicon and aluminum content to obtain the active silicon and aluminum content of the raw material. The results are shown in Table 2.
[0049] Table 2. Activity test results
[0050]
[0051]
[0052] (3) The active silicon-aluminum molar ratio of the raw material is adjusted by using silica fume and bauxite as the silicon source and aluminum source. The calculation formula of the active silicon-aluminum molar ratio is as follows:
[0053]
[0054] The iron tailings are used as the main raw material, and the molar ratio of active silicon to aluminum is adjusted by controlling the proportion of bauxite added, so as to obtain a formula for preparing tailings bricks.
[0055] Among them, silica fume as a silicon source can improve the strength of tailings bricks, but excessive silica fume will bring about an air entrainment effect, making it difficult for the slurry to flow and form a dense structure, which is manifested as a decrease in macroscopic compressive strength. Therefore, the optimal silica fume dosage of the present invention is 4%, and the formula for preparing tailings bricks is obtained:
[0056] A non-fired and non-steamed tailings brick is prepared from solid raw materials and an alkali activator. Based on 100% by weight, the solid raw materials include 70% iron tailings sand, 4% silica fume, and 26% bauxite. The alkali activator is a mixture of 23% by solid weight of sodium silicate, 4% by solid weight of sodium hydroxide, and 22% by solid weight of water.
[0057] S21, according to the obtained formula, 70 parts of iron tailings, 4 parts of silica fume, and 26 parts of bauxite are weighed and mixed evenly to obtain a dry material;
[0058] S22, according to the obtained formula, weigh 23 parts of sodium silicate, 4 parts of sodium hydroxide, and 22 parts of water to prepare an alkali activator, and add the alkali activator to the dry material, and stir to mix the dry material and the alkali activator evenly to obtain a wet mixture;
[0059] S23, placing the wet mixture in a mold, placing it on a vibrating machine for shaking, scraping the mold surface flat with a scraper, drying, curing and forming, demolding, and obtaining a brick;
[0060] S24, curing the bricks to obtain steaming-free and fire-free tailings bricks.
[0061] Example 2
[0062] It is basically the same as Example 1, except that the raw materials in the formula are different. The specific formula and the results of the active Si / Al content determination are shown in Table 3.
[0063] Example 3
[0064] It is basically the same as Example 1, except that the raw materials in the formula are different. The specific formula and the results of the active Si / Al content determination are shown in Table 3.
[0065] Comparative Example 1
[0066] It is basically the same as Example 1, except that the formula is different. The specific formula and the results of the active Si / Al content determination are shown in Table 3.
[0067] Comparative Example 2
[0068] It is basically the same as Example 1, except that the formula is different. The specific formula and the results of the active Si / Al content determination are shown in Table 3.
[0069] Table 3 shows the raw material composition and active Si / Al results of Examples 1 to 3 and Comparative Examples 1 to 2
[0070]
[0071] The calculations involved are as follows:
[0072]
[0073] According to GB / T 2542-2012 "Test Method for Wall Bricks", the compressive strength of the tailings bricks prepared in Examples 1 to 3 and Comparative Examples 1 to 2 was tested. The compressive strength standard of tailings bricks is based on JC-T 422-2007 "Non-sintered Garbage Tailings Bricks". After testing, the compressive strength of the iron tailings steam-free bricks prepared in Comparative Example 1 after curing for 3 days, 7 days, and 28 days is 7.92MPa, 11.72MPa, and 15.02MPa. The addition of sodium hydroxide will make the OH in the system - The concentration of ions increases, penetrating the surface of iron tailing particles and Ca 2+ Combined with and dissociated the glassy structure in the iron tailings, making more Ca 2+ Freed, at the same time in OH - Under the action of the Al-O-Al and Si-O-Si bonds in the iron tailings break to generate SiO4 4- With AlO4 5- , the ions in the system undergo a series of reactions to generate a large amount of flocculent gels such as CASH, which greatly promotes the hydration process of the gel material, thereby making the tailings bricks have a certain strength. The compressive strength of the iron tailings steam-free and unburned bricks prepared in Comparative Example 2 after curing for 3 days, 7 days, and 28 days is 12.97MPa, 15.42MPa, and 18.47MPa. Compared with Comparative Example 1, the excitation effect of sodium silicate in Comparative Example 2 is better than that of sodium hydroxide. This is because sodium silicate has a dual excitation effect on the excitation of iron tailings. After hydrolysis, sodium silicate generates sodium hydroxide and hydrated silica gel, which not only provides OH - , and provides SiO4 4- , OH - It has a similar effect to sodium hydroxide in Example 1, SiO4 4-The increase further promotes the hydration process, which improves the strength of the tailings bricks. The compressive strength of the iron tailings steam-free bricks prepared in Example 1 after curing for 3 days, 7 days, and 28 days is 7.92MPa, 11.72MPa, and 15.02MPa; the compressive strength of the iron tailings steam-free bricks prepared in Example 2 after curing for 3 days, 7 days, and 28 days is 15.24MPa, 21.09MPa, and 31.32MPa; the compressive strength of the iron tailings steam-free bricks prepared in Example 3 after curing for 3 days, 7 days, and 28 days is 14.91MPa, 19.28MPa, and 22.37MPa, respectively; the use of a composite activator of sodium hydroxide and sodium silicate is better than the excitation effect of a single alkali activator, because in the composite alkali activator, sodium silicate can hydrolyze to generate OH - With SiO4 4- , sodium hydroxide can also provide more OH - That is, CSH gel can be generated faster in the gelling system, which increases the bonding force between aggregates and improves the strength of tailings bricks.
[0074] Comparing the results of Example 1 and Example 2, it can be seen that with the increase of the active silicon-aluminum ratio, the compressive strength of the tailings brick is improved. This is because in the geological polymerization reaction system, Al(OH)4 - The monomer cannot exist alone for a long time and will quickly undergo polycondensation with Si(OH)4. However, the speed at which Si(OH)4 monomer polycondenses to form silicate oligomers is relatively slow. In a low silicon-aluminum ratio system, free Si(OH)4 and Al(OH)4 - The monomers combine with each other and condense in the form of hydrated ions to form long chains with low oligomer dimer morphology and low structural strength. When the active silicon-aluminum ratio is relatively high, the continuous increase in Si content increases the content of elemental silicon, and the increase in Si(OH)4 monomers promotes the formation of more Si-O-Si bonds, forming a more stable bond structure. Generally, the higher the silicon content, the higher its stability, because the chemical bond strength of the Si-O-Si bond is higher than that of the Si-O-Al and Al-O-Al bonds, and the energy required to break its Si-O-Si chemical bond is higher. As the active silicon-aluminum ratio increases, the dissolved elemental silicon content is much higher than that of aluminum. At the same time, part of the Si(OH)4 condenses to form a dimer state, and then reacts with Al(OH)4 - Reaction to form more stable long chains, which improves the strength of tailings bricks.
[0075] Comparing the results of Example 2 and Example 3, it can be seen that when the active silicon-aluminum ratio of the raw material increases from 1.79 to 2.36, the compressive strength does not increase significantly, but instead decreases sharply. The reason is that the dissolution of the reaction process has reached a saturated state in a certain alkaline environment. Continuing to increase the active silicon-aluminum ratio will inhibit the dissolution and release of the precursor in an alkaline environment, resulting in a large number of unreacted raw material particles in the tailings bricks, thereby producing agglomeration, which is not conducive to geological polymerization reaction and affects the final strength of the tailings bricks.
[0076] In summary, when the active silicon-aluminum molar ratio of the raw materials is 1.79, the 28d compressive strength of the tailings bricks produced by the present invention can reach a maximum of 31.32MPa, which can reach the MU20 level of the "Non-sintered Garbage Tailings Bricks" standard, solving the problem of low active silicon-aluminum content in iron tailings and poor mechanical properties of tailings bricks.
[0077] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. A non-burning and non-steaming tailings brick, characterized in that: The invention is prepared from solid raw materials and alkaline activators. Based on 100% by mass, the solid raw materials include: 70% to 90% iron tailings sand, 4% silica fume, and 6% to 26% bauxite; the alkaline activator is a mixture of sodium silicate accounting for 23% to 25% of the solid raw materials, 4% to 6% of sodium hydroxide, and 20% to 22% of water.
2. The unburned and unsteamed tailings brick according to claim 1, characterized in that: The alkaline activator is prepared by mixing 23% of sodium silicate, 4% of sodium hydroxide and 22% of water, which account for 23% of the solid raw materials.
3. A method for preparing a non-burning and non-steaming tailings brick as claimed in claim 1 or 2, characterized in that: The following steps are involved: S1. Determine the active silicon and aluminum content to obtain the formula of the unburned and unsteamed tailings brick; S11, determining the silicon content and aluminum content in each raw material of iron ore tailings, silica fume and bauxite; S12, dissolving the raw materials with an alkaline solution to obtain an inactive substance, and testing the silicon and aluminum content in the obtained inactive substance to obtain the content of inactive silicon and aluminum in each raw material; S13, calculating the active silicon and aluminum content in each raw material according to the initial silicon and aluminum content and the inactive silicon and aluminum content of each raw material; S14, using silica ash and bauxite as silicon source and aluminum source to adjust the active silicon-aluminum molar ratio of the raw material, the calculation formula of the active silicon-aluminum molar ratio is as follows: Then, a formula for preparing unburned and unsteamed tailings bricks is obtained; S2. Preparation of unburned and unsteamed tailings bricks: S21, weighing iron tailings sand, silica fume, and bauxite according to the obtained formula, and mixing them evenly to obtain a dry material; S22, preparing an alkali activator according to the obtained formula, and then adding the obtained alkali activator to the dry material, stirring to make the dry material and the alkali activator mix evenly, to obtain a wet mixed material; S23, placing the wet mixture in a mold, placing it on a vibrator for shaking, scraping the mold surface flat with a scraper, drying, curing and forming, demolding, and obtaining a brick; S24, curing the brick blank to obtain a steaming-free and burning-free tailings brick.
4. The method for preparing the unburned and unsteamed tailings brick according to claim 3, characterized in that: The alkali used for the alkaline dissolution is a 10 mol / L sodium hydroxide solution, the liquid-to-solid ratio of the alkaline solution to the material to be dissolved is 100:1 mL / g, and the alkaline dissolution time is 7 days.
5. The method for preparing the unburned and unsteamed tailings brick according to claim 3, characterized in that: In step S13, the active silicon and aluminum content in the alkali-soluble material is tested, including the steps of: taking the material to be tested and fully stirring it in an alkaline solution to obtain a turbid liquid, filtering it to obtain a filtrate and a filter residue, testing the inactive silicon and aluminum content in the filter residue, and subtracting the inactive silicon and aluminum content from the initial silicon and aluminum content of the raw material to obtain the active silicon and aluminum content of the raw material.
6. The method for preparing the unburned and unsteamed tailings brick according to claim 3, characterized in that: In step S22, the stirring time is 5-12 minutes.
7. The method for preparing the unburned and unsteamed tailings brick according to claim 3, characterized in that: In step S23, the drying temperature is 50-60°C; and the curing time is 24-32h.
8. The method for preparing the unburned and unsteamed tailings brick according to claim 3, characterized in that: The curing includes two stages: curing at a constant temperature of 20° C. from the 1st to the 7th day, and natural curing after 7 days until the 28th day.
Citation Information
Patent Citations
Preparation method of high-ferrosilicon tailing autoclaved brick
CN103496933A
Iron tailing sintering brick and preparation method thereof
CN109111208A
Non-autoclaved and non-fired tailing brick and preparation method thereof
CN112897955A
Non-fired and non-steamed tailing brick and preparation method thereof
CN104230243A
Method for determining effective aluminum and activated silicon in gibbsite bauxite
CN106769300A