Multi-element doped zirconium oxide light-cured ceramic slurry as well as preparation method and application thereof

By modifying the combination of doped ceramic powder and photosensitive resin, a multi-doped zirconia photocured ceramic slurry is formed, which solves the problem of poor dispersion stability of ceramic powder, improves the mechanical properties of zirconia ceramics, and achieves high solidity Content and excellent rheological properties, suitable for 3D printing of high-performance ceramic parts.

CN118993729APending Publication Date: 2024-11-22SHENYANG LIGONG UNIV
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411127902.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-16
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The existing zirconia ceramic 3D printing technology faces the contradiction between high solid phase content, rheology and photocuring properties, resulting in poor dispersion stability of ceramic powder, difficulty in photopolymerization, and lack of reaction process for photocured ceramic slurry system The in-depth understanding of zirconia ceramic parts has limited the improvement of mechanical properties.

Method used

Multi-doped zirconia photocuring ceramic slurry composed of modified doped ceramic powder, photosensitive resin, dispersant and photoinitiator is used to form a three-dimensional structure cladding layer and space through the combination of modifier and dispersant. Chain resistance improves powder dispersion and fluidity, and achieves uniform doping and mixing of high solids content.

Benefits of technology

It significantly improves the rheological properties and printing self-leveling properties of ceramic slurries, improves the mechanical properties of zirconia ceramics, and obtains ceramic parts with Vickers hardness greater than 1900Hv and flexural strength greater than 600MPa, suitable for biomedicine, aerospace, etc. field.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118993729A_ABST
    Figure CN118993729A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of additive manufacturing and forming, and particularly relates to multi-element zirconium oxide-doped light-cured ceramic slurry as well as a preparation method and application of the multi-element zirconium oxide-doped light-cured ceramic slurry. The 3D printing slurry obtained by the traditional zirconia ceramic slurry preparation process has the defects of single ceramic powder type, low solid content, poorer dispersion stability and printing self-leveling property and the like. The mechanical property of a 3D printing ceramic part is poorer than that of zirconia ceramic prepared by a traditional forming process. In order to solve the problems, various oxide powders are uniformly dispersed in the ceramic slurry by utilizing modified doped ceramic powder and adopting a composite modification-multi-element co-doping method, so that the rheological property and the printing self-leveling property of the ceramic slurry are greatly improved, and the application range of the ceramic slurry is widened. The solid content of the powder is increased, meanwhile, uniform doping and mixing of multi-element oxide powder are achieved, the mechanical property is remarkably improved, and the method has huge potential application value in the medical clinical field and the military aviation and aerospace field.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of additive manufacturing, and in particular relates to a multi-element doped zirconium oxide photocuring ceramic slurry and a preparation method and application thereof. Background Art

[0002] As one of the important links in ceramic preparation, material forming technology plays a decisive role in the structure, performance and application of ceramic products. In recent years, 3D printing technology (also known as additive manufacturing technology) as an emerging forming and manufacturing technology has enabled "hard and brittle" ceramic products to meet the needs of personalization, refinement, lightness, complexity and rapid manufacturing while maintaining excellent mechanical properties, thermal properties and chemical stability, greatly expanding the development and application of high-performance ceramic products. Among them, light-curing 3D printing technology has attracted much attention for its faster production speed, better surface finish and isotropic material properties.

[0003] The component design and formulation of ceramic slurry is a key link in ceramic 3D printing technology, and plays a vital role in the photocuring process and the realization of excellent performance of ceramic parts. 3D printing technology usually requires the use of ceramic slurry with a high solid content (greater than 75wt%) to reduce shrinkage and maintain the density of the parts during post-processing. However, the introduction of ceramic powder will also cause the viscosity of the slurry to increase and the fluidity to decrease, making it difficult to spread the material and print, thereby affecting the thickness and uniformity of the cured layer. At the same time, the increase in the amount of ceramic powder will significantly affect the transmission effect of ultraviolet light, thereby reducing the degree of polymerization and curing depth of the slurry. Therefore, there is a natural contradiction between the excellent rheological properties and photocuring properties of ceramic slurry and its high solid content. How to further increase the solid content of the slurry while ensuring the printing effect and improve the mechanical properties of ceramic parts has become a bottleneck that currently restricts the development of ceramic 3D printing technology in various types of advanced ceramic fields.

[0004] Zirconia ceramic 3D printing technology has achieved remarkable development in the fields of biomedicine, aerospace, and automobile manufacturing, but it still faces some key problems that need to be solved. For example, in the production process of zirconia ceramic mechanical parts, there are often higher requirements for mechanical properties. When preparing zirconia ceramics by traditional molding processes, complex doping element regulation can often be used to guide grain boundary engineering to improve ceramic performance. However, for 3D printed zirconia ceramics, the zirconia powder has a high refractive index and often contains a large number of hydroxyl groups on the surface, which makes the dispersion stability of zirconia ceramic slurry poor and the photopolymerization reaction difficult. In addition, there is currently a lack of in-depth understanding of the reaction process of photocurable ceramic slurry systems, making the preparation of highly dispersed, multi-doped modified zirconia slurry still challenging. Summary of the invention

[0005] In view of the problems in the prior art, the primary purpose of the present invention is to provide a multi-doped zirconium oxide photocurable ceramic slurry. Secondly, the purpose of the present invention is to provide a method for preparing the multi-doped zirconium oxide photocurable ceramic slurry. Thirdly, the purpose of the present invention is to provide an application of the multi-doped zirconium oxide photocurable ceramic slurry.

[0006] The multi-doped zirconium oxide photocurable ceramic slurry described in the present invention is composed of modified doped ceramic powder, photosensitive resin, dispersant, and photoinitiator; the modified doped ceramic powder is composed of metal oxide doped ceramic powder and modifier, the metal oxide doped ceramic powder includes zirconium oxide powder and doped oxide powder, and the doped oxide powder is a mixture of yttrium oxide powder, samarium oxide powder, cerium oxide powder, and lanthanum oxide powder.

[0007] The modifier forms a three-dimensional coating layer on the surface of the metal oxide-doped ceramic powder, a part of the dispersant is filled between the modified powder particles and the resin molecules, and the other part forms a bridge with the steric hindrance chain of the modifier.

[0008] The photocurable ceramic slurry contains 75wt%-95wt% of modified doped ceramic powder and 5wt%-25wt% of photosensitive resin, and the total amount of the two is 100%. The added dispersant is 2wt% of the modified doped ceramic powder, the photoinitiator is 2wt% of the photosensitive resin, and the modifier is 2wt% of the metal oxide doped ceramic powder.

[0009] The metal oxide doped ceramic powder is a nearly spherical or spherical powder particle with a particle size of 50nm-10μm.

[0010] The doped oxide powder is 8wt% to 15wt% of the zirconium oxide powder; the mass ratio of lanthanum oxide powder, samarium oxide powder, cerium oxide powder and yttrium oxide powder in the doped oxide powder is 0.7:7:0.3:5.

[0011] The modifier is any one of silane coupling agents such as n-decyltrimethoxysilane (CAS No.: 5575-48-4), dodecyltriethoxysilane (CAS No.: 18536-91-9), octadecyltrimethoxysilane (CAS No.: 3069-42-9), docosyltriethoxysilane (CAS No.: 330457-44-8) or a mixture of several of them in any proportion; preferably, the silane coupling agent has an anchoring group number of ≥2, and an alkane main chain carbon atom number (excluding carbon in the anchoring group) of ≥10, and the longer the alkane main chain, the better the overall modification effect.

[0012] The photosensitive resin is an acrylate resin, including resin A and resin B, wherein resin A accounts for 60-80% of the total volume of the photosensitive resin, and resin B accounts for 20-40% of the total volume of the photosensitive resin; resin A includes any one of trimethylolpropane triacrylate (CAS No.: 15625-89-5), ethoxylated pentaerythritol tetraacrylate (CAS No.: 51728-26-8), dipentaerythritol hexaacrylate (CAS No.: 29570-58-9) or Several kinds are mixed in any proportion; Resin B includes any one or several kinds of methyl methacrylate (CAS No.: 80-62-6), 1,6-hexanediol diacrylate (CAS No.: 13048-33-4), isobornyl acrylate (CAS No.: 5888-33-5), dipropylene glycol diacrylate (CAS No.: 57472-68-1), and tripropylene glycol diacrylate (CAS No.: 42978-66-5) are mixed in any proportion.

[0013] The photoinitiator is any one of diphenyl (2,4,6-trimethylbenzoyl) phosphine oxide (CAS No.: 75980-60-8), benzoyl peroxide (CAS No.: 94-36-0), and phenyl bis (2,4,6-trimethylbenzoyl) phosphine oxide (CAS No.: 162881-26-7).

[0014] The dispersant is an acrylate compound containing an alkane chain, including dispersant A or dispersant B;

[0015] The dispersant A comprises any one of methyl acrylate, ethyl acrylate, propyl acrylate and other acrylic esters containing short-chain alkanes, or a mixture of several of them in any proportion, wherein the number of carbon atoms in the alkane chain (excluding the carbon in the acrylic acid group) is 1 to 3;

[0016] The dispersant B includes any one of butyl acrylate, pentyl acrylate, hexyl acrylate, n-heptyl acrylate and other acrylates containing long-chain alkanes, or a mixture of several of them in any proportion, wherein the carbon number of the alkane chain (excluding the carbon in the acrylic acid group) is 4-20.

[0017] The method for preparing a multi-element doped zirconium oxide light-cured ceramic slurry of the present invention comprises the following steps:

[0018] S1 Preparation of modified doped ceramic powder

[0019] The zirconium oxide powder, the doped oxide powder and the modifier are mixed, and the mixed powder is ball-milled in a microwave environment of 800-1200 W for 6-8 hours to obtain a modified doped ceramic powder;

[0020] S2 Preparation of Multi-doped Zirconia Photocurable Ceramic Slurry

[0021] The modified doped ceramic powder, photosensitive resin, dispersant and photoinitiator are uniformly mixed under stirring conditions in 100-150W ultrasonic dispersion for 5-10 minutes to obtain multi-doped zirconia photocurable ceramic slurry with a viscosity of 2000-5000mPa·s.

[0022] The specific preparation method of step S1 is as follows:

[0023] Take 90-110g of zirconium oxide powder and 8-15wt% of doped oxide powder of zirconium oxide powder for later use;

[0024] 1.8-2.2 g of modifier, 15-30 ml of ethanol (or acetone) and 20-40 ml of deionized water are placed in a beaker and fully premixed with an electric stirrer at 400-420 rpm for 10-20 min, and then placed in an ultrasonic disperser and dispersed at a power of 30-60 W for 20-40 min to obtain a ceramic powder modifier for standby use;

[0025] Measure 200-500 ml of deionized water and put it into a beaker. Use a water bath high-speed stirrer to stir for 30-50 minutes at a water bath temperature of 80°C and a stirring speed of 400-430 rpm. During the stirring process, gradually add the weighed zirconium oxide powder and doped oxide powder, and then add the ceramic powder modifier to prepare the oxide powder premix for use.

[0026] The oxide powder premix is ​​placed in a high-energy ball mill and ball-milled in a 800-1200W microwave environment for 6-8 hours. The solution is then filtered. After the filtration is completed, the powder is dried at 80-100°C for 8-10 hours, aged for 15-20 hours, and pulverized by a pulverizer to obtain a modified doped ceramic powder for use.

[0027] Step S2

[0028] The specific preparation method is as follows:

[0029] Place the photosensitive resin, dispersant and photoinitiator in a beaker and premix them using a high-speed stirrer. The mixing time is 5 to 15 minutes and the stirring speed is 350 to 450 rpm.

[0030] The modified doped ceramic powder is gradually added to the mixed solution of photosensitive resin, dispersant and photoinitiator in batches, stirred for 3 to 5 minutes at a stirring speed of 550 to 650 rpm, and then placed in an ultrasonic disperser for dispersion at a power of 100 to 150 W for 5 to 10 minutes to obtain the multi-element doped zirconia photocurable ceramic slurry of the present invention, the viscosity of which is in the range of 2000-5000 mPa·s, and is placed in a light-shielding bottle and stored away from light for later use.

[0031] The application of the multi-element doped zirconium oxide photocurable ceramic slurry of the present invention is to design a 3D printing model that meets the requirements in the fields of biomedicine, aerospace and automobile manufacturing, and to perform 3D printing using the multi-element doped zirconium oxide photocurable ceramic slurry of the present invention as a raw material, including the following specific steps:

[0032] (1) 3D printed ceramic body

[0033] The prepared multi-doped zirconia ceramic slurry is printed using a digital light processing printer (DLP) or a stereolithography printer (SLA) with a light source wavelength of 405 nm and a light source intensity of 10 to 280 mW / cm 2 , exposure time 2 to 10 s, and a 3D printed body is obtained.

[0034] (2) Degreasing and sintering of 3D printed ceramic bodies

[0035] Place the 3D printed body in a high temperature oxidation furnace and heat it to 180-200°C at 1-3°C / min and keep it warm for 1-1.5h; heat it to 240-250°C at 1-3°C / min and keep it warm for 1-1.5h; heat it to 380-400°C at 1-3°C / min and keep it warm for 1-1.5h; heat it to 450-470°C at 1-3°C / min and keep it warm for 1-1.5h; heat it to 1-3°C / min and keep it warm for 1-1.5h. The method comprises heating the temperature to 590-610°C at 3-7°C / min and keeping the temperature for 1.5-2.5h; heating the temperature to 1000°C at 3-7°C / min and keeping the temperature for 20-40min; then heating the temperature to 1450°C at 3-7°C / min and keeping the temperature for 0.8-1.2h; then heating the temperature to 1550-1650°C at 3-7°C / min, keeping the temperature for 1.5-2.5h and then cooling the temperature naturally to obtain a multinary doped zirconia ceramic product.

[0036] The present invention adopts a "composite modification-multi-element co-doping" method of combining a modifier with a dispersant and co-doping with multiple metal oxides to improve the overall performance of zirconium oxide photocurable ceramic slurry. High-energy ball milling is used to homogenize the doped powder, and mechanical crushing is used to increase the hydroxyl groups on the surface of the powder. At the same time, the microwave and high-energy ball milling environment promote the modification process. The silane coupling agent containing multiple anchoring groups is anchored at multiple points on the surface of the metal oxide doped ceramic powder, and the long-chain alkane at the other end forms a long-lasting and stable three-dimensional structure coating layer with a steric hindrance effect as the main effect. The coating layer forms a "steric barrier" on the outer space of the metal oxide doped ceramic powder; the dispersant A is uniformly filled and dispersed between the modified powder particles and the resin molecules through ultrasonic oscillation of a specific power. One end of its alkane chain is similar to the alkane molecular structure of the modifier, forming an effective mutual solubility, and one end of its acrylic acid group forms an effective mutual solubility with the resin. Dispersant A has a shorter molecular chain and can act as a lubricant between the long chains of the modifier, preventing particles from agglomerating, forming a synergistic dispersion effect of "long and short molecular chains-steric barriers", reducing the viscosity of the slurry and improving the fluidity of the slurry; dispersant B is uniformly filled and dispersed between the powder particles and the resin molecules through ultrasonic oscillation at a specific power. One end of its alkane chain is longer than that of dispersant A, and can be miscible with the alkane chain of the modifier and form a bridging effect, forming a grafted steric chain on the surface of the ceramic powder to enhance spatial steric hindrance. The acrylic acid group at the other end of its molecular chain has extremely strong miscibility with the resin, preventing powders from agglomerating due to further bridging of the steric hindrance long chain, thereby achieving a synergistic dispersion effect of "chain extension and solubilization".

[0037] After being modified by a modifier, the metal oxide doped ceramic powder is coupled with a variety of dispersants to form a multi-dimensional synergistic dispersion of "chain extension and solubilization" and "long and short molecular chains-steric barriers", which enhances the dispersion effect of different oxide powders in the resin system, thereby achieving uniform dispersion of various metal oxide powders such as zirconia powder and doped oxide powder in the ceramic slurry.

[0038] The 3D printing slurry products obtained by the traditional zirconia ceramic slurry preparation process have the disadvantages of single ceramic powder type, low solid content, poor dispersion stability, rheology and printing self-leveling, which seriously affect the printing process; the mechanical properties of the prepared 3D printed ceramic parts are worse than those of zirconia ceramics prepared by traditional molding processes. In order to solve the above problems, the present invention uses modified doped ceramic powders and adopts the method of "composite modification-multi-element co-doping" to achieve uniform dispersion of multiple oxide powders in ceramic slurry, greatly improving the rheological properties, viscosity and printing self-leveling of ceramic slurry, while improving the solid content of powders. At the same time, the uniform doping and mixing of multi-element oxide powders are achieved, and the mechanical properties are significantly improved by directional regulation of the grain boundary segregation behavior of metal cations in zirconia, and zirconia ceramics with Vickers hardness greater than 1900Hv and flexural strength greater than 600MPa are obtained, which has great potential application value in the medical clinical field and military aerospace field. BRIEF DESCRIPTION OF THE DRAWINGS

[0039] Figure 1 The figures are rectangular parallelepiped ceramic product sample pictures, wherein A is the multinary doped zirconia ceramic product sample picture of Example 1, B is the ceramic product sample picture of Comparative Example 1, and C is the ceramic product sample picture of Comparative Example 3.

[0040] Figure 2 This is a microstructure diagram of the multi-element doped zirconia rectangular ceramic component of Example 1.

[0041] Figure 3 This is a micrograph of the printed surface (3 mm×3 mm) of the multinary-doped zirconia rectangular ceramic component of Example 1.

[0042] Figure 4 This is a microstructure diagram of the multi-element doped zirconia rectangular ceramic component of Example 2.

[0043] Figure 5 This is a microstructure diagram of the multi-component doped zirconia rectangular ceramic component of Example 3.

[0044] Figure 6 This is the microstructure diagram of the rectangular ceramic component of Comparative Example 1.

[0045] Figure 7 This is the microstructure diagram of the rectangular ceramic component of comparative example 3.

[0046] Figure 8 This is the microstructure diagram of the rectangular ceramic component of comparative example 5.

[0047] Fig. 9 This is a micrograph of the printed surface (3 mm × 3 mm) of the rectangular ceramic component of Comparative Example 6.

[0048] Fig.10The mechanical properties of the rectangular ceramic parts in each embodiment and comparative example are shown.

[0049] Fig.11 ] are infrared spectra of ceramic powders, wherein a is the infrared spectrum of the unmodified doped ceramic powder of comparative example 4, and b is the infrared spectrum of the modified doped ceramic powder of embodiment 1.

[0050] Fig.12 This is a sample picture of a pentagonal dodecahedron hollow sphere of a multi-component doped zirconia ceramic product according to Example 1. DETAILED DESCRIPTION

[0051] The equipment and reagents used in the present invention are described as follows, and those not described herein can be obtained from conventional commercial sources.

[0052] The microwave reaction furnace is a HAMiLab-AS1500 microwave muffle furnace;

[0053] The electric kiln model is the German Nabertherm high-temperature furnace;

[0054] The drying oven is the electric constant temperature blast drying oven DHG-9146A from Shanghai Jinghong Experimental Equipment Co., Ltd.

[0055] The stirrer is a DF-101S constant temperature heating magnetic stirrer from Shanghai Niyue Instrument Co., Ltd.

[0056] The ultrasonic disperser is a BT-50 ultrasonic disperser from Dandong Better Instrument Co., Ltd.

[0057] Resin A and resin B were purchased from Shanghai Yinchang New Materials Co., Ltd.;

[0058] Yttrium oxide powder, samarium oxide powder, cerium oxide powder, lanthanum oxide powder, modifier, dispersant A, and dispersant B were purchased from Sinopharm Chemical Reagent Co., Ltd.

[0059] The present invention adopts the "microwave-high energy ball milling" process to quickly realize the "doping-refining-surface activation" of zirconium oxide powder and other doped oxide powders simultaneously without high-temperature heating conditions, to obtain modified doped ceramic powder, to make the ceramic powder evenly dispersed and doped in the ceramic slurry, and to obtain a 3D printed ceramic product with excellent performance after 3D printing of the ceramic green body, degreasing and sintering.

[0060] The present invention uses a 3D printer such as a digital light processing printer (DLP) or a stereolithography printer (SLA) to print a ceramic body. For ease of detection, the rectangular parallelepiped ceramic model of the present invention is designed to have a size of 3mm×3mm×50mm. The present invention is further described in detail below in conjunction with an embodiment.

[0061] Example 1

[0062] In this embodiment, the ceramic slurry contains 90 wt% of modified and doped ceramic powder, 10 wt% of photosensitive resin, 2 wt% of the dispersant and 2 wt% of the modified and doped ceramic powder, and 2 wt% of the photoinitiator.

[0063] Both the zirconium oxide powder and the doped oxide powder are spherical powder particles with a particle size of 1 μm, wherein the doped oxide powder is lanthanum oxide powder, samarium oxide powder, cerium oxide powder, and yttrium oxide powder, with a mass ratio of 0.7:7:0.3:5, and the total mass of the doped oxide powder is 13% of the zirconium oxide powder; the modifier is docosyltriethoxysilane and octadecyltrimethoxysilane, and the volume ratio of the two is 1:1;

[0064] Resin A accounts for 70% of the total volume of the photosensitive resin, and is ethoxylated pentaerythritol tetraacrylate and trimethylolpropane triacrylate, and the volume ratio of the two is 1:1;

[0065] Resin B accounts for 30% of the total volume of the photosensitive resin and is 1,6-hexanediol diacrylate;

[0066] The photoinitiator is diphenyl (2,4,6-trimethylbenzoyl) phosphine oxide (TPO); the dispersant A is ethyl acrylate;

[0067] The specific slurry preparation steps are as follows:

[0068] S1 Preparation of modified doped ceramic powder

[0069] Take 100g of zirconium oxide powder and 13wt% of doped oxide powder for later use; put 2.26g of modifier, 25ml of ethanol and 30ml of deionized water into a beaker and fully premix them with an electric stirrer at 410rpm for 15min, then put them into an ultrasonic disperser and disperse them at a power of 50W for 30min to obtain a ceramic powder modifier for later use; measure 350ml of deionized water and put it into a beaker, use a water bath high-speed stirrer to stir for 40min at a water bath temperature of 80°C and a stirring speed of 420rpm, and during the stirring process, gradually add weighed zirconium oxide powder, doped oxide powder and ceramic powder modifier to obtain an oxide powder premix for later use; put the oxide powder premix into a high-energy ball mill and ball mill it in a 1000W microwave environment for 7h, then filter the solution, after the filtration is completed, dry the powder at 90°C for 9h, leave it for aging for 18h, and obtain modified doped ceramic powder after powdering with a powder mill for later use.

[0070] The infrared spectra of the modified doped ceramic powder in this embodiment and the unmodified doped ceramic powder in comparative example 4 are as follows: Fig.11 As shown in Figure 2, compared with the unmodified doped ceramic powder, the infrared spectrum of the modified doped ceramic powder is between 2800 and 3000 cm -1There is a CH stretching vibration absorption valley at 860cm -1 The stretching vibration of Si-O-Zr appeared at the surface, indicating that the silanol formed by the hydrolysis of the modifier reacted with the hydroxyl group on the surface of zirconia to form a Zr-O-Si bond, and the modifier was successfully grafted on the surface of zirconia.

[0071] S2 Preparation of Multi-doped Zirconia Photocurable Ceramic Slurry

[0072] The photosensitive resin, dispersant and photoinitiator are placed in a beaker and premixed with a high-speed stirrer for 10 minutes at a stirring speed of 400 rpm. Next, the modified doped ceramic powder is gradually added to the mixed solution of the photosensitive resin, dispersant and photoinitiator in batches for 4 minutes at a stirring speed of 600 rpm. The powder is then placed in an ultrasonic disperser and dispersed at a power of 110 W for 8 minutes to obtain a multi-element doped zirconia ceramic slurry with a viscosity range of 3500 mPa·s. The slurry is placed in a light-proof bottle and protected from light for later use.

[0073] The multi-element doped zirconia ceramic slurry is used as a raw material to perform 3D printing, including the following specific steps:

[0074] (1) 3D printed ceramic body

[0075] The prepared multi-doped zirconia ceramic slurry was printed with a 3D printer, the light source wavelength was 405nm, and the light source intensity was 150mW / cm 2 , exposure time 3s, obtain 3D printed ceramic body;

[0076] (2) Degreasing and sintering of 3D printed ceramic bodies

[0077] The 3D printed body was placed in a high-temperature oxidation furnace and heated to 190°C at 2°C / min and kept warm for 1.3 hours; heated to 245°C at 2°C / min and kept warm for 1.2 hours; heated to 390°C at 2°C / min and kept warm for 1.2 hours; heated to 460°C at 2°C / min and kept warm for 1.2 hours; heated to 600°C at 2°C / min and kept warm for 2 hours; heated to 1000°C at 5°C / min, kept warm for 30 minutes; then heated to 1450°C at 5°C / min, kept warm for 1 hour; then heated to 1600°C at 5°C / min, kept warm for 2 hours and then cooled naturally to obtain a multi-doped zirconia ceramic product.

[0078] The doping of lanthanum oxide or cerium oxide will increase the Vickers hardness of ceramic parts while reducing the flexural strength of ceramics. The doping of samarium oxide has the opposite performance change. By doping lanthanum oxide and cerium oxide, the transformation of samarium oxide and yttrium oxide doped zirconia ceramics from tetragonal phase to cubic phase can be significantly inhibited under high temperature conditions of 1550℃, thereby producing ceramics with excellent mechanical properties, such as Figure 1 A. Figure 2 As shown, the printed layers of the fired modified doped zirconia ceramics are in close contact, as shown in Figure 3 As shown, the zirconium oxide grains are uniform and small. Fig.10 It can be seen that its Vickers hardness can reach 2015Hv and maintain a relatively excellent flexural strength of 700MPa. The prepared ceramic slurry has excellent rheological properties and light curing properties, high solid content, and can achieve fine printing, such as Fig.12 The printed pentagonal dodecahedron hollow sphere (side length 5mm).

[0079] Example 2

[0080] In this embodiment, in the ceramic slurry, the modified doped ceramic powder is 95wt%; the photosensitive resin is 5wt%; the dispersant is 2wt% of the modified doped ceramic powder; and the photoinitiator is 2wt% of the photosensitive resin.

[0081] Both the zirconium oxide powder and the doped oxide powder are nearly spherical and spherical powder particles with a particle size of 50 nm, wherein the doped oxide powder is lanthanum oxide powder, samarium oxide powder, cerium oxide powder, and yttrium oxide powder, with a mass ratio of 0.7:7:0.3:5, and the total mass of the doped oxide powder is 15% of the zirconium oxide powder; the modifier is n-decyltrimethoxysilane;

[0082] Resin A accounts for 80% of the total volume of the photosensitive resin and is trimethylolpropane triacrylate and dipentaerythritol hexaacrylate, which are mixed in a volume ratio of 1:2;

[0083] Resin B accounts for 20% of the total volume of the photosensitive resin and is a mixture of methyl methacrylate and tripropylene glycol diacrylate in a volume ratio of 1:2;

[0084] The photoinitiator is benzoyl peroxide (BPO); the dispersant B is a mixture of n-heptyl acrylate and hexyl acrylate in a volume ratio of 1:1;

[0085] The specific slurry preparation steps are as follows:

[0086] S1 Preparation of modified doped ceramic powder

[0087] Take 110g of zirconium oxide powder and 15wt% of doped oxide powder for later use; put 2.53g of modifier, 30ml of ethanol (or acetone) and 40ml of deionized water into a beaker, and premix them with an electric stirrer at 420rpm for 20min, then put them into an ultrasonic disperser and disperse them at a power of 60W for 40min to obtain a ceramic powder modifier for later use; measure 500ml of deionized water and put it into a beaker, stir it with a water bath high-speed stirrer at a water bath temperature of 80°C and a stirring speed of 430rpm for 50min, and during the stirring process, gradually add the weighed zirconium oxide powder, doped oxide powder and ceramic powder modifier to obtain an oxide powder premix for later use. The oxide powder premix is ​​placed in a high-energy ball mill and ball-milled in a 1200W microwave environment for 8 hours. The solution is then filtered. After the filtration is completed, the powder is dried at 100°C for 10 hours, aged for 20 hours, and pulverized by a powder grinder to obtain modified doped ceramic powder for use.

[0088] S2 Preparation of Multi-doped Zirconia Photocurable Ceramic Slurry

[0089] The photosensitive resin, dispersant and photoinitiator were placed in a beaker and premixed with a high-speed stirrer, and the mixing time was 15 minutes at a stirring speed of 450rpm; next, the modified doped ceramic powder was gradually added to the mixed solution of the photosensitive resin, dispersant and photoinitiator in batches, and the stirring time was 5 minutes at a stirring speed of 650rpm, and then placed in an ultrasonic disperser and dispersed at a power of 150W for 10 minutes to obtain a multi-element doped zirconia ceramic slurry with a viscosity of 5000mPa·s, which was placed in a light-shielding bottle and stored away from light for later use;

[0090] The multi-element doped zirconia ceramic slurry is used as a raw material to perform 3D printing, including the following specific steps:

[0091] (1) 3D printed ceramic body

[0092] The prepared multi-doped zirconia ceramic slurry was printed with a 3D printer, the light source wavelength was 405nm, and the light source intensity was 50mW / cm 2 , exposure time 5s, to obtain 3D printed ceramic body;

[0093] (2) Degreasing and sintering of 3D printed ceramic bodies

[0094] The 3D printed body was placed in a high-temperature oxidation furnace and heated to 200°C at 3°C / min and kept warm for 1.5 hours; heated to 250°C at 3°C / min and kept warm for 1.5 hours; heated to 400°C at 3°C / min and kept warm for 1.5 hours; heated to 470°C at 3°C / min and kept warm for 1.5 hours; heated to 610°C at 3°C / min and kept warm for 2.5 hours; heated to 1000°C at 7°C / min, kept warm for 40 minutes; then heated to 1450°C at 7°C / min, kept warm for 1.2 hours; then heated to 1650°C at 7°C / min, kept warm for 2.5 hours and then cooled naturally to obtain a multi-doped zirconia ceramic product.

[0095] Compared with Example 1, this embodiment has a finer powder particle size and a higher solid content, so that the green body forms fewer structural defects during the degreasing and sintering process, and the sample density and mechanical properties are more excellent. Figure 4 As shown in Figure 2, the structure of multi-doped zirconia ceramics is more compact. Fig.10 It can be seen that its Vickers hardness can reach 2068Hv and maintain an excellent flexural strength of 750MPa.

[0096] Example 3

[0097] In this embodiment, the ceramic slurry contains 75wt% of modified and doped ceramic powder, 25wt% of photosensitive resin, 2wt% of dispersant and 2wt% of modified and doped ceramic powder, and 2wt% of photoinitiator to the photosensitive resin.

[0098] Both the zirconium oxide powder and the doped oxide powder are nearly spherical and spherical powder particles with a particle size of 10 μm, wherein the doped oxide powder is lanthanum oxide powder, samarium oxide powder, cerium oxide powder, and yttrium oxide powder, and the mass ratio is 0.7:7:0.3:5, and the total mass of the doped oxide powder is 8% of the zirconium oxide powder; the modifier is dodecyltriethoxysilane;

[0099] Resin A accounts for 60% of the total volume of the photosensitive resin and is ethoxylated pentaerythritol tetraacrylate;

[0100] Resin B accounts for 40% of the total volume of the photosensitive resin and is a mixture of isobornyl acrylate, 1,6-hexanediol diacrylate (HDDA), and dipropylene glycol diacrylate in a volume ratio of 1:1:2;

[0101] The photoinitiator was phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide (Omnirad 819); dispersant B was butyl acrylate and pentyl acrylate, mixed in a volume ratio of 1:1:1;

[0102] The specific slurry preparation steps are as follows:

[0103] S1 Preparation of modified doped ceramic powder

[0104] Take 90g of zirconium oxide powder and 8wt% of doped oxide powder for standby use; put 1.94g of modifier, 15ml of acetone and 20ml of deionized water into a beaker and premix them with an electric stirrer at 400rpm for 10min, then put them into an ultrasonic disperser and disperse them at 30W for 20min to obtain a ceramic powder modifier for standby use; measure 200ml of deionized water and put it into a beaker, stir it with a water bath high-speed stirrer at a water bath temperature of 80℃ and a stirring speed of 400rpm for 30min, and gradually add weighed zirconium oxide powder, doped oxide powder and ceramic powder modifier during the stirring process to obtain an oxide powder premix for standby use. Put the oxide powder premix into a high-energy ball mill and ball mill it in an 800W microwave environment for 6h, then filter the solution, dry the powder at 80℃ for 8h after filtration, place it for aging for 15h, and obtain modified doped ceramic powder after powdering it with a powder mill for standby use.

[0105] S3 Preparation of Multi-doped Zirconia Photocurable Ceramic Slurry

[0106] The photosensitive resin, dispersant and photoinitiator were placed in a beaker and premixed with a high-speed stirrer, with a mixing time of 5 minutes and a stirring speed of 350 rpm; next, the modified doped ceramic powder was gradually added to the mixed solution of the photosensitive resin, dispersant and photoinitiator in batches, with a stirring time of 3 minutes and a stirring speed of 550 rpm, and then placed in an ultrasonic disperser and dispersed at a power of 100 W for 5 minutes to obtain a multi-element doped zirconia ceramic slurry with a viscosity of 2000 mPa·s, which was placed in a light-shielding bottle and stored away from light for later use;

[0107] The multi-element doped zirconia ceramic slurry is used as a raw material to perform 3D printing, including the following specific steps:

[0108] (1) 3D printed ceramic body

[0109] The prepared multi-doped zirconia ceramic slurry was printed with a 3D printer, the light source wavelength was 405nm, and the light source intensity was 200mW / cm 2 , exposure time 4s, to obtain 3D printed ceramic body;

[0110] (2) Degreasing and sintering of 3D printed ceramic bodies

[0111] The 3D printed body was placed in a high-temperature oxidation furnace and heated to 180°C at 1°C / min and kept warm for 1h; heated to 240°C at 1°C / min and kept warm for 1h; heated to 380°C at 1°C / min and kept warm for 1h; heated to 450°C at 1°C / min and kept warm for 1h; heated to 590°C at 1°C / min and kept warm for 1.5h; heated to 1000°C at 3°C / min, kept warm for 20min; then heated to 1450°C at 3°C / min, kept warm for 0.8h; then heated to 1550°C at 3°C / min, kept warm for 1.5h, and then cooled naturally to obtain a multi-doped zirconia ceramic product.

[0112] Due to the relatively low solid content, the green body shrinkage during sintering is greater than that of Examples 1 and 2. Figure 5 As shown, the printed interlayer bonding surface is also clearer than that of Examples 1 and 2, and the mechanical properties of the obtained zirconia ceramic are lower than those of Example 1. Fig.10 It can be seen that its Vickers hardness is 1910Hv and its flexural strength is 600MPa.

[0113] Comparative Example 1

[0114] In this comparative example, in step S1 for preparing modified doped ceramic powder, the microwave power used is 700 W, and the ball milling time is 5 h. In step S2 for preparing multi-element doped zirconia photocured ceramic slurry, the ultrasonic power used is 90 W, and the dispersion time is 4 min. The other conditions are the same as those in Example 1.

[0115] Although the method of "composite modification-multi-element co-doping" was adopted, the mechanical crushing degree of the oxide powder was limited, the surface activity was insufficiently enhanced, and the modification process was not fully carried out due to the low microwave power and short ball milling time. At the same time, in the process of preparing multi-element doped zirconia ceramic slurry, the ultrasonic disperser also had low power and short dispersion time, which resulted in the inability of the dispersant molecules to be evenly filled and dispersed between the powder particles and the resin molecules, and partially bridged with the alkane chain of the modifier, reducing its lubrication effect between the long chains of the macromolecular modifier in space steric hindrance, and failing to effectively disperse the powder particles. Due to the high powder content and low solvent resin, the powder dispersibility in the ceramic slurry was poor, and agglomerated particles appeared in the slurry. The slurry viscosity reached 6200mPa·s, affecting the printing process. The green body failed to successfully print the target length, and after firing, the following problems occurred: Figure 1 B, and Figure 6 The contact surface between the printed layers of the ceramic surface is obvious, and clear grooves between the surfaces appear, and its mechanical properties deteriorate. Fig.10 As shown, its Vickers hardness is 1840Hv and its flexural strength is 500MPa.

[0116] Comparative Example 2

[0117] In this comparative example, in step S2 of preparing multi-doped zirconium oxide photocurable ceramic slurry, no dispersant B is added, and the other conditions are the same as those of the method in Example 2.

[0118] Due to the lack of the "chain extension and solubilization" synergistic dispersion of dispersant B, the surface-modified steric long chains of the powder in the slurry will further undergo bridging to form agglomerates, and the slurry solid content is high, resulting in an increase in the slurry viscosity, which exceeds 10000mPa·s. Due to the high slurry viscosity, it is impossible to prepare a multi-doped zirconia ceramic slurry that can be used for printing.

[0119] Comparative Example 3

[0120] In this comparative example, in step S1 for preparing modified doped ceramic powder, the microwave power used is 1300 W, and the ball milling time is 9 h. In step S2 for preparing multi-element doped zirconia photocured ceramic slurry, the ultrasonic power used is 160 W, and the dispersion time is 11 min. The other conditions are the same as those in Example 2.

[0121] In the process of preparing modified doped ceramic powders, due to excessive microwave power and long ball milling time, the oxide powders undergo intense thermal motion and strong agglomeration, and the modifier undergoes a large amount of self-polymerization reaction, resulting in a decrease in the modification effect. The modifier cannot form a long-lasting, stable, and fully grafted steric hindrance coating layer on the surface of the metal oxide doped ceramic powders, and the coating layer cannot form an effective "steric barrier" on the outer space of the metal oxide doped ceramic powders.

[0122] In the process of preparing multi-doped zirconia ceramic slurry, the ultrasonic disperser also has too high power and long dispersion time, which leads to the destruction of the bridging effect formed by the dispersant molecules and the modifier alkane chains, making it difficult to form grafted steric chains on the surface of the ceramic powder, and unable to effectively achieve the "chain extension and solubilization" synergistic dispersion effect. After the preparation process, the modified steric long chains on the surface of the powder in the slurry will further undergo bridging to form agglomerations, resulting in an increase in the slurry viscosity. The slurry viscosity reaches 7300mPa·s, which seriously affects the printing process and eventually appears. Figure 1 The printed body shown in sample C is bent, and Figure 7 The serious cracking phenomenon between the ceramic layers and its mechanical properties are extremely poor, such as Fig.10 As shown, its Vickers hardness is 1860Hv. Since there are many nearly penetrating cracks in the ceramic rod, its flexural strength is too low to be measured using an instrument.

[0123] Comparative Example 4

[0124] In this comparative example, no modifier is added in step S1 to prepare unmodified doped ceramic powder. The infrared spectrum of the ceramic powder is as follows: Fig.11 As shown in a, the remaining conditions are the same as those in Example 2.

[0125] Due to the lack of modifiers, the dispersant cannot achieve the "chain extension and solubilization" synergistic dispersion of the metal oxide-doped ceramic powder in the slurry, and the slurry solid content is high, resulting in a high overall viscosity of the slurry that cannot meet the printing conditions. Due to the excessive viscosity of the slurry, the viscosity of the slurry reached 8800mPa·s, and it was impossible to prepare a multi-doped zirconia ceramic slurry that can be used for printing.

[0126] Comparative Example 5

[0127] In this comparative example, the amount of modifier used in the step S1 for preparing the modified doped ceramic powder is 3.89 g, that is, the amount of modifier is 4 wt % of the metal oxide doped ceramic powder; the amount of dispersant used in the step S2 for preparing the multi-doped zirconia photocured ceramic slurry is 1 wt % of the modified doped ceramic powder; and the other conditions are the same as those in Example 3.

[0128] During the modification process, the excess modifier will bridge the powder surface coating, resulting in flocculation and agglomeration between the powder particles; during the slurry preparation process, the dispersant content is low, and it is unable to fully graft with the long-chain alkane of the ceramic powder surface coating, resulting in fewer grafted steric chains and reduced steric hindrance enhancement effects, which significantly reduces the "chain extension and solubilization" synergistic dispersion effect, resulting in an increase in the slurry viscosity of 5800mPa·s, and powder agglomeration, such as Figure 8 The surface depressions between the printed layers are large and have certain cracking phenomena, and their mechanical properties are poor. Fig.10 As shown, its Vickers hardness is 1880Hv and its flexural strength is 360MPa.

[0129] Comparative Example 6

[0130] In this comparative example, the doped oxide powders used in the step S1 of preparing the modified doped ceramic powder are lanthanum oxide powder and cerium oxide powder, with a mass ratio of 7:3, and the other conditions are the same as those of the method in Example 3.

[0131] The doping of lanthanum oxide powder and cerium oxide powder has a certain effect on the grain refinement of zirconia ceramics, and can prevent the transformation of zirconia ceramics from tetragonal phase to monoclinic phase at low temperature, thereby further enhancing the Vickers hardness of zirconia ceramics, but it cannot effectively eliminate cracks, such as Fig. 9 As shown. Cracks lead to a decrease in the flexural strength and hardness of ceramics, such as Fig.10 As shown, its Vickers hardness is 1730Hv and its flexural strength is 540MPa.

Claims

1. A multi-element doped zirconium oxide light-cured ceramic slurry, characterized in that: The photocurable ceramic slurry is composed of modified doped ceramic powder, photosensitive resin, dispersant and photoinitiator; the modified doped ceramic powder is composed of metal oxide doped ceramic powder and modifier, the metal oxide doped ceramic powder includes zirconium oxide powder and doped oxide powder, and the doped oxide powder includes a mixture of yttrium oxide powder, samarium oxide powder, cerium oxide powder and lanthanum oxide powder.

2. The multi-element doped zirconium oxide light-cured ceramic slurry according to claim 1, characterized in that: The modifier forms a three-dimensional coating layer on the surface of the metal oxide-doped ceramic powder, a part of the dispersant is filled between the modified powder particles and the resin molecules, and the other part forms a bridge with the steric hindrance chain of the modifier.

3. The multi-element doped zirconium oxide light-cured ceramic slurry according to claim 1, characterized in that: The amount of each material in the photocurable ceramic slurry is as follows: 75wt%-95wt% of modified doped ceramic powder, 5wt%-25wt% of photosensitive resin, and the total amount of the two is 100%; the dispersant is 2wt% of the modified doped ceramic powder, the photoinitiator is 2wt% of the photosensitive resin, and the modifier is 2wt% of the metal oxide doped ceramic powder.

4. The multi-element doped zirconium oxide light-cured ceramic slurry according to claim 1, characterized in that: The metal oxide doped ceramic powder is a nearly spherical or spherical powder particle with a particle size of 50 nm-10 μm; the doped oxide powder is 8wt% to 15wt% of the zirconium oxide powder; the mass ratio of lanthanum oxide powder, samarium oxide powder, cerium oxide powder and yttrium oxide powder in the doped oxide powder is 0.7:7:0.3:

5.

5. The multi-doped zirconium oxide light-cured ceramic slurry according to claim 1, characterized in that: The modifier is a silane coupling agent, including any one of n-decyltrimethoxysilane, dodecyltriethoxysilane, octadecyltrimethoxysilane, and docosyltriethoxysilane, or a mixture of several of them in any proportion; The photoinitiator includes any one of diphenyl (2,4,6-trimethylbenzoyl) phosphine oxide, benzoyl peroxide, and phenyl bis (2,4,6-trimethylbenzoyl) phosphine oxide; The dispersant is an acrylate compound containing an alkane chain, including dispersant A or dispersant B; the dispersant A includes any one of methyl acrylate, ethyl acrylate, and propyl acrylate, or a mixture of several of them in any proportion; the dispersant B includes any one of butyl acrylate, pentyl acrylate, hexyl acrylate, and n-heptyl acrylate, or a mixture of several of them in any proportion.

6. The multi-element doped zirconium oxide light-cured ceramic slurry according to claim 1, characterized in that: The photosensitive resin is an acrylic resin, including resin A and resin B, wherein resin A accounts for 60-80% of the total volume of the photosensitive resin, and resin B accounts for 20-40% of the total volume of the photosensitive resin; Resin A includes any one of trimethylolpropane triacrylate, ethoxylated pentaerythritol tetraacrylate, and dipentaerythritol hexaacrylate, or a mixture of several of them in any proportion; Resin B includes any one of methyl methacrylate, 1,6-hexanediol diacrylate, isobornyl acrylate, dipropylene glycol diacrylate, and tripropylene glycol diacrylate, or a mixture of several of them in any proportion.

7. A method for preparing a multinary doped zirconium oxide light-cured ceramic slurry, characterized in that: The photocurable ceramic slurry is composed of the photocurable ceramic slurry according to any one of claims 1 to 6, and the preparation method comprises the following steps: S1 Preparation of modified doped ceramic powder The zirconium oxide powder, the doped oxide powder and the modifier are mixed, and the mixed powder is ball-milled in a microwave environment of 800-1200 W for 6-8 hours to obtain a modified doped ceramic powder; S2 Preparation of Multi-Doped Zirconia Photocurable Ceramic Slurry The modified doped ceramic powder, photosensitive resin, dispersant and photoinitiator are ultrasonically dispersed at 100-150W for 5-10 minutes under stirring conditions to mix the materials evenly to obtain multi-doped zirconia photocurable ceramic slurry.

8. The method for preparing a multi-element doped zirconium oxide light-cured ceramic slurry according to claim 7, characterized in that: The specific steps include: S1 Preparation of modified doped ceramic powder Take 90-110g of zirconium oxide powder and 8-15wt% of doped oxide powder of zirconium oxide powder for later use; 1.8-2.2 g of modifier, 15-30 ml of ethanol or acetone, and 20-40 ml of deionized water are fully premixed at 400-420 rpm for 10-20 min, and then ultrasonically dispersed at 30-60 W for 20-40 min to obtain a ceramic powder modifier for later use; Measure 200-500 ml of deionized water, gradually add weighed zirconium oxide powder and doped oxide powder during stirring, then add ceramic powder modifier, stir for 30-50 min at a water bath temperature of 80° C. and a stirring speed of 400-430 rpm to prepare an oxide powder premix for standby use; The oxide powder premix is ​​ball-milled in a microwave environment at 800-1200W for 6-8h, filtered to obtain filtered powder, dried at 80-100°C for 8-10h, aged for 15-20h, and pulverized by a pulverizer to obtain modified doped ceramic powder for later use; S2 Preparation of Multi-Doped Zirconia Photocurable Ceramic Slurry Premix the photosensitive resin, dispersant and photoinitiator for 5 to 15 minutes at a stirring speed of 350 to 450 rpm; The modified doped ceramic powder is gradually added to the photosensitive resin, dispersant and photoinitiator premix in batches, with a stirring time of 3 to 5 minutes and a stirring speed of 550 to 650 rpm, and then ultrasonically dispersed at 100 to 150 W for 5 to 10 minutes to obtain the multi-doped zirconia photocurable ceramic slurry of the present invention, with a viscosity ranging from 2000 to 5000 mPa·s.

9. An application of a multi-element doped zirconium oxide light-cured ceramic slurry, characterized in that: The ceramic slurry is prepared by the method according to any one of claims 7 or 8, and the application comprises the following steps: (1) 3D printed ceramic body The multi-doped zirconium oxide light-cured ceramic slurry was printed with a 3D printer, the light source wavelength was 405nm, and the light source intensity was 10-280mW / cm 2 , exposure time 2 to 10 s, to obtain a 3D printed ceramic body; (2) Degreasing and sintering of 3D printed ceramic bodies The 3D printed ceramic body is placed in an oxidation furnace and heated to 180-200°C at 1-3°C / min and kept warm for 1-1.5h; heated to 240-250°C at 1-3°C / min and kept warm for 1-1.5h; heated to 380-400°C at 1-3°C / min and kept warm for 1-1.5h; heated to 450-470°C at 1-3°C / min and kept warm for 1-1.5h; heated to 1-3°C / min and kept warm for 1-1.5h; heated to 240-250°C at 1-3°C / min and kept warm for 1-1.5h; heated to 380-400°C at 1-3°C / min and kept warm for 1-1.5h; heated to 450-470°C at 1-3°C / min The method comprises heating the temperature to 590-610°C at 3-7°C / min and keeping the temperature for 1.5-2.5h; heating the temperature to 1000°C at 3-7°C / min and keeping the temperature for 20-40min; then heating the temperature to 1450°C at 3-7°C / min and keeping the temperature for 0.8-1.2h; then heating the temperature to 1550-1650°C at 3-7°C / min, keeping the temperature for 1.5-2.5h and then cooling the temperature naturally to obtain a multinary doped zirconia ceramic product.

10. An application of a multi-element doped zirconium oxide light-cured ceramic slurry, characterized in that: The ceramic slurry is composed of the ceramic slurry described in any one of claims 1 to 6, and the application fields of the ceramic product prepared by the ceramic slurry include biomedicine, aerospace, and automobile manufacturing.

Citation Information

Patent Citations

  • Process for preparing superfine tungsten-base alloy powder by microwave-assisted ball-milling

    CN103521763A

  • Yttria-stabilized zirconia powder and preparation method thereof

    CN103708831A

  • Preparation method of microwave dielectric ceramic material

    CN103864420A

  • Ceramic slurry for DLP (Digital Light Processing) additive manufacturing and preparation method thereof, and method for preparing finished product by adopting slurry

    CN109133917A

  • 3D printing colored zirconia ceramic slurry as well as preparation method and application thereof

    CN117285349A