Solid-waste-based lightweight roof prefabricated material and preparation method thereof
By combining solid waste-based sulfa-aluminate cement and semi-water desulfurization gypsum, prefabricated foam is prepared in combination with protein foaming agent, which solves the problems of high density, low compressive strength and high thermal conductivity of photovoltaic building roof materials, and realizes the The lightweight insulation effect of rapid mold release and high compression resistance simplifies the process and reduces the maintenance time.
Patent Information
- Application Number
- CN202411228579.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-03
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-09-03
AI Technical Summary
The existing photovoltaic building roof materials have problems such as high density, low compressive strength, low thermal resistance, high thermal conductivity and long demolding cycle, and it is difficult to achieve the requirements of rapid demolding, low thermal conductivity, lightweight and high compression resistance.
Using solid waste-based sulfhydrate aluminate cement, semi-water desulfurization gypsum, retarder, water reducing agent and prefabricated foam, a solid waste-based lightweight roof prefabricated material is prepared through specific ratios and process flows. , achieve rapid molding and demolding, and prepare prefabricated foams through protein foaming agent to improve the mechanical properties and thermal resistance of the material.
It realizes rapid mold release, low thermal conductivity and high compressive strength of the material, meets the improvement of lightweight insulation effect of photovoltaic building roofs, while maintaining mechanical properties, simplifying processes and reducing maintenance time.
Smart Images

Figure CN118993683A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of building thermal insulation materials and photovoltaic roofing, and specifically relates to a solid waste-based lightweight roofing prefabricated material and a preparation method thereof. Background Art
[0002] The statements herein merely provide background information related to the present invention and do not necessarily constitute prior art.
[0003] At present, building roofs generally use cement as the main cementitious material, and are prepared and formed by adding lightweight mineral admixtures such as kaolin and fly ash, as well as admixtures and modifiers, and introducing gas at the same time. Photovoltaic building roofing materials mainly focus on parameters such as density, compressive strength, thermal conductivity, and water resistance. However, under conventional preparation processes, photovoltaic building roofing materials have problems such as high density, low compressive strength, low thermal resistance and high thermal conductivity, and long demolding and curing cycle. It is difficult to meet the mechanical strength requirements after using lightweight materials and introducing gas, and it usually takes 1-2 days to demold, and curing for 28 days or more to meet the factory requirements. In addition, the strength will also be affected when the material density is low through foaming, and low density will inevitably lead to low compressive strength. Therefore, to achieve better lightweight insulation effect of photovoltaic building roofs, it is necessary to do so without sacrificing mechanical strength.
[0004] Photovoltaic building roofs are advantageous for high thermal resistance, low thermal conductivity, high compressive strength and low density. When building roofs are prepared with a variety of lightweight mineral admixtures and the introduction of gas, although low density is achieved, the mechanical strength is reduced and the setting time is long, making it difficult to achieve rapid demoulding, and the maintenance process is complicated and strict. Therefore, the existing technology cannot achieve rapid demoulding, on-site prefabrication, low thermal conductivity, light weight and high compressive strength requirements for photovoltaic building roofs. Summary of the invention
[0005] In view of the deficiencies in the prior art, an object of the present invention is to provide a solid waste-based lightweight roofing prefabricated material and a preparation method thereof.
[0006] In order to achieve the above object, the present invention is implemented through the following technical solutions:
[0007] In a first aspect, the present invention provides a solid waste-based lightweight prefabricated roofing material, which is composed of the following components, by weight: 30-60 parts of solid waste-based sulphoaluminate cement, 40-70 parts of semi-hydrated desulfurized gypsum, 0.2-0.4 parts of retarder, 0.02-0.2 parts of water reducer, 0-0.2 parts of gypsum retarder, and 5-15 parts of prefabricated foam; the water-cement ratio is 0.2-0.4.
[0008] The solid waste-based sulphoaluminate cement described in the present invention is produced by using solid waste as raw material, aiming at improving the utilization rate of solid waste.
[0009] Semi-hydrated desulfurized gypsum sets quickly in the early stage and has stable performance, which is conducive to rapid demoulding in the later stage.
[0010] The present invention uses a large amount of semi-hydrated gypsum, and the gypsum sets quickly in the early stage, so the effect of using a targeted gypsum retarder is better; adding the retarder has a retarding effect on other components.
[0011] In some embodiments, the solid waste-based lightweight roofing prefabricated material is composed of the following components, by weight: 30-50 parts of solid waste-based sulphoaluminate cement, 40-70 parts of semi-hydrated desulfurized gypsum, 0.2-0.4 parts of retarder, 0.1-0.2 parts of water reducer, 0.1-0.2 parts of gypsum retarder, and 5-15 parts of prefabricated foam; the water-cement ratio is 0.2-0.4.
[0012] In some embodiments, the prefabricated foam is prepared from a protein foaming agent and water in a mass ratio of 1:20-40.
[0013] Protein foaming agent is made of animal (such as cattle and sheep) keratin as the main raw material, adding a certain amount of sodium hydroxide, magnesium chloride, hydrochloric acid and other chemical raw materials, through heating dissolution, dilution, filtration, high temperature dehydration and other processes. It is generally a dark brown viscous liquid with the advantages of high foaming multiple, high strength, good stability and low cost.
[0014] In some embodiments, the retarder is boric acid or tartaric acid.
[0015] In some embodiments, the gypsum retarder is an amino acid gypsum retarder.
[0016] In some embodiments, the water reducer is a polycarboxylate water reducer or a naphthalene water reducer.
[0017] In some embodiments, the solid waste-based lightweight roofing prefabricated material also includes a foam stabilizer, the foam stabilizer is calcium stearate, and the mass fraction of the foam stabilizer is 0.2-0.6 parts.
[0018] In a second aspect, the present invention provides a method for preparing the solid waste-based lightweight roofing prefabricated material, comprising the following steps:
[0019] The solid waste-based sulphoaluminate cement, hemihydrate gypsum, retarder, water reducing agent and gypsum retarder are mixed in proportion to prepare a composite material;
[0020] According to the water-cement ratio, water and compound materials are mixed to obtain slurry;
[0021] Prefabricated foam is prepared by mixing a protein foaming agent with water at a ratio of 1:20-40;
[0022] The prepared prefabricated foam is mixed with the slurry in proportion, poured, formed, demoulded and cured to obtain the lightweight prefabricated roofing material.
[0023] In some embodiments, the forming is natural forming, and the forming time is 4-6 hours.
[0024] In some embodiments, the curing time is 20-30 days.
[0025] The beneficial effects achieved by one or more embodiments of the present invention are as follows:
[0026] The synergistic effect of solid waste-based sulphoaluminate cement and hemihydrate gypsum can significantly improve the mechanical properties in the short term and meet the demand for lightweight. At the same time, the early strength and fast hardening characteristics can achieve rapid molding and demoulding (4-6h); the density is significantly reduced after physical foaming, and the strength can still meet the standard limit, and the thermal insulation effect of the high thermal resistance environment is improved. Therefore, it can better meet the requirements of rapid demoulding, on-site prefabrication, low thermal conductivity, light weight and high pressure resistance of photovoltaic building roofs. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] The accompanying drawings in the specification, which constitute a part of the present invention, are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute improper limitations on the present invention.
[0028] Figure 1 It is a process flow chart of an embodiment of the present invention. DETAILED DESCRIPTION
[0029] It should be noted that the following detailed descriptions are illustrative and intended to provide further explanation of the present invention. Unless otherwise specified, all technical and scientific terms used in the present invention have the same meanings as those commonly understood by those skilled in the art to which the present invention belongs.
[0030] The present invention will be further described below in conjunction with the embodiments.
[0031] Example 1
[0032] A prefabricated material for a lightweight roof for photovoltaics, consisting of the following components, measured by mass: 40 parts of solid waste-based sulphoaluminate cement, 60 parts of semi-hydrated desulfurized gypsum, 0.2 parts of a retarder, 0.04 parts of a water reducing agent, 0.2 parts of a gypsum retarder, 0.4 parts of a foam stabilizer, and 10 parts of prefabricated foam.
[0033] The water reducer is a polycarboxylate water reducer, the foam stabilizer is calcium stearate, and the water meets the requirements for concrete mixing water.
[0034] A method for preparing a prefabricated material for a photovoltaic lightweight roof comprises the following steps:
[0035] (1) 40 parts of solid waste-based sulphoaluminate cement and 60 parts of hemihydrate gypsum are fully premixed and stirred for later use;
[0036] (2) adding 0.2 parts of retarder, 0.04 parts of water reducing agent and 0.2 parts of gypsum retarder to the raw materials prepared in step (1), stirring and mixing for 2 minutes to prepare a composite material for use;
[0037] (3) Take 20 parts of tap water, pour it into the premix prepared in step (2) at one time, and stir rapidly for 180 seconds;
[0038] (4) preparing fresh prefabricated foam using a physical foaming agent in a ratio of 1:40 between a protein foaming agent and water;
[0039] (5) The prefabricated foam prepared in step (4) is mixed with the slurry prepared in step (3), stirred and mixed, and then the mixed slurry is poured into a mold, naturally formed for 6 hours, demolded (the demolding can be completely achieved within 6 hours), and cured for 28 days under standard curing conditions (temperature of 20°C ± 2°C, humidity of 95% standard curing), thereby obtaining a lightweight photovoltaic roof prefabricated material.
[0040] Comparative Example 1
[0041] Material composition: 32 parts of desulfurized gypsum, 16 parts of red mud, 24 parts of aluminum ash, and 28 parts of calcium carbide slag.
[0042] Preparation method: Physical foaming of air and mixing with slurry to prepare foamed concrete.
[0043] The complete demoulding time is 24h.
[0044] Comparative Example 2
[0045] The semi-hydrated gypsum in Example 1 was replaced with desulfurized gypsum. The other conditions were the same as those in Example 1. Complete demoulding could be achieved in 12 hours.
[0046] Comparative Example 3
[0047] The semi-hydrated gypsum in Example 1 was replaced with solid waste-based sulphoaluminate cement. The rest was the same as in Example 1. Complete demoulding could be achieved in 8 hours.
[0048] Comparative Example 4
[0049] The solid waste-based sulphoaluminate cement in Example 1 was replaced with silicate cement. The rest was the same as in Example 1, and complete demoulding could be achieved within 24 hours.
[0050] Table 1 Relevant properties of photovoltaic lightweight roofing materials of Example 1 and Comparative Example
[0051]
[0052]
[0053] Example 2
[0054] A prefabricated material for a lightweight roof for photovoltaics, composed of the following components, measured by mass: 40 parts of solid waste-based sulphoaluminate cement, 60 parts of semi-hydrated desulfurized gypsum, 0.2 parts of a retarder, 0.04 parts of a water reducing agent, 0.2 parts of a gypsum retarder, 0.6 parts of a foam stabilizer, and 15 parts of prefabricated foam.
[0055] The water reducer is a polycarboxylate water reducer, the foam stabilizer is calcium stearate, and the water meets the requirements for concrete mixing water.
[0056] A prefabricated material for a photovoltaic lightweight roof and a preparation method thereof, the method comprising the following steps:
[0057] (1) 40 parts of solid waste-based sulphoaluminate cement and 60 parts of hemihydrate gypsum are fully premixed and stirred for later use;
[0058] (2) adding 0.2 parts of retarder, 0.04 parts of water reducing agent and 0.2 parts of gypsum retarder to the raw materials prepared in step (1), stirring and mixing for 2 minutes to prepare a composite material for use;
[0059] (3) Take 20 parts of tap water, pour it into the premix prepared in step (2) at one time, and stir rapidly for 120 seconds;
[0060] (4) preparing fresh prefabricated foam using a physical foaming agent in a ratio of 1:30 by mass of a protein foaming agent to water;
[0061] (5) The prefabricated foam prepared in step (4) is mixed with the slurry prepared in step (3), stirred and mixed, and then the mixed slurry is poured into a mold, naturally formed for 4 hours, demolded (complete demolding can be achieved in 4 hours), and cured under standard curing conditions for 28 days to obtain a lightweight photovoltaic roof prefabricated material.
[0062] Table 2 Performance data of photovoltaic lightweight roofing materials in Example 2
[0063]
[0064] Example 3
[0065] A prefabricated material for a lightweight roof for photovoltaics, consisting of the following components, measured by mass: 30 parts of solid waste-based sulphoaluminate cement, 60 parts of semi-hydrated desulfurized gypsum, 0.2 parts of a retarder, 0.04 parts of a water reducing agent, 0.2 parts of a gypsum retarder, 0.3 parts of a foam stabilizer, and 5 parts of prefabricated foam.
[0066] The water reducer is a polycarboxylate water reducer, the foam stabilizer is calcium stearate, the foam stabilizer is hydroxypropyl methylcellulose ether, and the water meets the requirements for concrete mixing water.
[0067] A prefabricated material for a photovoltaic lightweight roof and a preparation method thereof, the method comprising the following steps:
[0068] (1) 30 parts of solid waste-based sulphoaluminate cement and 70 parts of hemihydrate gypsum are fully premixed and stirred for later use;
[0069] (2) The raw material prepared in (1) is further mixed with 0.2 parts of retarder, 0.04 parts of water reducing agent, and 0.2 parts of gypsum retarder, and stirred for 2 minutes to prepare a composite material for use;
[0070] (3) Take 30 parts of tap water, pour it into the composite material of step (2) at one time, and stir rapidly for 160 seconds;
[0071] (4) preparing fresh prefabricated foam using a physical foaming agent in a ratio of 1:30 by mass of a protein foaming agent to water;
[0072] (5) The prefabricated foam prepared in step (4) is mixed with the slurry prepared in step (3), and after stirring evenly, the mixed slurry is poured into a mold, naturally formed for 5 hours, demolded, and cured under standard curing conditions for 28 days to obtain a lightweight photovoltaic roof prefabricated material.
[0073] Table 3 Performance comparison of photovoltaic lightweight roofing materials in Example 3
[0074]
[0075] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A solid waste-based lightweight prefabricated roofing material, Features: The invention is composed of the following components by weight: 30-60 parts of solid waste-based sulphoaluminate cement, 40-70 parts of semi-hydrated desulfurized gypsum, 0.2-0.4 parts of retarder, 0.02-0.2 parts of water reducing agent, 0-0.2 parts of gypsum retarder and 5-15 parts of prefabricated foam; the water-cement ratio is 0.2-0.
4.
2. The solid waste-based lightweight roofing prefabricated material according to claim 1, Features: The invention is composed of the following components by weight: 30-50 parts of solid waste-based sulphoaluminate cement, 40-70 parts of semi-hydrated desulfurized gypsum, 0.2-0.4 parts of retarder, 0.1-0.2 parts of water reducing agent, 0.1-0.2 parts of gypsum retarder and 5-15 parts of prefabricated foam; the water-cement ratio is 0.2-0.
4.
3. The solid waste-based lightweight roofing prefabricated material according to claim 1, Features: The prefabricated foam is prepared from a protein foaming agent and water in a mass ratio of 1:20-40.
4. The solid waste-based lightweight roofing prefabricated material according to claim 1, Features: The retarder is boric acid or tartaric acid.
5. The solid waste-based lightweight roofing prefabricated material according to claim 1, Features: The gypsum retarder is an amino acid gypsum retarder.
6. The solid waste-based lightweight prefabricated roofing material according to claim 1, Features: The water reducer is a polycarboxylate water reducer or a naphthalene water reducer.
7. The solid waste-based lightweight roofing prefabricated material according to claim 1, Features: The solid waste-based lightweight roof prefabricated material also includes a foam stabilizer, which is calcium stearate, and the mass fraction of the foam stabilizer is 0.2-0.6 parts.
8. The method for preparing the solid waste-based lightweight prefabricated roofing material according to any one of claims 1 to 7, Features: The steps include: The solid waste-based sulphoaluminate cement, hemihydrate gypsum, retarder, water reducing agent and gypsum retarder are mixed in proportion to prepare a composite material; According to the water-cement ratio, water and compound materials are mixed to obtain slurry; Prefabricated foam is prepared by mixing a protein foaming agent with water at a ratio of 1:20-40; The prepared prefabricated foam is mixed with the slurry in proportion, poured, formed, demoulded and cured to obtain the lightweight prefabricated roofing material.
9. The method for preparing the solid waste-based lightweight roofing prefabricated material according to claim 8, Features: The forming is natural forming, and the forming time is 4-6 hours.
10. The method for preparing the solid waste-based lightweight prefabricated roofing material according to claim 8, Features: The curing time is 20-30 days.
Citation Information
Patent Citations
Foamed desulfurized building gypsum based slurry and prefabricated lightweight composite partition wall board thereof
CN107298456A
Gypsum-based foam concrete with large mixing amount of phosphogypsum and preparation method thereof
CN112062529A
Desulfurized gypsum-based foam concrete as well as preparation method and application thereof
CN112624795A
Steam-curing-free high-strength aerated concrete material and preparation method of aerated concrete
CN113185318A
Etringite-based energy storage foam light soil as well as preparation method and application thereof
CN114804790A
Cited By
Composite material for solid-waste-based quick-setting anti-cracking truss laminated slab, laminated slab and preparation method of composite material for solid-waste-based quick-setting anti-cracking truss laminated slab