Soybean crude enzyme induced calcium phosphate curing agent as well as preparation method and use method thereof
Through the preparation and application of soybean crude enzyme-induced calcium phosphate curing agent, the problems of low ammonia emissions and bone resource utilization in microbial/enzyme-induced calcium carbonate deposition technology are solved, and environmentally friendly and healthy soil treatment is achieved, suitable for civil and water conservancy projects. foundation reinforcement and slope protection in the middle.
Patent Information
- Application Number
- CN202411065378.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-05
- Publication Date
- 2024-11-22
AI Technical Summary
The existing microbial/enzyme-induced calcium carbonate deposition technology has problems such as excessive ammonia emissions and low bone resource utilization in civil water conservancy projects, which affects environmental protection and efficient utilization of resources.
The preparation method of soy crude enzyme-induced calcium phosphate curing agent is adopted. By mixing soy crude enzyme with urea and bovine bone calcium phosphate solution, it forms a cementitious solution, which is used to fill the pores inside the sand sample, cement and wrap sand particles, and reduce ammonia. The air is released.
It significantly reduces the ammonia release, improves the biocompatibility and mechanical properties of the curing agent, and provides an environmentally friendly and healthy method of bone waste utilization, suitable for foundation reinforcement, slope erosion protection, wind and sand control and other fields.
Smart Images

Figure CN118993688A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the fields of civil water conservancy engineering foundation reinforcement, and in particular to a soybean crude enzyme-induced calcium phosphate curing agent and a preparation method and a use method thereof. Background Art
[0002] With the development of society, people's demand for construction land is increasing. How to use poor land containing sand to meet the construction needs of engineering or civil buildings has become a highly concerned issue. In recent years, MICP (Microbial Induced Calcite Precipitation) / EICP (Enzyme Induced Calcite Precipitation) technology has been a hot research topic in the fields of foundation reinforcement, slope erosion protection, windbreak and sand control. However, during the implementation of this technology, the soil pH will be greatly increased to about 9, making the soil too alkaline, and this process is accompanied by the release of a large amount of ammonia, which is not conducive to environmental protection.
[0003] my country produces about 2,000 tons of various types of livestock bones each year. Animal bones are cheap and inconvenient to store, and are often processed into products with low added value or made into feed, resulting in great waste. Animal bones are rich in calcium phosphate, and the solubility of calcium phosphate is easily affected by the pH of the environment. Calcium phosphate has a high solubility in an acidic environment. As the pH increases, the solubility of calcium phosphate decreases and forms a precipitate. Compared with enzyme-induced calcium carbonate deposition technology, the deposition of calcium phosphate usually requires a lower pH range (2.5-8), which can significantly reduce ammonia emissions. Bone waste has great application potential in related technical fields such as foundation reinforcement of civil water conservancy projects, slope erosion protection of soil and water conservation projects, and windbreak and sand control of ecological and environmental projects.
[0004] Therefore, there is an urgent need to find a soil treatment technology that can not only efficiently utilize bone waste but also be beneficial to environmental protection, so as to be applied in the fields of foundation reinforcement, slope erosion protection, wind and sand control, etc. Summary of the invention
[0005] In order to solve the above-mentioned technical problems existing in the prior art, the present invention provides a soybean crude enzyme-induced calcium phosphate solidifying agent and a preparation method and a use method thereof, so as to overcome the problems of excessive ammonia emission, being unfavorable to environmental protection and low bone resource utilization in the prior art of microbial / enzyme-induced calcium carbonate deposition.
[0006] In order to achieve the above object, the technical solution of the embodiment of the present invention is:
[0007] The first aspect of the present invention provides a method for preparing a soybean crude enzyme-induced calcium phosphate solidifying agent, comprising:
[0008] preparing a crude soybean enzyme solution, wherein the concentration of the crude soybean enzyme solution is 100 g / L;
[0009] Using discarded cattle bones to prepare a bovine bone calcium phosphate solution, wherein the concentration of the bovine bone calcium phosphate solution is 250 g / L;
[0010] After uniformly mixing urea with the bovine bone calcium phosphate solution, a cementing liquid is obtained;
[0011] The crude soybean enzyme solution and the cementing liquid are uniformly mixed to obtain the crude soybean enzyme-induced calcium phosphate curing agent.
[0012] In combination with the first aspect, preferably, the preparation of the crude soybean enzyme solution comprises:
[0013] The soybeans are placed in an oven and baked at 40° C. for 6 to 8 hours, dried and ground into powder, added into water to form a suspension, shaken, centrifuged and filtered to obtain the soybean crude enzyme solution.
[0014] In combination with the first aspect, preferably, the preparation of the bovine bone calcium phosphate solution comprises:
[0015] The discarded bovine bones are placed in an oven and baked at 40-60° C. for 24 hours, dried and ground into bone powder, added into 0.5 mol / L hydrochloric acid to form a suspension, shaken, centrifuged and filtered to obtain the bovine bone calcium phosphate solution.
[0016] In combination with the first aspect, preferably, when the urea and the bovine bone calcium phosphate solution are uniformly mixed, the concentration of the urea is 0.1-0.2 mol / L.
[0017] In combination with the first aspect, preferably, when the urea and the bovine bone calcium phosphate solution are uniformly mixed, the molar ratio of the urea to the bovine bone calcium phosphate solution is 2 to 4:5.
[0018] In combination with the first aspect, preferably, when the crude soybean enzyme solution and the binding liquid are uniformly mixed, the volume ratio of the crude soybean enzyme solution to the binding liquid is 1 to 2.5:5.
[0019] The second aspect of the present invention provides a soybean crude enzyme-induced calcium phosphate solidifying agent prepared by the method described in the first aspect.
[0020] The third aspect of the present invention provides a method for using the soybean crude enzyme-induced calcium phosphate solidifying agent according to the second aspect, wherein the soybean crude enzyme-induced calcium phosphate solidifying agent comprises a soybean crude enzyme solution and a cementing liquid, including:
[0021] Preparation of sand sample: A PVC pipe is used as a mold to prepare a sand sample, wherein the inner diameter of the PVC pipe is 40 mm and the height is 78 mm; 167 g of ISO standard sand sample is weighed and added into the PVC pipe, and a piece of geotextile is placed on the top and bottom of the sand sample to prevent the loss of sand particles;
[0022] The crude soybean enzyme solution and the binder are added into the sand sample by grouting or spraying to obtain a solidified sand sample.
[0023] In combination with the third aspect, preferably, the grouting method comprises:
[0024] Adding 4-10 mL of the crude soybean enzyme solution into the sand sample at a rate of 5 mL / min;
[0025] After the soybean crude enzyme solution grouting is completed, 20 mL of the cementing liquid is added to the sand sample at a rate of 5 mL / min;
[0026] After the soybean crude enzyme solution and the cementing liquid are grouted in sequence, the grouting is allowed to stand for 24 hours, and the soybean crude enzyme solution and the cementing liquid are grouted in a cycle for 6 to 14 times to obtain the solidified sand sample.
[0027] In combination with the third aspect, preferably, the spraying method comprises:
[0028] Spray 4-10 mL of the crude soybean enzyme solution on the surface of the sand sample;
[0029] After the soybean crude enzyme solution is sprayed, 20 mL of the binder is sprayed on the surface of the sand sample;
[0030] After spraying the crude soybean enzyme solution and the binder solution in sequence, the mixture is allowed to stand for 24 hours, and the crude soybean enzyme solution and the binder solution are sprayed repeatedly for 6 to 14 times to obtain the solidified sand sample.
[0031] Compared with the prior art, the advantages or beneficial effects of the embodiments of the present invention include at least:
[0032] The preparation method provided by the embodiment of the present invention is to prepare a soybean crude enzyme solution by soybeans, and to prepare a calcium phosphate solution by using discarded cattle bones, and to obtain a cementing liquid after mixing urea and cattle bone calcium phosphate solution evenly; and to obtain a soybean crude enzyme-induced calcium phosphate curing agent after mixing the soybean crude enzyme solution and the cementing liquid evenly. In this way, on the one hand, calcium phosphate can effectively fill the pores inside the sand sample to achieve cementation and wrapping of adjacent sand particles, and has a significant curing effect on sand, and has broad application prospects in foundation reinforcement, slope erosion protection, windbreak and sand control, etc.; on the other hand, in view of the problems of excessive alkalinity and excessive ammonia release in enzymatic calcium carbonate deposition technology, the soybean crude enzyme-induced calcium phosphate precipitation technology can greatly reduce ammonia release, which is more environmentally friendly and healthy. The present invention provides a new idea for the rational use of bone waste. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 The crude soybean enzyme solution prepared by the present invention;
[0034] Figure 2 The bovine bone calcium phosphate solution prepared by the present invention;
[0035] Figure 3 A schematic diagram of a grouting device used for curing sand samples of the present invention;
[0036] Figure 4 The sand column obtained after solidification of the present invention;
[0037] Figure 5 It is a bar graph of the unconfined compressive strength of calcium phosphate-solidified sand induced by soybean crude enzyme under different pH binders, soybean crude enzyme solution amounts and urea concentrations;
[0038] Figure 6 It is a bar graph of calcium phosphate content in calcium phosphate-solidified sand induced by soybean crude enzyme under different pH cementing solutions, soybean crude enzyme solution amounts and urea concentrations;
[0039] Figure 7 The graph is the relationship between the calcium ion concentration and pH in the mixture of the cementing liquid and the soybean crude enzyme solution;
[0040] Figure 8 This is a graph of calcium phosphate precipitation generated in the mixed solution;
[0041] Fig. 9 This is a scanning electron microscope image of the bovine bone calcium phosphate precipitate prepared by the present invention;
[0042] Fig.10 For the corresponding Fig. 9 Energy spectrum analysis diagram of precipitation in the middle;
[0043] Fig.11 It is the percentage graph of ammonia release at different pH;
[0044] Fig.12 This is a scanning electron microscope image of calcium phosphate-solidified sand in Example 2 when the initial binder pH is 3, the amount of soybean crude enzyme solution is 4 mL, and the urea concentration is 0.15 M;
[0045] Fig.13 For the corresponding Fig.12 The scanning electron microscope image of area a in the middle is an enlarged image of area a;
[0046] Fig.14 For the corresponding Fig.13 Energy spectrum analysis diagram of the precipitation. DETAILED DESCRIPTION
[0047] In order to make the purpose, technical solutions and advantages of the present invention clearer, the present invention will be further described in detail below in conjunction with the accompanying drawings. The described embodiments should not be regarded as limiting the present invention. All other embodiments obtained by ordinary technicians in the field without making creative work are within the scope of protection of the present invention.
[0048] In the following description, reference is made to "some embodiments", which describe a subset of all possible embodiments, but it is understood that "some embodiments" may be the same subset or different subsets of all possible embodiments, and may be combined with each other without conflict. Unless otherwise defined, all technical and scientific terms used in the embodiments of the present invention have the same meaning as those commonly understood by those skilled in the art to which the embodiments of the present invention pertain. The terms used in the embodiments of the present invention are only for the purpose of describing the embodiments of the present invention and are not intended to limit the present invention.
[0049] In the following description of this embodiment, the terms "include", "comprising", "having" and "containing" are all open terms, meaning including but not limited to.
[0050] It should be noted that all raw materials / reagents in the embodiments of the present invention can be purchased on the market or prepared according to conventional methods well known to those skilled in the art; the term "and / or" in the embodiments of the present invention is only used to describe the association relationship between associated objects, indicating that three relationships may exist, for example, A and / or B means the existence of A alone, B alone, and A and B at the same time, wherein A and B can be singular or plural, and the character " / " generally indicates that the associated objects before and after are in an "or" relationship.
[0051] In the following description of this embodiment, the term "at least one" refers to one or more, and "plurality" refers to two or more. "At least one of the following" or similar expressions refers to any combination of these items, including any combination of single items or plural items. For example, "at least one of a, b or c", or "at least one of a, b and c", can all represent: a, b, c, ab (i.e., a and b), ac, bc, or abc, where a, b, c can be single or multiple, respectively.
[0052] Those skilled in the art should understand that in the following description of the embodiments of the present invention, the order of serial numbers does not mean the order of execution, some or all of the steps can be executed in parallel or sequentially, and the execution order of each process should be determined by its function and internal logic, and should not constitute any limitation on the implementation process of the embodiments of the present invention.
[0053] The terms used in the embodiments of the present invention are only for the purpose of describing specific embodiments, and are not intended to limit the present invention. The singular forms "a", "an" and "the" used in the embodiments of the present invention and the appended claims are also intended to include plural forms, unless the context clearly indicates other meanings.
[0054] It will be appreciated by those skilled in the art that the numerical ranges in the embodiments of the present invention are to be understood as also specifically disclosing each intermediate value between the upper and lower limits of the range. Each smaller range between the intermediate values in any stated value and stated range and any other stated value or intermediate value in the range is also included in the present invention. The upper and lower limits of these smaller ranges may be independently included or excluded in the range.
[0055] Unless otherwise specified, the technical / scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention only describes preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the embodiments or test cases of the present invention. All documents mentioned in this specification are generally incorporated by reference to disclose and describe methods and / or materials related to the documents. In the event of a conflict with any incorporated document, the content of the present invention shall prevail.
[0056] It should be noted that all raw materials and / or reagents in the examples of the present invention are purchased on the market or prepared according to conventional methods well known to those skilled in the art.
[0057] In view of the fact that MICP / EICP technology has excessive ammonia emissions in the field of foundation treatment and that waste bone resources in my country cannot be properly disposed of, in a first aspect, an embodiment of the present invention provides a method for preparing a soybean crude enzyme-induced calcium phosphate curing agent, the preparation method comprising:
[0058] preparing a crude soybean enzyme solution, wherein the concentration of the crude soybean enzyme solution is 100 g / L;
[0059] Using discarded cattle bones to prepare a bovine bone calcium phosphate solution, wherein the concentration of the bovine bone calcium phosphate solution is 250 g / L;
[0060] After uniformly mixing urea with the bovine bone calcium phosphate solution, a cementing liquid is obtained;
[0061] The crude soybean enzyme solution and the cementing liquid are uniformly mixed to obtain the crude soybean enzyme-induced calcium phosphate curing agent.
[0062] The preparation method provided by the embodiment of the present invention is to prepare a soybean crude enzyme solution by soybeans, and to prepare a calcium phosphate solution by using discarded cattle bones, and to obtain a cementing liquid after mixing urea and cattle bone calcium phosphate solution evenly; and to obtain a soybean crude enzyme-induced calcium phosphate curing agent after mixing the soybean crude enzyme solution and the cementing liquid evenly. In this way, on the one hand, calcium phosphate can effectively fill the pores inside the sand sample to achieve cementation and wrapping of adjacent sand particles, and has a significant curing effect on sand, and has broad application prospects in foundation reinforcement, slope erosion protection, windbreak and sand control, etc.; on the other hand, in view of the problems of excessive alkalinity and excessive ammonia release in enzymatic calcium carbonate deposition technology, the soybean crude enzyme-induced calcium phosphate precipitation technology can greatly reduce ammonia release, which is more environmentally friendly and healthy. The present invention provides a new idea for the rational use of bone waste.
[0063] In a specific embodiment, the crude soybean enzyme solution is prepared in the embodiment of the present invention by placing soybeans in an oven and baking them at 40° C. for 6 to 8 hours, drying them, grinding them into powder, adding them into water to form a suspension, shaking, centrifuging, and filtering to obtain the crude soybean enzyme solution.
[0064] Among them, the crude soybean enzyme solution plays a role in promoting biodegradation and catalysis, improving the biocompatibility of the curing agent, and the synergistic effect between the crude soybean enzyme and bovine bone calcium phosphate.
[0065] In a specific embodiment, the bovine bone calcium phosphate solution is prepared in the embodiment of the present invention by placing the discarded bovine bones in an oven and baking them at 40-60° C. for 24 hours, grinding them into bone powder after drying, adding them to 0.5 mol / L hydrochloric acid to form a suspension, oscillating, centrifuging, and filtering to obtain the bovine bone calcium phosphate solution.
[0066] Among them, bovine bone calcium phosphate solution provides an inorganic skeleton similar to bones, which provides strength and stability for the curing agent, and also improves the mechanical properties of the curing agent such as compressive strength and tensile strength; at the same time, soybean crude enzyme can catalyze the hydrolysis of urea, increase the pH of the curing agent, and then promote the recrystallization process of bovine bone calcium phosphate, thereby forming a denser and more uniform cured structure.
[0067] It should be noted that the embodiments of the present invention do not specifically limit the types of discarded cattle bones.
[0068] In a specific embodiment, when urea and bovine bone calcium phosphate solution are uniformly mixed in the embodiment of the present invention, the concentration of urea is preferably 0.1-0.2 mol / L.
[0069] Among them, when the concentration of the urea solution is less than 0.1 mol / L, the precipitation rate of calcium phosphate in the curing agent will be too slow, which is not conducive to the cementation of the sand; when the concentration of the urea solution is greater than 0.2 mol / L, the precipitation rate of calcium phosphate in the curing agent will be too fast, so that the calcium phosphate precipitation is mainly generated at the top of the sand sample, which hinders the downward penetration of the curing agent, resulting in uneven distribution of calcium phosphate precipitation and poor curing effect.
[0070] In a specific embodiment, when urine and bovine bone calcium phosphate solution are uniformly mixed in the embodiment of the present invention, the molar ratio of urea to bovine bone calcium phosphate solution is preferably 2 to 4:5.
[0071] Among them, when the molar ratio of urea to calcium ions in bovine bone calcium phosphate solution is less than 2:5, the precipitation rate of calcium phosphate in the curing agent will be too slow, which is not conducive to the cementation of sand; when the molar ratio of urea to calcium ions in bovine bone calcium phosphate solution is greater than 4:5, the precipitation rate of calcium phosphate in the curing agent will be too fast, so that the calcium phosphate precipitate is mainly generated at the top of the sand sample, hindering the downward penetration of the curing agent, resulting in uneven distribution of calcium phosphate precipitation and poor curing effect.
[0072] In a specific embodiment, when the crude soybean enzyme solution and the binder are uniformly mixed in the embodiment of the present invention, the volume ratio of the crude soybean enzyme solution to the binder is preferably 1 to 2.5:5.
[0073] Among them, when the volume ratio of soybean crude enzyme solution to the cementing liquid is less than 1:5, the precipitation rate of calcium phosphate in the curing agent will be too slow, which is not conducive to the cementation of sand; when the volume ratio of soybean crude enzyme solution to the cementing liquid is greater than 2.5:5, the precipitation rate of calcium phosphate in the curing agent will be too fast, so that the calcium phosphate precipitate is mainly generated on the top of the sand sample, hindering the downward penetration of the curing agent, resulting in uneven distribution of calcium phosphate precipitation and poor curing effect.
[0074] In a second aspect, an embodiment of the present invention provides a soybean crude enzyme-induced calcium phosphate solidifying agent prepared by the method described in the first aspect.
[0075] In a third aspect, an embodiment of the present invention provides a method for using the soybean crude enzyme-induced calcium phosphate curing agent according to the second aspect, the method comprising:
[0076] Preparation of sand sample: A PVC pipe is used as a mold to prepare a sand sample, wherein the inner diameter of the PVC pipe is 40 mm and the height is 78 mm; 167 g of ISO standard sand sample is weighed and added into the PVC pipe, and a piece of geotextile is placed on the top and bottom of the sand sample to prevent the loss of sand particles;
[0077] The crude soybean enzyme solution and the binder are added into the sand sample by grouting or spraying to obtain a solidified sand sample.
[0078] In a specific embodiment, the grouting method in the embodiment of the present invention is preferably: 4 to 10 mL of crude soybean enzyme solution is added to the sand sample at a rate of 5 mL / min; after the grouting of the crude soybean enzyme solution is completed, 20 mL of the binder is added to the sand sample at a rate of 5 mL / min; after the grouting of the crude soybean enzyme solution and the binder is completed, the crude soybean enzyme solution and the binder are allowed to stand for 24 hours, and the crude soybean enzyme solution and the binder are circulated for 6 to 14 times to obtain a solidified sand sample.
[0079] In a specific embodiment, the spraying method in the embodiment of the present invention is preferably: spraying 4 to 10 mL of crude soybean enzyme solution on the surface of the sand sample;
[0080] After the soybean crude enzyme solution was sprayed, 20 mL of the cementing liquid was sprayed on the surface of the sand sample;
[0081] After spraying the crude soybean enzyme solution and the binder in sequence, the mixture was allowed to stand for 24 hours, and the crude soybean enzyme solution and the binder were sprayed repeatedly for 6 to 14 times to obtain a solidified sand sample.
[0082] It should be noted that the treated sand sample is washed and placed in an oven to dry to constant weight, and the solidified sand sample is demolded. Specifically, after the multi-stage addition of soybean crude enzyme solution and binder solution is completed, pure water is injected from top to bottom several times to wash the residual soluble salt until the conductivity of the discharged liquid remains stable. After washing, the sample is placed in an oven at 50°C and dried for 48 hours. Finally, the sample is demolded to obtain a solidified sand sample.
[0083] The technical method of the present invention will be further described below in conjunction with specific embodiments.
[0084] It should be noted that the calcium phosphate source in the embodiment of the present invention is waste bovine bones.
[0085] The present invention provides a method for preparing a soybean crude enzyme solution and a bovine bone calcium phosphate solution, and the specific steps are as follows:
[0086] Put the soybeans with full and round grains into an oven and bake at 40℃ for 6-8h, then grind them into powder with a crusher; add 100g / L of soybean powder into pure water, put it into a shaker and shake for 5min, then centrifuge it at 3000rpm and 35℃ for 15min, filter it, and the clear liquid is the crude soybean enzyme solution.
[0087] Place the discarded cattle bones in an oven at 40-60℃ for 24h, then grind them into bone powder using a crusher, add 250g / L of bone powder into 0.5mol / L hydrochloric acid, place it in a shaker and shake for 1h, filter it, and the clear liquid is the calcium phosphate solution. Urea is added to the calcium phosphate solution at 0.4, 0.8 and 2mol / L respectively.
[0088] Take 20mL of crude soybean enzyme solution and mix it with 40mL of calcium phosphate solution added with 0.4, 0.8 and 2mol / L urea, and test the changes in pH and calcium ion concentration in the solution within 90min.
[0089] Test methods: pH test, EDTA determination of calcium ion concentration, scanning electron microscopy.
[0090] The above test results show that the pH in the reaction solution continues to rise, indicating that soybean crude enzyme can promote the decomposition of urea. After 90 minutes, the calcium ion concentration in the solution decreased significantly, and a large amount of white precipitate was generated in the mixed solution. According to the results of scanning electron microscopy, the white precipitate was mainly calcium phosphate.
[0091] Example 1
[0092] Example 1 of the present invention provides a method for inducing calcium phosphate solidification of sand by soybean crude enzyme, and the specific steps are as follows:
[0093] Step 1: Place the soybeans with full and round grains in an oven and bake at 40°C for 7 hours, then grind them into powder using a crusher; add 100g / L of soybean powder into pure water, place it in a shaker and shake for 5 minutes, then centrifuge at 3000rpm and 35°C for 15 minutes, filter, and the clear liquid is the crude soybean enzyme solution.
[0094] Step 2: Place the discarded cattle bones in an oven and bake at 50°C for 24 hours, then grind them into bone powder using a crusher, add 250 g / L of the bone powder into 0.5 mol / L hydrochloric acid, place it in a shaker and shake for 1 hour, filter, and the clear liquid is the calcium phosphate solution. Then use 0.5 mol / L sodium hydroxide solution to adjust the pH of the calcium phosphate solution to 3.
[0095] Step 3: Mix 0.18 g of urea with 20 mL of calcium phosphate solution to obtain a cementing solution with a urea concentration of 0.15 mol / L.
[0096] Step 4: Use a PVC pipe as a mold to prepare a sand sample. The inner diameter of the PVC pipe is 40 mm and the height is 78 mm. Weigh 167 g of ISO standard sand and add it to the PVC mold. The diameter of the sand sample is 40 mm and the height is 78 mm. Place a piece of geotextile on the top and bottom of the sand sample to prevent the loss of sand particles.
[0097] Step 5: Take 4 mL of soybean crude enzyme solution and add it to the sand sample by grouting or spraying.
[0098] Step 6: After the soybean crude enzyme solution is grouted or sprayed, immediately add the cementing liquid to the sand sample by grouting or spraying, and let it stand for 24 hours. Repeat steps 5 and 6 14 times.
[0099] Step 7: Inject the treated sand sample into pure water for multiple times to remove the residual soluble salts, then place it in a 50°C oven and bake it for 48 hours. Take it out and demould it to obtain a sand column.
[0100] Example 2
[0101] Example 2 of the present invention provides a method for inducing calcium phosphate solidification of sand with soybean crude enzyme, and the specific steps are as follows:
[0102] Step 1: Place the soybeans with full and round grains in an oven and bake at 40°C for 7 hours, then grind them into powder using a crusher; add 100g / L of soybean powder into pure water, place it in a shaker and shake for 5 minutes, then centrifuge at 3000rpm and 35°C for 15 minutes, filter, and the clear liquid is the crude soybean enzyme solution.
[0103] Step 2: Bake the discarded cattle bones in an oven at 50°C for 24 hours, then grind them into bone powder using a crusher, add 250 g / L of the bone powder into 0.5 mol / L hydrochloric acid, place it in a shaker and shake for 1 hour, filter it, and the clear liquid is the calcium phosphate solution. Then use 0.5 mol / L sodium hydroxide solution to adjust the pH of the calcium phosphate solution to 3.5.
[0104] Step 3: Mix 0.24 g of urea with 20 mL of calcium phosphate solution to obtain a cementing solution with a urea concentration of 0.2 mol / L.
[0105] Step 4: Use a PVC pipe as a mold to prepare a sand sample. The inner diameter of the PVC pipe is 40 mm and the height is 78 mm. Weigh 167 g of ISO standard sand and add it to the PVC mold. The diameter of the sand sample is 40 mm and the height is 78 mm. Place a piece of geotextile on the top and bottom of the sand sample to prevent the loss of sand particles.
[0106] Step 5: Take 8 mL of crude soybean enzyme solution and add it to the sand sample by grouting or spraying.
[0107] Step 6: After the soybean crude enzyme solution is grouted or sprayed, immediately add the cementing liquid to the sand sample by grouting or spraying, and let it stand for 24 hours. Repeat steps 5 and 6 6 times.
[0108] Step 7: Inject the treated sand sample into pure water for multiple times to remove the residual soluble salts, then place it in a 50°C oven and bake it for 48 hours. Take it out and demould it to obtain a sand column.
[0109] Example 3
[0110] Example 3 of the present invention provides a method for inducing calcium phosphate solidification of sand by soybean crude enzyme, and the specific steps are as follows:
[0111] Step 1: Place the soybeans with full and round grains in an oven and bake at 40°C for 7 hours, then grind them into powder using a crusher; add 100g / L of soybean powder into pure water, place it in a shaker and shake for 5 minutes, then centrifuge at 3000rpm and 35°C for 15 minutes, filter, and the clear liquid is the crude soybean enzyme solution.
[0112] Step 2: Place the discarded cattle bones in an oven and bake at 50°C for 24 hours, then grind them into bone powder using a crusher, add 250 g / L of the bone powder into 0.5 mol / L hydrochloric acid, place it in a shaker and shake for 1 hour, filter, and the clear liquid is the calcium phosphate solution. Then use 0.5 mol / L sodium hydroxide solution to adjust the pH of the calcium phosphate solution to 3.
[0113] Step 3: Mix 0.12 g of urea with 20 mL of calcium phosphate solution to obtain a cementing solution with a urea concentration of 0.1 mol / L.
[0114] Step 4: Use a PVC pipe as a mold to prepare a sand sample. The inner diameter of the PVC pipe is 40 mm and the height is 78 mm. Weigh 167 g of ISO standard sand and add it to the PVC mold. The diameter of the sand sample is 40 mm and the height is 78 mm. Place a piece of geotextile on the top and bottom of the sand sample to prevent the loss of sand particles.
[0115] Step 5: Take 6 mL of soybean crude enzyme solution and add it to the sand sample by grouting or spraying.
[0116] Step 6: After the soybean crude enzyme solution is grouted or sprayed, immediately add the cementing liquid to the sand sample by grouting or spraying, and let it stand for 24 hours. Repeat steps 5 and 6 10 times.
[0117] Step 7: Inject the treated sand sample into pure water for multiple times to remove the residual soluble salts, then place it in a 50°C oven and bake it for 48 hours. Take it out and demould it to obtain a sand column.
[0118] Example 4
[0119] Example 4 of the present invention provides a method for inducing calcium phosphate solidification of sand with soybean crude enzyme, and the specific steps are as follows:
[0120] Step 1: Place the soybeans with full and round grains in an oven and bake at 40°C for 6 hours, then grind them into powder using a crusher; add 100g / L of soybean powder into pure water, place it in a shaker and shake for 5 minutes, then centrifuge at 3000rpm, 35°C for 15 minutes, filter, and the clear liquid is the crude soybean enzyme solution.
[0121] Step 2: Place the discarded cattle bones in an oven and bake at 40°C for 24 hours, then grind them into bone powder using a crusher, add 250 g / L of the bone powder into 0.5 mol / L hydrochloric acid, place it in a shaker and shake for 1 hour, filter, and the clear liquid is the calcium phosphate solution. Then use 0.5 mol / L sodium hydroxide solution to adjust the pH of the calcium phosphate solution to 3.
[0122] Step 3: Mix 0.24 g of urea with 20 mL of calcium phosphate solution to obtain a cementing solution with a urea concentration of 0.2 mol / L.
[0123] Step 4: Use a PVC pipe as a mold to prepare a sand sample. The inner diameter of the PVC pipe is 40 mm and the height is 78 mm. Weigh 167 g of ISO standard sand and add it to the PVC mold. The diameter of the sand sample is 40 mm and the height is 78 mm. Place a piece of geotextile on the top and bottom of the sand sample to prevent the loss of sand particles.
[0124] Step 5: Take 6 mL of soybean crude enzyme solution and add it to the sand sample by grouting or spraying.
[0125] Step 6: After the soybean crude enzyme solution is grouted or sprayed, immediately add the cementing liquid to the sand sample by grouting or spraying, and let it stand for 24 hours. Repeat steps 5 and 6 7 times.
[0126] Step 7: Inject the treated sand sample into pure water for multiple times to remove the residual soluble salts, then place it in a 50°C oven and bake it for 48 hours. Take it out and demould it to obtain a sand column.
[0127] Example 5
[0128] Example 5 of the present invention provides a method for inducing calcium phosphate solidification of sand with soybean crude enzyme, and the specific steps are as follows:
[0129] Step 1: Place the soybeans with full and round grains in an oven and bake at 40°C for 8 hours, then grind them into powder using a crusher; add 100g / L of soybean powder into pure water, place it in a shaker and oscillate for 5 minutes, then centrifuge at 3000rpm and 35°C for 15 minutes, filter, and the clear liquid is the crude soybean enzyme solution.
[0130] Step 2: Bake the discarded cattle bones in an oven at 60°C for 24 hours, then grind them into bone powder using a crusher, add 250 g / L of the bone powder into 0.5 mol / L hydrochloric acid, place it in a shaker and shake for 1 hour, filter it, and the clear liquid is the calcium phosphate solution. Then use 0.5 mol / L sodium hydroxide solution to adjust the pH of the calcium phosphate solution to 3.
[0131] Step 3: Mix 0.18 g of urea with 20 mL of calcium phosphate solution to obtain a cementing solution with a urea concentration of 0.15 mol / L.
[0132] Step 4: Use a PVC pipe as a mold to prepare a sand sample. The inner diameter of the PVC pipe is 40 mm and the height is 78 mm. Weigh 167 g of ISO standard sand and add it to the PVC mold. The diameter of the sand sample is 40 mm and the height is 78 mm. Place a piece of geotextile on the top and bottom of the sand sample to prevent the loss of sand particles.
[0133] Step 5: Take 6 mL of soybean crude enzyme solution and add it to the sand sample by grouting or spraying.
[0134] Step 6: After the soybean crude enzyme solution is grouted or sprayed, immediately add the cementing liquid to the sand sample by grouting or spraying, and let it stand for 24 hours. Repeat steps 5 and 6 8 times.
[0135] Step 7: Inject the treated sand sample into pure water for multiple times to remove the residual soluble salts, then place it in a 50°C oven and bake it for 48 hours. Take it out and demould it to obtain a sand column.
[0136] Example 6
[0137] Example 6 of the present invention provides a method for inducing calcium phosphate solidification of sand with soybean crude enzyme, and the specific steps are as follows:
[0138] Step 1: Place the soybeans with full and round grains in an oven and bake at 40°C for 7 hours, then grind them into powder using a crusher; add 100g / L of soybean powder into pure water, place it in a shaker and shake for 5 minutes, then centrifuge at 3000rpm and 35°C for 15 minutes, filter, and the clear liquid is the crude soybean enzyme solution.
[0139] Step 2: Place the discarded cattle bones in an oven and bake at 50°C for 24 hours, then grind them into bone powder using a crusher, add 250 g / L of the bone powder into 0.5 mol / L hydrochloric acid, place it in a shaker and shake for 1 hour, filter, and the clear liquid is the calcium phosphate solution. Then use 0.5 mol / L sodium hydroxide solution to adjust the pH of the calcium phosphate solution to 3.
[0140] Step 3: Mix 0.12 g of urea with 20 mL of calcium phosphate solution to obtain a cementing solution with a urea concentration of 0.1 mol / L.
[0141] Step 4: Use a PVC pipe as a mold to prepare a sand sample. The inner diameter of the PVC pipe is 40 mm and the height is 78 mm. Weigh 167 g of ISO standard sand and add it to the PVC mold. The diameter of the sand sample is 40 mm and the height is 78 mm. Place a piece of geotextile on the top and bottom of the sand sample to prevent the loss of sand particles.
[0142] Step 5: Take 8 mL of crude soybean enzyme solution and add it to the sand sample by grouting or spraying.
[0143] Step 6: After the soybean crude enzyme solution is grouted or sprayed, immediately add the cementing liquid to the sand sample by grouting or spraying, and let it stand for 24 hours. Repeat steps 5 and 6 11 times.
[0144] Step 7: Inject the treated sand sample into pure water for multiple times to remove the residual soluble salts, then place it in a 50°C oven and bake it for 48 hours. Take it out and demould it to obtain a sand column.
[0145] Example 7
[0146] Example 7 of the present invention provides a method for inducing calcium phosphate solidification of sand with soybean crude enzyme, and the specific steps are as follows:
[0147] Step 1: Place the soybeans with full and round grains in an oven and bake at 40°C for 7 hours, then grind them into powder using a crusher; add 100g / L of soybean powder into pure water, place it in a shaker and shake for 5 minutes, then centrifuge at 3000rpm and 35°C for 15 minutes, filter, and the clear liquid is the crude soybean enzyme solution.
[0148] Step 2: Place the discarded cattle bones in an oven and bake at 50°C for 24 hours, then grind them into bone powder using a crusher, add 250 g / L of the bone powder into 0.5 mol / L hydrochloric acid, place it in a shaker and shake for 1 hour, filter, and the clear liquid is the calcium phosphate solution. Then use 0.5 mol / L sodium hydroxide solution to adjust the pH of the calcium phosphate solution to 3.
[0149] Step 3: Mix 0.18 g of urea with 20 mL of calcium phosphate solution to obtain a cementing solution with a urea concentration of 0.15 mol / L.
[0150] Step 4: Use a PVC pipe as a mold to prepare a sand sample. The inner diameter of the PVC pipe is 40 mm and the height is 78 mm. Weigh 167 g of ISO standard sand and add it to the PVC mold. The diameter of the sand sample is 40 mm and the height is 78 mm. Place a piece of geotextile on the top and bottom of the sand sample to prevent the loss of sand particles.
[0151] Step 5: Take 10 mL of soybean crude enzyme solution and add it to the sand sample by grouting or spraying.
[0152] Step 6: After the soybean crude enzyme solution is grouted or sprayed, immediately add the cementing liquid to the sand sample by grouting or spraying, and let it stand for 24 hours. Repeat steps 5 and 6 6 times.
[0153] Step 7: Inject the treated sand sample into pure water for multiple times to remove the residual soluble salts, then place it in a 50°C oven and bake it for 48 hours. Take it out and demould it to obtain a sand column.
[0154] Example 8
[0155] Example 8 of the present invention provides a method for inducing calcium phosphate solidification of sand with soybean crude enzyme, and the specific steps are as follows:
[0156] Step 1: Place the soybeans with full and round grains in an oven and bake at 40°C for 7 hours, then grind them into powder using a crusher; add 100g / L of soybean powder into pure water, place it in a shaker and shake for 5 minutes, then centrifuge at 3000rpm and 35°C for 15 minutes, filter, and the clear liquid is the crude soybean enzyme solution.
[0157] Step 2: Bake the discarded cattle bones in an oven at 50°C for 24 hours, then grind them into bone powder using a crusher, add 250 g / L of the bone powder into 0.5 mol / L hydrochloric acid, place it in a shaker and shake for 1 hour, filter it, and the clear liquid is the calcium phosphate solution. Then use 0.5 mol / L sodium hydroxide solution to adjust the pH of the calcium phosphate solution to 4.
[0158] Step 3: Mix 0.12 g of urea with 20 mL of calcium phosphate solution to obtain a cementing solution with a urea concentration of 0.1 mol / L.
[0159] Step 4: Use a PVC pipe as a mold to prepare a sand sample. The inner diameter of the PVC pipe is 40 mm and the height is 78 mm. Weigh 167 g of ISO standard sand and add it to the PVC mold. The diameter of the sand sample is 40 mm and the height is 78 mm. Place a piece of geotextile on the top and bottom of the sand sample to prevent the loss of sand particles.
[0160] Step 5: Take 4 mL of soybean crude enzyme solution and add it to the sand sample by grouting or spraying.
[0161] Step 6: After the soybean crude enzyme solution is grouted or sprayed, immediately add the cementing liquid to the sand sample by grouting or spraying, and let it stand for 24 hours. Repeat steps 5 and 6 8 times.
[0162] Step 7: Inject the treated sand sample into pure water for multiple times to remove the residual soluble salts, then place it in a 50°C oven and bake it for 48 hours. Take it out and demould it to obtain a sand column.
[0163] Example 9
[0164] Example 9 of the present invention provides a method for inducing calcium phosphate solidification of sand with soybean crude enzyme, and the specific steps are as follows:
[0165] Step 1: Place the soybeans with full and round grains in an oven and bake at 40°C for 7 hours, then grind them into powder using a crusher; add 100g / L of soybean powder into pure water, place it in a shaker and shake for 5 minutes, then centrifuge at 3000rpm and 35°C for 15 minutes, filter, and the clear liquid is the crude soybean enzyme solution.
[0166] Step 2: Bake the discarded cattle bones in an oven at 50°C for 24 hours, then grind them into bone powder using a crusher, add 250 g / L of the bone powder into 0.5 mol / L hydrochloric acid, place it in a shaker and shake for 1 hour, filter it, and the clear liquid is the calcium phosphate solution. Then use 0.5 mol / L sodium hydroxide solution to adjust the pH of the calcium phosphate solution to 4.
[0167] Step 3: Mix 0.24 g of urea with 20 mL of calcium phosphate solution to obtain a cementing solution with a urea concentration of 0.2 mol / L.
[0168] Step 4: Use a PVC pipe as a mold to prepare a sand sample. The inner diameter of the PVC pipe is 40 mm and the height is 78 mm. Weigh 167 g of ISO standard sand and add it to the PVC mold. The diameter of the sand sample is 40 mm and the height is 78 mm. Place a piece of geotextile on the top and bottom of the sand sample to prevent the loss of sand particles.
[0169] Step 5: Take 8 mL of crude soybean enzyme solution and add it to the sand sample by grouting or spraying.
[0170] Step 6: After the soybean crude enzyme solution is grouted or sprayed, immediately add the cementing liquid to the sand sample by grouting or spraying, and let it stand for 24 hours. Repeat steps 5 and 6 7 times.
[0171] Step 7: Inject the treated sand sample into pure water for multiple times to remove the residual soluble salts, then place it in a 50°C oven and bake it for 48 hours. Take it out and demould it to obtain a sand column.
[0172] Example 10
[0173] Example 10 of the present invention provides a method for inducing calcium phosphate solidification of sand with soybean crude enzyme, and the specific steps are as follows:
[0174] Step 1: Place the soybeans with full and round grains in an oven and bake at 40°C for 7 hours, then grind them into powder using a crusher; add 100g / L of soybean powder into pure water, place it in a shaker and shake for 5 minutes, then centrifuge at 3000rpm and 35°C for 15 minutes, filter, and the clear liquid is the crude soybean enzyme solution.
[0175] Step 2: Place the discarded cattle bones in an oven and bake at 50°C for 24 hours, then grind them into bone powder using a crusher, add 250 g / L of the bone powder into 0.5 mol / L hydrochloric acid, place it in a shaker and shake for 1 hour, filter, and the clear liquid is the calcium phosphate solution. Then use 0.5 mol / L sodium hydroxide solution to adjust the pH of the calcium phosphate solution to 3.
[0176] Step 3: Mix 0.12 g of urea with 20 mL of calcium phosphate solution to obtain a cementing solution with a urea concentration of 0.1 mol / L.
[0177] Step 4: Use a PVC pipe as a mold to prepare a sand sample. The inner diameter of the PVC pipe is 40 mm and the height is 78 mm. Weigh 167 g of ISO standard sand and add it to the PVC mold. The diameter of the sand sample is 40 mm and the height is 78 mm. Place a piece of geotextile on the top and bottom of the sand sample to prevent the loss of sand particles.
[0178] Step 5: Take 4 mL of soybean crude enzyme solution and add it to the sand sample by grouting or spraying.
[0179] Step 6: After the soybean crude enzyme solution is grouted or sprayed, immediately add the cementing liquid to the sand sample by grouting or spraying, and let it stand for 24 hours. Repeat steps 5 and 6 14 times.
[0180] Step 7: Inject the treated sand sample into pure water for multiple times to remove the residual soluble salts, then place it in a 50°C oven and bake it for 48 hours. Take it out and demould it to obtain a sand column.
[0181] Comparative Example 1
[0182] This comparative example provides a method for ordinary sand solidification, and the specific steps are as follows:
[0183] Step 1: Place the soybeans with full and round grains in an oven and bake at 40°C for 7 hours, then grind them into powder using a crusher; add 100g / L of soybean powder into pure water, place it in a shaker and shake for 5 minutes, then centrifuge at 3000rpm and 35°C for 15 minutes, filter, and the clear liquid is the crude soybean enzyme solution.
[0184] Step 2: Use a PVC pipe as a mold to prepare a sand sample. The inner diameter of the PVC pipe is 40 mm and the height is 78 mm. Weigh 167 g of ISO standard sand and add it to the PVC mold. The sand sample has a diameter of 40 mm and a height of 78 mm. Place a piece of geotextile on the top and bottom of the sand sample to prevent the loss of sand particles.
[0185] Step 3: Take 10 mL of soybean crude enzyme solution and add it to the sand sample by grouting or spraying and let it stand for 24 hours. Repeat step 3 14 times.
[0186] Step 4: Inject the treated sand sample into pure water for multiple times for cleaning, place it in a 50°C oven for 48 hours, and then take it out and demold it.
[0187] Comparative Example 2
[0188] This comparative example provides another method for ordinary sand solidification, and the specific steps are as follows:
[0189] Step 1: Bake the discarded cattle bones in an oven at 50°C for 24 hours, then grind them into bone powder using a crusher, add 250 g / L of bone powder into 0.5 mol / L hydrochloric acid, put it in a shaker and shake for 1 hour, filter, and the clear liquid is the calcium phosphate solution. Then use 0.5 mol / L sodium hydroxide solution to adjust the pH of the calcium phosphate solution to 3.
[0190] Step 2: Mix 0.18 g of urea with 20 mL of calcium phosphate solution to obtain a cementing solution with a urea concentration of 0.15 mol / L.
[0191] Step 3: Use a PVC pipe as a mold to prepare a sand sample. The inner diameter of the PVC pipe is 40 mm and the height is 78 mm. Weigh 167 g of ISO standard sand and add it to the PVC mold. The sand sample has a diameter of 40 mm and a height of 78 mm. Place a piece of geotextile on the top and bottom of the sand sample to prevent the loss of sand particles.
[0192] Step 4: Add the binder to the sand sample by grouting or spraying and let it stand for 24 hours. Repeat step 4 14 times.
[0193] Step 7: Inject the treated sand sample into pure water several times to remove the residual soluble salt, then place it in a 50°C oven for 48 hours and remove it from the mold.
[0194] Comparative Example 3
[0195] This comparative example provides another method for consolidating sand in general, and the specific steps are as follows:
[0196] Step 1: Place the soybeans with full and round grains in an oven and bake at 40°C for 7 hours, then grind them into powder using a crusher; add 100g / L of soybean powder into pure water, place it in a shaker and shake for 5 minutes, then centrifuge at 3000rpm and 35°C for 15 minutes, filter, and the clear liquid is the crude soybean enzyme solution.
[0197] Step 2: Place the discarded cattle bones in an oven and bake at 50°C for 24 hours, then grind them into bone powder using a crusher, add 250 g / L of the bone powder into 0.5 mol / L hydrochloric acid, place it in a shaker and shake for 1 hour, filter, and the clear liquid is the calcium phosphate solution. Then use 0.5 mol / L sodium hydroxide solution to adjust the pH of the calcium phosphate solution to 3.
[0198] Step 3: Use a PVC pipe as a mold to prepare a sand sample. The inner diameter of the PVC pipe is 40 mm and the height is 78 mm. Weigh 167 g of ISO standard sand and add it to the PVC mold. The sand sample has a diameter of 40 mm and a height of 78 mm. Place a piece of geotextile on the top and bottom of the sand sample to prevent the loss of sand particles.
[0199] Step 4: Take 4 mL of soybean crude enzyme solution and add it to the sand sample by grouting or spraying.
[0200] Step 5: After the soybean crude enzyme solution is grouted or sprayed, immediately add 20 ml of calcium phosphate solution to the sand sample by grouting or spraying, and let it stand for 24 hours. Repeat steps 4 and 5 14 times.
[0201] Step 6: Inject the treated sand sample into pure water several times to remove the residual soluble salt, then place it in a 50°C oven for 48 hours and remove it from the mold.
[0202] Comparative Example 4
[0203] This comparative example provides a method for enzyme-induced calcium carbonate solidification of sand, and the specific steps are as follows:
[0204] Step 1: Place the soybeans with full and round grains in an oven and bake at 40°C for 7 hours, then grind them into powder using a crusher; add 100g / L of soybean powder into pure water, place it in a shaker and shake for 5 minutes, then centrifuge at 3000rpm and 35°C for 15 minutes, filter, and the clear liquid is the crude soybean enzyme solution.
[0205] Step 2: Take 1.2g urea and 2.22g calcium chloride and dissolve them in 20mL water to obtain a cementing solution with a urea and calcium chloride concentration of 1 mol / L.
[0206] Step 3: Use a PVC pipe as a mold to prepare a sand sample. The inner diameter of the PVC pipe is 40 mm and the height is 78 mm. Weigh 167 g of ISO standard sand and add it to the PVC mold. The sand sample has a diameter of 40 mm and a height of 78 mm. Place a piece of geotextile on the top and bottom of the sand sample to prevent the loss of sand particles.
[0207] Step 4: Take 10 mL of crude soybean enzyme solution and add it to the sand sample by grouting or spraying.
[0208] Step 5: After the soybean crude enzyme solution is grouted or sprayed, immediately add the cementing liquid to the sand sample by grouting or spraying, and let it stand for 24 hours. Repeat steps 4 and 5 5 times.
[0209] Step 6: Inject the treated sand sample into pure water several times to remove the residual soluble salt, then place it in a 50°C oven for 48 hours and remove it from the mold.
[0210] Table 1 Comparison of the test results of unconfined compressive strength, calcium phosphate / calcium carbonate content and average pH value of the effluent of Examples 1-10 and Comparative Examples 1-4
[0211]
[0212] According to the analysis of Table 1, the unconfined compressive strength has no direct relationship with the content of calcium phosphate in the sand column. The calcium phosphate content is between 0.8% and 2.1%, and the calcium phosphate content in most sand columns is about 1%. The unconfined compressive strength is mainly related to the uniformity of calcium phosphate distribution. The smaller the difference in calcium phosphate content in the upper and lower parts of the sand column, the more uniform the distribution of calcium phosphate precipitation in the sand column, and the higher the unconfined compressive strength of the sand column. The final pH of the curing agent reaction is stable between 7 and 8, and this range can effectively reduce the release of ammonia. Comparative Example 4 is a sand sample solidified by enzyme-induced calcium carbonate. By comparing it with soybean crude enzyme-induced calcium phosphate, it can be seen that the average pH of the effluent obtained by soybean crude enzyme-induced calcium phosphate is lower, indicating that it can reduce the emission of ammonia during the reaction and is more environmentally friendly.
[0213] according to Figure 1 It can be seen that the crude soybean enzyme solution is a yellow turbid liquid.
[0214] according to Figure 2 It can be seen that bovine bone calcium phosphate solution is an orange-yellow transparent solution.
[0215] according to Figure 3 It can be seen that the sand column was grouted with a peristaltic pump at a grouting speed of 5 ml / min.
[0216] according to Figure 4 It can be seen that after treatment with a curing agent, the loose sand becomes a sand column with a certain strength.
[0217] according to Figure 5 It can be seen that the strength of the sand column after curing agent treatment can reach up to 625kPa, but the strength of most sand columns is around 300kPa.
[0218] according to Figure 6 It can be seen that the calcium phosphate content in the sand column after curing agent treatment is between 0.8% and 2.1%.
[0219] according to Figure 7 It can be seen that the calcium ion concentration in the curing agent decreases with the increase of pH, indicating that calcium ions precipitate from the solution in the form of calcium phosphate precipitation.
[0220] according to Figure 8 It can be seen that as the pH of the curing agent increases, a large amount of white calcium phosphate precipitates are generated in the solution.
[0221] according to Fig. 9 It can be seen that the microscopic morphology of the calcium phosphate precipitate generated in the solution is petal-shaped.
[0222] Fig.10 for Fig. 9 The energy spectrum analysis results are based on Fig.10 It can be seen that the petal-shaped precipitate is calcium phosphate precipitate.
[0223] according to Fig.11 It can be seen that the percentage of ammonium ions converted into ammonia in the process of soybean crude enzyme-induced calcium phosphate (5% to 14.27%) is much lower than that of EICP / MICP technology (14.27% to 62.92%), which significantly reduces the release of ammonia.
[0224] according to Fig.12 It can be seen that the microscopic morphology of calcium phosphate generated in the sand column is mainly spherical.
[0225] Fig.13 for Fig.12 The enlarged image of the area (a) is based on Fig.13 It can be seen that calcium phosphate plays a connecting and filling role between sand particles.
[0226] Fig.14 for Fig.13 The energy spectrum analysis results are based on Fig.14 It can be seen that the spherical precipitate is calcium phosphate precipitate.
[0227] In summary, the present invention provides a method for solidifying sand by inducing calcium phosphate with soybean crude enzyme, which can effectively improve the strength of sand, provide a new idea for the proper disposal of waste animal aggregates, and compared with MICP / EICP technology, this method can reduce ammonia emissions. This method has good application prospects in the fields of foundation reinforcement, slope erosion protection, windbreak and sand control.
[0228] The above is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any person skilled in the art can easily think of changes or substitutions within the technical scope disclosed by the present invention, which should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope of the claims.
Claims
1. A method for preparing a soybean crude enzyme-induced calcium phosphate curing agent, characterized in that: include: preparing a crude soybean enzyme solution, wherein the concentration of the crude soybean enzyme solution is 100 g / L; Using discarded cattle bones to prepare a bovine bone calcium phosphate solution, wherein the concentration of the bovine bone calcium phosphate solution is 250 g / L; After uniformly mixing urea with the bovine bone calcium phosphate solution, a cementing liquid is obtained; The crude soybean enzyme solution and the cementing liquid are uniformly mixed to obtain the crude soybean enzyme-induced calcium phosphate curing agent.
2. The method for preparing the crude soybean enzyme-induced calcium phosphate curing agent according to claim 1, characterized in that: The preparation of soybean crude enzyme solution comprises: The soybeans are placed in an oven and baked at 40° C. for 6 to 8 hours, dried and ground into powder, added into water to form a suspension, shaken, centrifuged and filtered to obtain the soybean crude enzyme solution.
3. The method for preparing the crude soybean enzyme-induced calcium phosphate curing agent according to claim 1, characterized in that: The preparation of the bovine bone calcium phosphate solution comprises: The discarded bovine bones are placed in an oven and baked at 40-60° C. for 24 hours, dried and ground into bone powder, added into 0.5 mol / L hydrochloric acid to form a suspension, shaken, centrifuged and filtered to obtain the bovine bone calcium phosphate solution.
4. The method for preparing the crude soybean enzyme-induced calcium phosphate curing agent according to claim 1, characterized in that: When the urea and the bovine bone calcium phosphate solution are uniformly mixed, the concentration of the urea is 0.1-0.2 mol / L.
5. The method for preparing the soybean crude enzyme-induced calcium phosphate curing agent according to claim 1, characterized in that: When the urea and the bovine bone calcium phosphate solution are uniformly mixed, the molar ratio of the urea to the bovine bone calcium phosphate solution is 2 to 4:
5.
6. The method for preparing the crude soybean enzyme-induced calcium phosphate curing agent according to claim 1, characterized in that: When the crude soybean enzyme solution and the binder are uniformly mixed, the volume ratio of the crude soybean enzyme solution to the binder is 1-2.5:
5.
7. A soybean crude enzyme-induced calcium phosphate solidifying agent prepared by the method according to any one of claims 1 to 6.
8. A method for using the crude soybean enzyme-induced calcium phosphate solidifying agent according to claim 7, wherein the crude soybean enzyme-induced calcium phosphate solidifying agent comprises a crude soybean enzyme solution and a cementing liquid, characterized in that: include: Preparation of sand sample: A PVC pipe is used as a mold to prepare a sand sample, wherein the inner diameter of the PVC pipe is 40 mm and the height is 78 mm; 167 g of ISO standard sand sample is weighed and added into the PVC pipe, and a piece of geotextile is placed on the top and bottom of the sand sample to prevent the loss of sand particles; The crude soybean enzyme solution and the binder are added into the sand sample by grouting or spraying to obtain a solidified sand sample.
9. The method for using the soybean crude enzyme-induced calcium phosphate curing agent according to claim 8, characterized in that: The grouting method comprises: Adding 4-10 mL of the crude soybean enzyme solution into the sand sample at a rate of 5 mL / min; After the soybean crude enzyme solution grouting is completed, 20 mL of the cementing liquid is added to the sand sample at a rate of 5 mL / min; After the soybean crude enzyme solution and the cementing liquid are grouted in sequence, the grouting is allowed to stand for 24 hours, and the soybean crude enzyme solution and the cementing liquid are grouted in a cycle for 6 to 14 times to obtain the solidified sand sample.
10. The method for using the soybean crude enzyme-induced calcium phosphate curing agent according to claim 8, characterized in that: The spraying method comprises: Spray 4-10 mL of the crude soybean enzyme solution on the surface of the sand sample; After the soybean crude enzyme solution is sprayed, 20 mL of the binder is sprayed on the surface of the sand sample; After spraying the crude soybean enzyme solution and the binder solution in sequence, the mixture is allowed to stand for 24 hours, and the crude soybean enzyme solution and the binder solution are sprayed repeatedly for 6 to 14 times to obtain the solidified sand sample.