Ultra-high performance concrete and application thereof in engineering structure
By modifying metal fibers and non-metal fibers, adding micro-bead fly ash and micro-bead fume, combined with specific chemical agents, the pores and cracking problems of ultra-high performance concrete during use are solved, and the compression resistance is improved. Anti-corrosion and toughness properties improve the overall performance of concrete.
Patent Information
- Application Number
- CN202411211504.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-11-22
AI Technical Summary
Existing ultra-high performance concrete is prone to pores and cracks during use, resulting in reduced compressive strength and tensile strength, and steel fibers are prone to corrosion, affecting performance.
By modifying metal fibers and non-metal fibers, and adding micro-bead fly ash and micro-bead fume, the dispersion and stability of the fibers in the concrete system are improved, and epoxidized phenolic resin, cashew shell oil and Ferrocene acetylene coated steel fibers, nano SiO2 and silane coupling agent modified magnesium fibers, combined with tributyl citrate and silane coupling agent to form modified concrete.
It significantly improves the compressive, anti-corrosion and toughness properties of concrete, reduces the later cracking of concrete, enhances the dispersion and bonding strength of steel fibers, and improves the overall performance.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of concrete, and specifically relates to an ultra-high performance concrete and an application thereof in engineering structures. Background Art
[0002] Ultra-high performance concrete (UHPC) is a new type of cement-based composite material made of high-performance powders, minerals and chemical additives. It has good mechanical properties such as strength, durability and durability; it can be used in various construction projects, including bridges, tunnels, buildings and other building structures.
[0003] At present, ultra-high performance concrete mostly uses cement, silica fume, quartz sand and high-efficiency water reducing agent as raw materials. Although the use of these raw materials can effectively improve the mechanical strength of ultra-high performance concrete, the large-scale use of cement and quartz sand brings about the problem of high economic cost and has a great impact on the environment. Compared with ordinary cement, ultra-high performance concrete can reduce the use of large amounts of materials, reduce costs and save resources. Steel fiber is an important material for enhancing the toughness and strength of ultra-high performance concrete. In order to prevent the steel fiber from rusting, it is usually necessary to plate the steel fiber with metal to form a smooth protective layer. However, the ultra-high performance concrete made of existing steel fibers has problems such as forming pores during use and cracking in the later stage, and reduces the compressive strength and tensile strength of the concrete. Therefore, it is of great significance to develop an ultra-high performance concrete and apply it to engineering structures. Summary of the invention
[0004] The purpose of the present invention is to provide ultra-high performance concrete. By modifying metal fibers and non-metallic fibers separately and adding micro-bead fly ash and micro-bead silica fume at the same time, the dispersion and stability of the fibers in the concrete system are significantly improved, thereby obtaining concrete with excellent compression resistance, corrosion resistance, toughness and other properties.
[0005] In order to achieve the above object, the present invention provides the following technical solutions: An ultra-high performance concrete comprises the following components, measured by weight: 30-50 parts of sulphoaluminate cement, 200-300 parts of coarse aggregate, 60-80 parts of fine aggregate, 10-20 parts of modified non-metallic fiber, 8-15 parts of modified metal fiber, 1-3 parts of micro-bead fly ash, 2-6 parts of micro-bead silica fume, 10-14 parts of tributyl citrate, 3-6 parts of silane coupling agent, 2-4 parts of polycarboxylate water reducer, 1-3 parts of sodium tripolyphosphate retarder and 100-150 parts of water.
[0006] Furthermore, the coarse aggregate is crushed stone with a particle size of 12-14 mm; the fine aggregate is machine-made sand with a particle size of 3-5 mm; the modified non-metallic fiber is a resin modified product with brucite fiber as the matrix, and the length of the modified non-metallic fiber is 7-10 mm; the modified metal fiber is a resin modified product with steel fiber as the matrix, and the length of the modified metal fiber is 3-5 mm.
[0007] The method for preparing the ultra-high performance concrete comprises the following steps: S1: In parts by weight, 5-10 parts of phenolic resin and 6-15 parts of epichlorohydrin are added to a reactor and mixed evenly, reacted at a temperature of 60-80°C for 3-6h, then concentrated under reduced pressure and washed to obtain epoxidized phenolic resin; 2-5 parts of cashew nut shell oil, 0.5-1 part of ferrocene acetylene, and 0.3-0.6 parts of N,N-dimethylformamide are added thereto, reacted at a temperature of 90-110°C for 2-4h to form a mixed solution A; then, the mixed solution A is added to the steel fiber at a solid-liquid ratio of 1g:10-20ml, and stirred at a temperature of 100-120°C for 1-3h to obtain a modified metal fiber; S2: by weight, 3-6 parts of nano-SiO2, 2-4 parts of silane coupling agent, 10-30 parts of brucite fiber and 50-80 parts of water are ultrasonically treated at a temperature of 50-70° C. for 20-40 minutes to obtain modified non-metallic fiber; S3: In parts by weight, 8-15 parts of the modified metal fiber described in step S1, 10-20 parts of the modified non-metallic fiber described in step S2, 1-3 parts of micro-bead fly ash, 2-6 parts of micro-bead silica fume and 100-150 parts of water are stirred and reacted at a temperature of 40-60°C for 25-45 minutes; then 10-14 parts of tributyl citrate and 3-6 parts of silane coupling agent are added, and the mixture is reacted at a temperature of 100-120°C for 1-3 hours to obtain a mixed solution B; the mixed solution B, 30-50 parts of sulphoaluminate cement, 200-300 parts of coarse aggregate, 60-80 parts of fine aggregate, 2-4 parts of polycarboxylate water reducer and 1-3 parts of sodium tripolyphosphate retarder are added to a concrete mixer and stirred for 90-130 seconds to obtain ultra-high performance concrete.
[0008] Further, in step S1, 8 parts of phenolic resin and 12 parts of epichlorohydrin are added to the reactor by weight and mixed evenly, stirred at a temperature of 75° C. and a rate of 500 r / min for 4.5 hours, then vacuum concentrated at a pressure of -0.15 MPa for 25 minutes, and washed with deionized water 3 times to obtain epoxidized phenolic resin.
[0009] Furthermore, in step S1, 3.5 parts of cashew nut shell oil, 0.7 parts of ferrocene acetylene, and 0.45 parts of N,N-dimethylformamide are added thereto by weight, and the mixture is stirred and reacted at a rate of 600 r / min for 3 hours at a temperature of 100°C to form a mixed solution A; then, the mixed solution A is added to the steel fiber at a solid-liquid ratio of 1g:16ml, and the mixture is stirred and reacted at a rate of 450 r / min for 2 hours at a temperature of 115°C to obtain a modified metal fiber.
[0010] Furthermore, in step S2, 4 parts of nano-SiO2, 3 parts of silane coupling agent, 22 parts of brucite fiber and 65 parts of water are ultrasonically treated at a temperature of 65°C and a power of 2500W for 32 minutes to obtain modified non-metallic fiber.
[0011] Furthermore, step S3 is further optimized as follows: take 12 parts of the modified metal fiber described in step S1, 16 parts of the modified non-metallic fiber described in step S2, 2 parts of micro-bead fly ash, 4 parts of micro-bead silica fume and 130 parts of water, stir and react at a temperature of 55°C and a speed of 550r / min for 30 minutes.
[0012] Furthermore, step S3 is further optimized as follows: adding 12 parts of tributyl citrate and 5 parts of silane coupling agent, stirring and reacting at a temperature of 112° C. at a rate of 350 r / min for 2 hours to obtain a mixed solution B.
[0013] Furthermore, step S3 is further optimized as follows: adding mixed solution B, 44 parts of sulphoaluminate cement, 276 parts of coarse aggregate, 73 parts of fine aggregate, 3 parts of polycarboxylate water reducer, and 2 parts of sodium tripolyphosphate retarder into a concrete mixer and stirring for 112 seconds to obtain ultra-high performance concrete.
[0014] Any of the above applications of ultra-high performance concrete in engineering structures.
[0015] Compared with the prior art, the advantages and beneficial effects of the present invention are: 1. The present invention adopts a mixed solution of epoxidized phenolic resin, cashew nut shell oil and ferrocene acetylene to coat steel fiber, thereby improving the dispersibility, toughness and bonding strength of steel fiber in the concrete system, improving the performance of concrete, reducing the cracking phenomenon in the later stage of concrete, and effectively preventing the steel fiber from being corroded.
[0016] 2. The present invention uses nano-SiO2 and silane coupling agent to modify brucite fiber, and improves dispersant, toughness and boundary bonding by filling and attaching to the brucite fiber, so as to better prevent micro cracks from appearing inside.
[0017] 3. On the basis of the above, the present invention further introduces micro-bead fly ash and micro-bead silica fume, utilizing the characteristics of micro-beads to better fill the voids, increase the density and thus improve the impermeability; under the action of tributyl citrate and silane coupling agent, the overall performance is further improved. DETAILED DESCRIPTION
[0018] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0019] The sources of raw materials used in the present invention are as follows: Cashew nut shell liquid Sulphoaluminate cement came from Wuhan Jiyesheng Chemical Co., Ltd. with item number A00305; polycarboxylic acid water reducer came from Liaoning Kelong Fine Chemical Co., Ltd. with item number SP609; sodium tripolyphosphate retarder came from Shanghai Yuanye Biotechnology Co., Ltd. with item number S30235.
[0020] Example 1 This embodiment provides ultra-high performance concrete, and the preparation method thereof comprises the following steps: S1: 5g of phenolic resin and 6g of epichlorohydrin were added to the reactor and mixed evenly, and the mixture was stirred at a temperature of 60°C and a speed of 500r / min for 3h, and then concentrated under vacuum at a pressure of -0.15MPa for 20min, and washed with deionized water for 3 times to obtain epoxidized phenolic resin; 2g of cashew nut shell oil, 0.5g of ferroceneacetylene, and 0.3g of N,N-dimethylformamide were added thereto, and the mixture was stirred at a speed of 600r / min for 2h at a temperature of 90°C to form a mixed solution A; then, the mixed solution A was added to the steel fiber at a solid-liquid ratio of 1g:10ml, and the mixture was stirred at a speed of 450r / min for 1h at a temperature of 100°C to obtain a modified metal fiber with a length of 3-5mm; S2: 3g of nano-SiO2, 2g of silane coupling agent, 10g of brucite fiber and 50g of water were ultrasonically treated at 50°C and 2500w for 20min to obtain modified non-metallic fibers with a length of 7-10mm; S3: Take 8g of the modified metal fiber described in step S1, 10g of the modified non-metallic fiber described in step S2, 1g of micro-bead fly ash, 2g of micro-bead silica fume and 100g of water, stir and react at a temperature of 40°C at a rate of 550r / min for 25min; then add 10g of tributyl citrate and 3g of silane coupling agent, react at a temperature of 100°C at a rate of 350r / min for 1h to obtain a mixed solution B; add the mixed solution B, 30g of sulphoaluminate cement, 200g of coarse aggregate (crushed stone with a particle size of 12-14mm), 60g of fine aggregate (mechanical sand with a particle size of 3-5mm), 2g of polycarboxylate water reducer, and 1g of sodium tripolyphosphate retarder into a concrete mixer and stir at a rate of 600r / min for 90s to obtain ultra-high performance concrete.
[0021] Example 2 This embodiment provides ultra-high performance concrete, and the preparation method thereof comprises the following steps: S1: 10g of phenolic resin and 15g of epichlorohydrin were added to the reactor and mixed evenly, and the mixture was stirred at 80°C at a rate of 500r / min for 6h, and then concentrated under vacuum at a pressure of -0.15MPa for 30min, and washed with deionized water for 3 times to obtain epoxidized phenolic resin; 5g of cashew nut shell oil, 1g of ferroceneacetylene, and 0.6g of N,N-dimethylformamide were added thereto, and the mixture was stirred at 110°C at a rate of 600r / min for 4h to form a mixed solution A; then, the mixed solution A was added to the steel fiber at a solid-liquid ratio of 1g:20ml, and the mixture was stirred at 120°C at a rate of 450r / min for 3h to obtain a modified metal fiber with a length of 3-5mm; S2: 6g of nano-SiO2, 4g of silane coupling agent, 30g of brucite fiber and 80g of water were ultrasonically treated at 70°C and 2500w for 40min to obtain modified non-metallic fibers with a length of 7-10mm; S3: Take 15g of the modified metal fiber described in step S1, 20g of the modified non-metallic fiber described in step S2, 3g of micro-bead fly ash, 6g of micro-bead silica fume and 150g of water, stir and react at a temperature of 60°C at a rate of 550r / min for 45min; then add 14g of tributyl citrate and 6g of silane coupling agent, react at a temperature of 120°C at a rate of 350r / min for 3h to obtain a mixed solution B; add the mixed solution B, 50g of sulphoaluminate cement, 300g of coarse aggregate (crushed stone with a particle size of 12-14mm), 80g of fine aggregate (mechanical sand with a particle size of 3-5mm), 4g of polycarboxylate water reducer, and 3g of sodium tripolyphosphate retarder into a concrete mixer and stir at a rate of 600r / min for 130s to obtain ultra-high performance concrete.
[0022] Example 3 This embodiment provides ultra-high performance concrete, and the preparation method thereof comprises the following steps: S1: 8g of phenolic resin and 12g of epichlorohydrin were added to the reactor and mixed evenly, and the mixture was stirred at a temperature of 75°C and a speed of 500r / min for 4.5h, and then concentrated under vacuum at a pressure of -0.15MPa for 25min, and washed with deionized water for 3 times to obtain epoxidized phenolic resin; 3.5g of cashew nut shell oil, 0.7g of ferroceneacetylene, and 0.45g of N,N-dimethylformamide were added thereto, and the mixture was stirred at a temperature of 100°C and a speed of 600r / min for 3h to form a mixed solution A; then, the mixed solution A was added to the steel fiber according to a solid-liquid ratio of 1g:16ml, and the mixture was stirred at a temperature of 115°C and a speed of 450r / min for 2h to obtain a modified metal fiber with a length of 3-5mm; S2: 4g of nano-SiO2, 3g of silane coupling agent, 22g of brucite fiber and 65g of water were ultrasonically treated at 65°C and 2500w for 32min to obtain modified non-metallic fibers with a length of 7-10mm; S3: Take 12g of the modified metal fiber described in step S1, 16g of the modified non-metallic fiber described in step S2, 2g of micro-bead fly ash, 4g of micro-bead silica fume and 130g of water, stir and react at a temperature of 55°C and a rate of 550r / min for 30min; then add 12g of tributyl citrate and 5g of silane coupling agent, react at a temperature of 112°C and a rate of 350r / min for 2h to obtain a mixed solution B; add the mixed solution B, 44g of sulphoaluminate cement, 276g of coarse aggregate (crushed stone with a particle size of 12-14mm), 73g of fine aggregate (mechanical sand with a particle size of 3-5mm), 3g of polycarboxylate water reducer, and 2g of sodium tripolyphosphate retarder into a concrete mixer and stir at a rate of 600r / min for 112s to obtain ultra-high performance concrete.
[0023] Comparative Example 1 The difference between this comparative example and Example 1 is that the epoxidized phenolic resin is missing in step S1, and the other steps are the same.
[0024] Comparative Example 2 The difference between this comparative example and Example 1 is that cashew nut shell oil is missing in step S1, and the other steps are the same.
[0025] Comparative Example 3 The difference between this comparative example and Example 1 is that ferroceneacetylene is missing in step S1, and the other steps are the same.
[0026] Comparative Example 4 The difference between this comparative example and Example 1 is that step S1 is missing, that is, the metal fiber is not modified, and the metal fiber is directly used in step S3, and the other steps are the same.
[0027] Comparative Example 5 The difference between this comparative example and Example 1 is that step S3 is missing, that is, the non-metallic fiber is not modified, and the non-metallic fiber is directly used in step S3, and the other steps are the same.
[0028] Comparative Example 6 The difference between this comparative example and Example 1 is that microbead fly ash and microbead silica fume are not added in step S3, and the other steps are the same.
[0029] The ultra-high performance concrete prepared in Example 1 was used for prefabricated components. The concrete was poured into a mold at a temperature of 25°C and a relative humidity of 98%, and cured for 3 hours. The temperature was then raised to 55°C at a rate of 5°C / min and cured for 5 hours. The temperature was then lowered to 25°C at a rate of 5°C / min, and the prefabricated components were demoulded to obtain the prefabricated components. The curing was then continued until 56 days.
[0030] Performance Testing: The compressive, flexural and tensile strengths are tested in accordance with GB / T50081-2019 "Standard Test Methods for Mechanical Properties of Ordinary Concrete"; the corrosion resistance is tested in accordance with GBJ82-85 "Test Methods for Long-term Performance and Durability of Ordinary Concrete".
[0031] Table 1 Performance test results
[0032] From the above performance test results, it can be seen that Examples 1-3 have good compression resistance, flexural resistance, ultimate tensile strength and corrosion resistance, especially the comprehensive performance of Example 3 is the most outstanding.
[0033] However, the comparative example does not adopt the necessary technical solution, resulting in its performance being significantly worse than that of the embodiment in the corresponding performance test. The above experimental results further prove the importance of the technical solution defined in the present invention to its technical effect.
[0034] The above is a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. An ultra-high performance concrete, characterized in that: The invention comprises the following components in parts by weight: 30-50 parts of sulphoaluminate cement, 200-300 parts of coarse aggregate, 60-80 parts of fine aggregate, 10-20 parts of modified non-metallic fiber, 8-15 parts of modified metal fiber, 1-3 parts of microsphere fly ash, 2-6 parts of microsphere silica fume, 10-14 parts of tributyl citrate, 3-6 parts of silane coupling agent, 2-4 parts of polycarboxylate water reducer, 1-3 parts of sodium tripolyphosphate retarder and 100-150 parts of water.
2. The ultra-high performance concrete according to claim 1, characterized in that: The coarse aggregate is crushed stone with a particle size of 12-14 mm; the fine aggregate is machine-made sand with a particle size of 3-5 mm; the modified non-metallic fiber is a resin modified product with brucite fiber as the matrix, and the length of the modified non-metallic fiber is 7-10 mm; the modified metal fiber is a resin modified product with steel fiber as the matrix, and the length of the modified metal fiber is 3-5 mm.
3. A method for preparing ultra-high performance concrete, characterized in that: The steps include: S1: In parts by weight, 5-10 parts of phenolic resin and 6-15 parts of epichlorohydrin are added to a reactor and mixed evenly, reacted at a temperature of 60-80°C for 3-6h, then concentrated under reduced pressure and washed to obtain epoxidized phenolic resin; 2-5 parts of cashew nut shell oil, 0.5-1 part of ferrocene acetylene, and 0.3-0.6 parts of N,N-dimethylformamide are added thereto, reacted at a temperature of 90-110°C for 2-4h to form a mixed solution A; then, the mixed solution A is added to the steel fiber at a solid-liquid ratio of 1g:10-20ml, and stirred at a temperature of 100-120°C for 1-3h to obtain a modified metal fiber; S2: by weight, 3-6 parts of nano-SiO2, 2-4 parts of silane coupling agent, 10-30 parts of brucite fiber and 50-80 parts of water are ultrasonically treated at a temperature of 50-70° C. for 20-40 minutes to obtain modified non-metallic fiber; S3: In parts by weight, 8-15 parts of the modified metal fiber described in step S1, 10-20 parts of the modified non-metallic fiber described in step S2, 1-3 parts of micro-bead fly ash, 2-6 parts of micro-bead silica fume and 100-150 parts of water are stirred and reacted at a temperature of 40-60°C for 25-45 minutes; then 10-14 parts of tributyl citrate and 3-6 parts of silane coupling agent are added, and the mixture is reacted at a temperature of 100-120°C for 1-3 hours to obtain a mixed solution B; the mixed solution B, 30-50 parts of sulphoaluminate cement, 200-300 parts of coarse aggregate, 60-80 parts of fine aggregate, 2-4 parts of polycarboxylate water reducer and 1-3 parts of sodium tripolyphosphate retarder are added to a concrete mixer and stirred for 90-130 seconds to obtain ultra-high performance concrete.
4. The method for preparing ultra-high performance concrete according to claim 3, characterized in that: In step S1, 8 parts of phenolic resin and 12 parts of epichlorohydrin are added to a reactor by weight and mixed evenly, stirred at a temperature of 75° C. and a rate of 500 r / min for 4.5 hours, then concentrated under vacuum at a pressure of -0.15 MPa for 25 minutes, and washed with deionized water 3 times to obtain an epoxidized phenolic resin.
5. The method for preparing ultra-high performance concrete according to claim 3, characterized in that: In step S1, 3.5 parts of cashew nut shell oil, 0.7 parts of ferrocene acetylene, and 0.45 parts of N,N-dimethylformamide are added thereto by weight, and the mixture is stirred and reacted at a rate of 600r / min for 3 hours at a temperature of 100°C to form a mixed solution A; then, the mixed solution A is added to the steel fiber at a solid-liquid ratio of 1g:16ml, and the mixture is stirred and reacted at a rate of 450r / min for 2 hours at a temperature of 115°C to obtain a modified metal fiber.
6. The method for preparing ultra-high performance concrete according to claim 3, characterized in that: In step S2, 4 parts of nano-SiO2, 3 parts of silane coupling agent, 22 parts of brucite fiber and 65 parts of water are ultrasonically treated at a temperature of 65° C. and a power of 2500 W for 32 minutes to obtain modified non-metallic fiber.
7. The method for preparing ultra-high performance concrete according to claim 3, characterized in that: Step S3 is further optimized as follows: 12 parts of the modified metal fiber described in step S1, 16 parts of the modified non-metal fiber described in step S2, 2 parts of micro-bead fly ash, 4 parts of micro-bead silica fume and 130 parts of water are stirred at a temperature of 55° C. and a speed of 550 r / min for 30 minutes.
8. The method for preparing ultra-high performance concrete according to claim 3, characterized in that: Step S3 is further optimized as follows: 12 parts of tributyl citrate and 5 parts of silane coupling agent are added, and the mixture is stirred at a temperature of 112° C. and a rate of 350 r / min for 2 h to obtain a mixed solution B.
9. The method for preparing ultra-high performance concrete according to claim 3, characterized in that: Step S3 is further optimized as follows: adding mixed solution B, 44 parts of sulphoaluminate cement, 276 parts of coarse aggregate, 73 parts of fine aggregate, 3 parts of polycarboxylate water reducer, and 2 parts of sodium tripolyphosphate retarder into a concrete mixer and stirring for 112 seconds to obtain ultra-high performance concrete.
10. Use of the ultra-high performance concrete according to any one of claims 1 to 9 in engineering structures.
Citation Information
Cited By
High-strength low-shrinkage concrete based on inorganic filler and preparation method thereof
CN122482769A