Preparation process of waterproof anti-crack mortar of multi-element inorganic gelling system

By performing the modification reaction of phenylenediamine and montmorillonite in the mortar, the modification reaction of graphite oxide and epoxy silane coupling agent, combined with silicate cement and quartz sand, the traditional mortar is solved. Problem, efficient compressive strength and waterproofing effect are achieved, process steps are simplified and cost is reduced.

CN118993638APending Publication Date: 2024-11-22HENAN JIAFANG IND CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410920313.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-10
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

In the prior art, traditional cement mortar materials have problems such as low strength, poor bonding ability, cracking and poor waterproofing, which leads to leakage of walls, and the distribution ratio of multiple raw material groups is complicated, making it difficult to achieve efficient waterproof and crack resistance.

Method used

Using a waterproof and crack-resistant mortar process with a multi-inorganic gelling system, the phenylenediamine and montmorillonite are intercalated, graphite oxide is modified with epoxy silane coupling agent, and is also modified with silicate cement and quartz sand. , styrene acrylic emulsion mixed to form a mortar with high compressive strength and waterproofing effect.

Benefits of technology

It achieves the compressive strength and waterproofing of the mortar without adding fiber, which is cost-effective, green and non-toxic, and is easy to produce and use.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a preparation process of waterproof anti-crack mortar of a multi-element inorganic gelling system, which comprises the following steps: adding phenylenediamine and montmorillonite into a solvent for intercalation; the preparation method comprises the following steps: adding graphite oxide and an epoxy silane coupling agent into a solvent, and carrying out a modification reaction; heating and stirring the two mixed solutions for reaction; after the reaction is completed, filtering and drying; and uniformly mixing and stirring the obtained material, the Portland cement, the quartz sand and the styrene-acrylic emulsion. The mortar produced by the process has excellent waterproof and anti-cracking capabilities, is green and safe, and is easy to produce and use.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of mortar, in particular to a preparation process of waterproof and crack-resistant mortar of a multi-component inorganic gelling system. Background Art

[0002] Mortar is a bonding material used for bricklaying in buildings. It is made of a certain proportion of sand and binder (cement, lime paste, clay, etc.) and water. Ordinary mortar and concrete are not dense but permeable to water. With the development of technology, traditional cement mortar materials have gradually exposed various defects in application, such as low strength, poor bonding ability, cracking, poor waterproofness, and wall leakage. Patent 201710812761.0 discloses a high crack resistance dry-mixed waterproof mortar, which increases the crack resistance and compressive strength of the mortar by adding modified loofah fiber, ramie fiber, and bamboo charcoal fiber, and improves the waterproof performance by acrylic latex powder, EVA latex powder, and styrene-butadiene latex. Patent 201810780749.0 discloses a special structural repair mortar and preparation method, which also respectively improves the waterproof performance and crack resistance and compressive performance by styrene-butadiene emulsion and fiber. The waterproofing agent and structural reinforcement in the above two technical solutions need to use a variety of different raw materials, and the component ratio is complicated. Patent 202211017499.8 discloses an additive for improving the strength and waterproof performance of mortar and its preparation process. The waterproof ability is further improved by adding additional graphene to improve the density of the mortar. However, graphene itself is light in texture and not easily soluble in water and oil solvents. It is easy to agglomerate in the mortar system, which greatly reduces its hydrophobic ability. Therefore, it is of great practical significance to research and develop a repair mortar that has good compatibility with sandstone cement, is easy to construct, and has good bonding performance, waterproof performance and mechanical strength. Summary of the invention

[0003] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a process for preparing a waterproof and crack-resistant mortar with a multi-component inorganic gelling system, which has few process steps and does not require the addition of fibers.

[0004] The purpose of the present invention is achieved through the following technical scheme: A process for preparing waterproof and crack-resistant mortar of a multi-component inorganic gelling system is prepared according to the following steps: S1. adding phenylenediamine and montmorillonite into a solvent for intercalation; S2. adding graphite oxide and epoxy silane coupling agent into a solvent for modification reaction; S3. The mixed solution of step S1 is added to the mixed solution of step S2 and the reaction is heated and stirred; S4. After the reaction is completed, filter and dry; S5. Mix the material obtained in step S4 with silicate cement, quartz sand and styrene-acrylic emulsion and stir for 0.5h.

[0005] Preferably, the components are 32-40 parts by weight of silicate cement, 26-42 parts by weight of quartz sand, 30-50 parts by weight of styrene acrylic emulsion, 26-32 parts by weight of montmorillonite, 6-8 parts by weight of phenylenediamine, 1-2 parts by weight of graphite oxide, and 2-5 parts by weight of epoxy silane coupling agent.

[0006] Preferably, the solvent used in steps S1 and S2 is methanol or ethanol.

[0007] Preferably, the phenylenediamine is p-phenylenediamine.

[0008] Preferably, the quartz sand includes 18-22 parts with a particle size of 20-40 mesh and 8-10 parts with a particle size of 200-250 mesh.

[0009] Preferably, in step S1, the intercalation reaction is stirred at room temperature for 2-3 hours.

[0010] Preferably, in step S2, the room temperature modification reaction time is 12-14 hours.

[0011] Preferably, in step S3, the reaction temperature is raised to 90-110° C. and the reaction is stirred for 6-8 hours.

[0012] The invention has the following advantages: preferential intercalation of phenylenediamine and montmorillonite is beneficial to the stripping of montmorillonite sheets; epoxysilane coupling agent is used to modify graphite oxide, which is beneficial to improving the oil solubility of graphite oxide; amino groups on phenylenediamine and epoxy groups on silane coupling agent undergo ring-opening reaction, which not only introduces water-absorbing hydroxyl groups and improves the hanging flow property, but also makes the three-layer I-shaped structure of graphite oxide sheets, benzene rings and montmorillonite sheets; the addition of rigid structure benzene rings supports the graphite oxide sheets and montmorillonite sheets, so that the cavity formed is beneficial to the filling of gelled cement and quartz sand, and the compressive strength of mortar is improved; the strong hydrophobicity of benzene rings themselves cooperates with the fish-scale structure formed by graphite oxide sheets and montmorillonite sheets, and the superposition of the two further improves the waterproof effect of mortar.

[0013] The mortar produced by this process not only meets the compressive and crack resistance without adding fibers, but also has excellent waterproof and hydrophobic effects, is cost-effective, green and non-toxic, and easy to produce, process and use. DETAILED DESCRIPTION

[0014] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in combination with the specific embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments.

[0015] A waterproof and crack-resistant mortar of a multi-component inorganic gelling system is prepared according to the following process steps: S1. Weigh the following components by mass: 32-40 parts of ordinary Portland cement, 26-42 parts of quartz sand, 30-50 parts of styrene acrylic emulsion, 26-32 parts of montmorillonite, 6-8 parts of phenylenediamine, 1-2 parts of graphite oxide, and 2-5 parts of epoxy silane coupling agent.

[0016] S2. Add phenylenediamine and montmorillonite to the solvent and stir for intercalation reaction for 2-3h; S3. adding graphite oxide and epoxy silane coupling agent to a solvent for modification reaction for 12-14h; S4. The mixed solution of step S2 is added to the mixed solution of step S3 and the temperature is raised to 90-110°C, and the reaction is stirred for 6-8h; S5. After the reaction is completed, filter and dry; S6. Mix the material obtained in step S5 with silicate cement, quartz sand and styrene-acrylic emulsion and stir for 0.5h.

[0017] A waterproof and crack-resistant mortar of a multi-component inorganic gelling system is prepared according to the following process steps. First, the following components are weighed according to mass fractions: 32 parts of ordinary Portland cement, 18 parts of quartz sand with a particle size of 40 meshes, 8 parts of quartz sand with a particle size of 250 meshes, 30 parts of styrene-acrylic emulsion, 26 parts of montmorillonite, 6 parts of p-phenylenediamine, 1 part of graphite oxide, and 2 parts of γ-(2,3-epoxypropoxy)propyltrimethoxysilane. Then, p-phenylenediamine and montmorillonite are added to 75% ethanol and stirred for intercalation reaction for 2 hours. Then, graphite oxide and γ-(2,3-epoxypropoxy)propyltrimethoxysilane are added to 75% ethanol for modification reaction for 12 hours. Then, the above two mixed solutions are mixed again and heated to 90°C, stirred for reaction for 8 hours, filtered after the reaction is completed, and dried at 50°C. Finally, the obtained graphite-montmorillonite composite material is mixed with Portland cement, quartz sand and styrene-acrylic emulsion and stirred for 0.5 hours.

[0018] A waterproof and crack-resistant mortar of a multi-component inorganic gelling system is prepared according to the following process steps. First, the following components are weighed according to mass fractions: 40 parts of ordinary Portland cement, 22 parts of quartz sand with a particle size of 20 meshes, 10 parts of quartz sand with a particle size of 200 meshes, 50 parts of styrene-acrylic emulsion, 32 parts of montmorillonite, 8 parts of p-phenylenediamine, 2 parts of graphite oxide, and 5 parts of γ-(2,3-epoxypropoxy)propyltrimethoxysilane. Then, p-phenylenediamine and montmorillonite are added to 75% methanol and stirred for intercalation reaction for 3 hours. Then, graphite oxide and γ-(2,3-epoxypropoxy)propyltrimethoxysilane are added to 75% methanol for modification reaction for 14 hours. Then, the above two mixed solutions are mixed again and heated to 110°C, stirred for reaction for 6 hours, filtered after the reaction is completed, and dried at 50°C. Finally, the obtained graphite-montmorillonite composite material is mixed with Portland cement, quartz sand and styrene-acrylic emulsion and stirred for 0.5 hours.

[0019] A waterproof and crack-resistant mortar of a multi-component inorganic gelling system is prepared according to the following process steps. First, the following components are weighed according to mass fractions: 32 parts of ordinary Portland cement, 18 parts of quartz sand with a particle size of 40 meshes, 8 parts of quartz sand with a particle size of 250 meshes, 30 parts of styrene-acrylic emulsion, 26 parts of montmorillonite, 6 parts of o-phenylenediamine, 1 part of graphite oxide, and 2 parts of γ-(2,3-epoxypropoxy)propyltrimethoxysilane. Then, o-phenylenediamine and montmorillonite are added to 75% ethanol and stirred for intercalation reaction for 2 hours. Then, graphite oxide and γ-(2,3-epoxypropoxy)propyltrimethoxysilane are added to 75% ethanol for modification reaction for 12 hours. Then, the above two mixed solutions are mixed again and heated to 90°C, stirred for reaction for 8 hours, filtered after the reaction is completed, and dried at 50°C. Finally, the obtained graphite-montmorillonite composite material is mixed with Portland cement, quartz sand and styrene-acrylic emulsion and stirred for 0.5 hours.

[0020] A waterproof and crack-resistant mortar of a multi-component inorganic gelling system is prepared according to the following process steps. First, the following components are weighed according to mass fractions: 32 parts of ordinary Portland cement, 22 parts of quartz sand with a particle size of 40 meshes, 10 parts of quartz sand with a particle size of 200 meshes, 30 parts of styrene-acrylic emulsion, 26 parts of montmorillonite, 6 parts of p-phenylenediamine, 1 part of graphite oxide, and 2 parts of γ-(2,3-epoxypropoxy)propyltrimethoxysilane. Then, p-phenylenediamine and montmorillonite are added to 75% ethanol and stirred for intercalation reaction for 2 hours. Then, graphite oxide and γ-(2,3-epoxypropoxy)propyltrimethoxysilane are added to 75% ethanol for modification reaction for 12 hours. Then, the above two mixed solutions are mixed again and heated to 90°C, stirred for reaction for 8 hours, filtered after the reaction is completed, and dried at 50°C. Finally, the obtained graphite-montmorillonite composite material is mixed with Portland cement, quartz sand and styrene-acrylic emulsion and stirred for 0.5 hours.

[0021] Comparative Example 1 A waterproof and crack-resistant mortar of a multi-component inorganic gelling system is prepared according to the following process steps. First, the following components are weighed according to mass fractions: 32 parts of ordinary Portland cement, 18 parts of quartz sand with a particle size of 40 meshes, 8 parts of quartz sand with a particle size of 250 meshes, 30 parts of styrene-acrylic emulsion, 26 parts of montmorillonite, 1 part of graphite oxide, and 2 parts of γ-aminopropyltriethoxysilane. Then, graphite oxide and γ-aminopropyltriethoxysilane are added to 75% ethanol for modification reaction for 12 hours. After that, montmorillonite is added to the above-mentioned mixed solution and stirred for intercalation reaction for 2 hours. After the reaction is completed, it is filtered and dried at 50°C. Finally, the obtained graphite-montmorillonite composite material is mixed with Portland cement, quartz sand and styrene-acrylic emulsion and stirred for 0.5 hours.

[0022] Comparative Example 2 A waterproof and crack-resistant mortar of a multi-component inorganic gelling system is prepared according to the following process steps. First, the following components are weighed according to mass fractions: 32 parts of ordinary Portland cement, 18 parts of quartz sand with a particle size of 40 meshes, 8 parts of quartz sand with a particle size of 250 meshes, 30 parts of styrene-acrylic emulsion, 26 parts of montmorillonite, 3 parts of ethylenediamine, 1 part of graphite oxide, and 2 parts of γ-(2,3-epoxypropoxy)propyltrimethoxysilane. Then, ethylenediamine and montmorillonite are added to 75% ethanol and stirred for intercalation reaction for 2 hours. Then, graphite oxide and γ-(2,3-epoxypropoxy)propyltrimethoxysilane are added to 75% ethanol for modification reaction for 12 hours. Then, the above two mixed solutions are mixed again and heated to 90°C, stirred for reaction for 8 hours, filtered after the reaction is completed, and dried at 50°C. Finally, the obtained graphite-montmorillonite composite material is mixed with Portland cement, quartz sand and styrene-acrylic emulsion and stirred for 0.5 hours.

[0023] Comparative Example 3 A waterproof and crack-resistant mortar of a multi-component inorganic gelling system is prepared according to the following process steps. First, the following components are weighed according to mass fractions: 32 parts of ordinary Portland cement, 18 parts of quartz sand with a particle size of 40 meshes, 8 parts of quartz sand with a particle size of 250 meshes, 30 parts of styrene-acrylic emulsion, 26 parts of montmorillonite, 12 parts of 4,4-diaminobiphenyl, 1 part of graphite oxide, 2 parts of γ-(2,3-epoxypropoxy)propyltrimethoxysilane, and then 4,4-diaminobiphenyl is added. The graphite and montmorillonite were added to 75% ethanol and stirred for intercalation reaction for 5 hours. Then, graphite oxide and γ-(2,3-epoxypropoxy)propyltrimethoxysilane were added to 75% ethanol for modification reaction for 12 hours. The two mixed solutions were mixed again and heated to 150°C, stirred for reaction for 12 hours. After the reaction was completed, it was filtered and dried at 50°C. Finally, the obtained graphite-montmorillonite composite material was mixed with silicate cement, quartz sand and styrene-acrylic emulsion and stirred for 0.5 hours.

[0024] Comparative Example 4 A waterproof and crack-resistant mortar with a multi-component inorganic gelling system is prepared according to the following process steps. First, the following components are weighed according to their mass fractions: 32 parts of ordinary Portland cement, 18 parts of quartz sand with a particle size of 40 mesh, 8 parts of quartz sand with a particle size of 250 mesh, 30 parts of styrene-acrylic emulsion, 26 parts of montmorillonite, 1 part of graphite oxide, 2 parts of polypropylene fiber, and 25 parts of water. The above components are mixed and stirred for 1.5 hours.

[0025] The mortars prepared in Examples 1-4 and Comparative Examples 1-4 were tested for performance in accordance with the provisions of JC / T984-2011 "Polymer Cement Waterproof Mortar", and the test results are shown in the following table.

[0026] Group Example 1 Example 2 Example 3 Example 4 Comparative Example 1 Comparative Example 2 Comparative Example 3 Comparative Example 4 Anti-osmotic pressure 7d / MPa 1.6 1.5 1.6 1.5 1.5 1.5 1.6 1.4 Impermeability pressure 28d / MPa 2.3 2.3 2.3 2.2 2.2 2.2 2.4 2.1 Compressive strength / MPa 33.4 33.6 33.4 33.2 31.4 32.7 33.8 33.5 Bond strength 7d / MPa 1.35 1.37 1.34 1.34 1.32 1.32 1.27 1.34 Bond strength 28d / MPa 1.53 1.58 1.53 1.53 1.51 1.51 1.48 1.52 Water absorption / % 3.1 3.3 3.2 3.1 3.4 3.4 2.8 3.9 From the comparison of the compressive results of Comparative Examples 1-2, it can be seen that the early intercalation of ethylenediamine and montmorillonite is beneficial to the stripping of the montmorillonite layer structure, which is beneficial to the uniform mixing of the mortar and the improvement of the compressive capacity; from the comparison of the compressive strength and water absorption results of Examples 1-4 and Comparative Example 2, it can be seen that the addition of benzene rings not only improves the waterproof ability, but also further improves the compressive strength. It is speculated that the rigid structure of the benzene ring is beneficial to the isolation of the graphite sheet and the montmorillonite sheet, which is beneficial to the filling sandwich structure of cement and quartz sand to improve the compressive capacity; after comparing with the results of Comparative Example 3, it can be seen that the above theory is basically correct, that is, the addition of benzene rings is beneficial to improve the waterproof ability and compressive strength of the mortar, but benzidine is relatively expensive and is a first-level carcinogen, and is not easy to be used as a production building material; the compressive strength of Examples 1-4 and Comparative Example 4 is basically the same, but the water absorption of Example 1-4 is significantly lower than that of Comparative Example 4. It can be seen that the mortar of Examples 1-4 not only maintains the compressive strength of the added anti-cracking fiber, but also improves the waterproof effect.

[0027] Although the present invention has been described in detail with reference to the aforementioned embodiments, it is still possible for those skilled in the art to modify the technical solutions described in the aforementioned embodiments, or to make equivalent substitutions for some of the technical features therein. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A process for preparing waterproof and crack-resistant mortar of a multi-component inorganic gelling system, characterized in that: Prepare according to the following steps, S1. adding phenylenediamine and montmorillonite into a solvent for intercalation; S2. adding graphite oxide and epoxy silane coupling agent into a solvent for modification reaction; S3. The mixed solution of step S1 is added to the mixed solution of step S2 and the reaction is heated and stirred; S4. After the reaction is completed, filter and dry; S5. Mix the material obtained in step S4 with silicate cement, quartz sand and styrene-acrylic emulsion and stir for 0.5h.

2. The process for preparing waterproof and crack-resistant mortar of multi-component inorganic gelling system according to claim 1, characterized in that: Calculated by weight, the components are 32-40 parts of silicate cement, 26-42 parts of quartz sand, 30-50 parts of styrene acrylic emulsion, 26-32 parts of montmorillonite, 6-8 parts of phenylenediamine, 1-2 parts of graphite oxide, and 2-5 parts of epoxy silane coupling agent.

3. The process for preparing waterproof and crack-resistant mortar of multi-component inorganic gelling system according to claim 1, characterized in that: The solvent used in steps S1 and S2 is methanol or ethanol.

4. The process for preparing waterproof and crack-resistant mortar of the multi-component inorganic gelling system according to any one of claims 1 or 2, characterized in that: The phenylenediamine is selected as p-phenylenediamine.

5. The process for preparing waterproof and crack-resistant mortar of the multi-component inorganic gelling system according to any one of claims 1 or 2, characterized in that: The quartz sand includes 18-22 parts with a particle size of 20-40 mesh and 8-10 parts with a particle size of 200-250 mesh.

6. The process for preparing waterproof and crack-resistant mortar of multi-component inorganic gelling system according to claim 1, characterized in that: In step S1, the intercalation reaction is stirred at room temperature for 2-3 hours.

7. The process for preparing waterproof and crack-resistant mortar of multi-component inorganic gelling system according to claim 1, characterized in that: In step S2, the room temperature modification reaction time is 12-14 hours.