Preparation method of lanthanum calcium manganese oxide and metal platinum multiphase composite ceramic material

The sol-gel method and solid-phase method are combined to prepare lanthanum calcium, manganese oxygen and metal platinum composite ceramics, which solves the problem of insufficient resistance temperature coefficient and magnetoresistance value of existing materials, and achieves the application improvement in the fields of temperature detection and magnetic storage. It also simplifies the process flow and is suitable for mass production.

CN118993734AActive Publication Date: 2024-11-22KUNMING UNIV OF SCI & TECH
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411184923.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-11-22
Estimated Expiration
2044-08-27

AI Technical Summary

Technical Problem

The application of existing rare earth manganate materials in the fields of temperature detection and magnetic storage is limited by the low resistance temperature coefficient and magnetoresistance value, and the preparation process is complicated and difficult to produce on a large scale.

Method used

The sol-gel method and solid phase method are combined to prepare the multi-phase composite ceramic materials of lanthanum calcium, manganese and metal platinum. Through precise control of stoichiometric ratio and multi-step process processing, La1-xCaxMnO3: Pty composite ceramics are formed to ensure that The transition temperature of the metal-insulator is close to room temperature, which increases the resistance temperature coefficient and magneto-resistance.

Benefits of technology

The resistance temperature coefficient and magnetoresistance value of the material are significantly improved, the application potential in the fields of temperature detection and magnetic storage is enhanced, the preparation process is simplified, and the production repeatability and efficiency are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118993734A_ABST
    Figure CN118993734A_ABST
Patent Text Reader

Abstract

The invention belongs to the field of functional ceramics, and relates to a preparation method of a lanthanum-calcium-manganese-oxygen and metal platinum multiphase composite ceramic material, which comprises the following specific steps: by taking lanthanum nitrate hexahydrate, calcium nitrate tetrahydrate and manganese nitrate tetrahydrate as raw materials, citric acid monohydrate as a chelating agent and methanol as a solvent, stirring and dissolving, adding and mixing by taking ethylene glycol as a dispersing agent, and uniformly stirring; stirring and heating the mixed solution, drying to obtain dry gel, grinding and calcining the dry gel to obtain precursor powder, uniformly mixing the precursor powder with platinum powder, pressing, and calcining to obtain the La1-xCaxMnO3: Pty composite ceramic block material. The metal-insulator transition temperature of the La1-xCaxMnO3: Pty composite ceramic prepared by the method is kept in a range close to room temperature, the resistivity is reduced, the resistance temperature coefficient and the magnetoresistance are remarkably improved, and the application possibility of the La1-xCaxMnO3: Pty composite ceramic in the fields of temperature detection, magnetic storage and the like is greatly improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a preparation method of a lanthanum calcium manganese oxygen and metal platinum multiphase composite ceramic material, belonging to the technical field of functional ceramics. Background Art

[0002] Rare earth manganate La with perovskite structure 1-x Ca x The metal-insulator transition temperature of MnO3 is close to room temperature, and the drastic resistivity change near the metal-insulator transition temperature leads to a higher temperature coefficient of resistance. These peculiar physical phenomena make this type of material have potential application value in the fields of temperature detection and thermal imaging. In addition, the colossal magnetoresistance effect near the metal-insulator transition temperature makes this type of material have potential application scenarios in the fields of magnetic storage and magnetic detection. The temperature coefficient of resistance (TCR), metal-insulator transition temperature (TMI) and magnetoresistance (MR) are important parameters that determine whether the material can achieve the above application scenarios. TMI determines the temperature range of the material's application. Generally, the closer to room temperature, the more conducive to its application. High TCR values ​​and MR can improve detection sensitivity, and also determine the possibility of its application. Summary of the invention

[0003] In order to solve the defects in the prior art, the present invention provides a method for preparing a lanthanum calcium manganese oxide and metal platinum multiphase composite ceramic material. The sol-gel method and the solid phase method are combined to prepare the lanthanum calcium manganese oxide and metal platinum composite ceramic material, which greatly improves the possibility of applying rare earth manganate ceramics in the fields of temperature detection and magnetic storage.

[0004] A method for preparing a lanthanum calcium manganese oxide and metal platinum multiphase composite ceramic material designed to achieve the above purpose comprises the following steps: (1) Weighing lanthanum nitrate hexahydrate, calcium nitrate tetrahydrate, and manganese nitrate tetrahydrate raw materials according to the stoichiometric ratio, adding citric acid as a complexing agent, ethylene glycol as a dispersant, and methanol as a solvent, and mixing all the mixed raw materials uniformly; (2) placing the mixed solution obtained in step (1) in a magnetic stirrer and stirring the mixture evenly, and heating the mixture to perform a foaming reaction until a viscous, transparent, and precipitate-free wet gel is obtained; (3) placing the wet gel obtained in step (2) in an oven and drying for 8-12 h to obtain a loose dry gel without precipitation; (4) Grinding the dry gel formed in step (3) into powder in an agate mortar, and calcining in a muffle furnace under normal pressure and air atmosphere to obtain a precursor powder; (5) using a solid phase method, mixing the precursor powder obtained in step (4) with platinum powder in a certain stoichiometric ratio in an agate mortar and grinding them thoroughly to obtain a mixed powder; (6) The mixed powder obtained in step (5) is pressed into a block in an automatic tablet press, and then finally sintered in a muffle furnace to obtain La 1-x Ca x MnO3:Pt y Composite ceramic blocks.

[0005] Furthermore, the purity of all raw materials in step (1) is not less than 99.9%, and the raw material weighing error is controlled within ±0.05 mg; Further optimization, the chemical formula of the Ag-doped nickelate composite ceramic target prepared in step (6) is La 1- x Ca x MnO3:Pt y , where 0< x ≤ 0.4,0.05 ≤ y ≤ 0.2.

[0006] Furthermore, in step (2), when the mixed solution is heated and stirred, the temperature of the magnetic stirrer is set to 70-100° C., and the stirring speed is 300 r / min. No precipitate is present after the foaming is completed.

[0007] Furthermore, in step (3), the wet gel is dried under normal pressure and air atmosphere, and the oven temperature is set at 100-180°C.

[0008] Furthermore, the grinding time in step (4) is 0.5-1 h, the calcination temperature is 400-700 °C in an air atmosphere, and the sintering and heat preservation time is 5-10 h.

[0009] Furthermore, the grinding time in step (5) is 1-2 h.

[0010] Furthermore, in step (6), the setting parameters of the automatic tablet press are 3-6 Mpa, the duration is about 20-30 min, the sintering temperature is 1400-1550 °C under normal pressure and air atmosphere, and the insulation time is 10-16 h.

[0011] The beneficial effects of the present invention are: The present invention uses a sol-gel method and a solid phase method to prepare La 1-x Ca x MnO3:Pt y Multiphase composite ceramics keep the metal-insulator transition temperature close to room temperature, which reduces the resistivity of the material, significantly improves the temperature coefficient of resistance and magnetoresistance, and greatly increases the possibility of applying rare earth manganate composite ceramics in temperature detection and magnetic storage.

[0012] La prepared by the method of the present invention 1-x Cax MnO3:Pt y The maximum TCR of the composite ceramic is as high as 52.6% / K at 266.3K, and the resistance in an applied magnetic field of 1T is as high as 80.7% at 269K. The method of the invention has a simple preparation process, a short cycle, and high repeatability, and can be used for mass production. BRIEF DESCRIPTION OF THE DRAWINGS

[0013] Figure 1 The La obtained in Comparative Example 1 of the present invention 0.67 Ca 0.33 Resistivity-temperature measurement curve of MnO3 ceramic target; Figure 2 The La obtained in Comparative Example 1 of the present invention 0.67 Ca 0.33 TCR-T measurement curve of MnO3 ceramic target; Figure 3 The La obtained in Comparative Example 1 of the present invention 0.67 Ca 0.33 MR-T measurement curve of MnO3 ceramic target; Figure 4 La obtained in Example 2 of the present invention 0.67 Ca 0.33 MnO3:Pt 0.05 Resistivity-temperature measurement curve of composite ceramic target; Figure 5 La obtained in Example 2 of the present invention 0.67 Ca 0.33 MnO3:Pt 0.05 TCR-T measurement curve of composite ceramic target; Figure 6 La obtained in Example 2 of the present invention 0.67 Ca 0.33 MnO3:Pt 0.05 MR-T measurement curve of composite ceramic target; Figure 7 The La obtained in Example 1 of the present invention 0.67 Ca 0.33 MnO3:Pt 0.10 Resistivity-temperature measurement curve of composite ceramic target; Figure 8 The La obtained in Example 1 of the present invention 0.67 Ca 0.33 MnO3:Pt 0.10 TCR-T measurement curve of composite ceramic target; Fig. 9 The La obtained in Example 1 of the present invention 0.67 Ca 0.33 MnO3:Pt0.10 MR-T measurement curve of composite ceramic target; Fig.10 The La obtained in Example 3 of the present invention 0.67 Ca 0.33 MnO3:Pt 0.15 Resistivity-temperature measurement curve of composite ceramic target; Fig.11 The La obtained in Example 3 of the present invention 0.67 Ca 0.33 MnO3:Pt 0.15 TCR-T measurement curve of composite ceramic target; Fig.12 The La obtained in Example 3 of the present invention 0.67 Ca 0.33 MnO3:Pt 0.15 MR-T measurement curve of composite ceramic target; DETAILED DESCRIPTION

[0014] In order to make the purpose, technical solution and advantages of the embodiments of the present application clearer, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.

[0015] Example 1 The preparation method of a lanthanum calcium manganese oxide and metal platinum multiphase composite ceramic material of the present embodiment specifically comprises the following steps: (1) Weighing lanthanum nitrate hexahydrate, calcium nitrate tetrahydrate, and manganese nitrate tetrahydrate with a purity of not less than 99.9% according to the stoichiometric ratio of cations in the chemical formula, using citric acid monohydrate as a complexing agent and methanol as a solvent, and stirring the weighed raw materials on a magnetic stirrer at room temperature to completely dissolve them, and controlling the weighing error within ±0.5 mg; (2) Ethylene glycol is used as a dispersant. After the raw materials in step (1) are completely dissolved, ethylene glycol is added to the mixed solution to allow it to be fully mixed with the solution, wherein the molar ratio of lanthanum calcium manganese oxide to ethylene glycol is 1:2; (3) After the mixed solution in step (2) is fully mixed, the solution is transferred to a magnetic heating stirrer at 88°C for heating and stirring. When the solution turns dark yellow and foaming is observed, the mixed solution is transferred to a 140°C constant temperature oven for full foaming and drying for 12 h to obtain a dry gel.

[0016] (4) The dry gel in step (3) was placed in an agate mortar and ground for 0.7 h. The ground powder was placed in a muffle furnace and calcined at 500 °C for 8 h to remove organic matter and nitrate ions in the gel, thereby obtaining a black precursor powder. (5) mixing the lanthanum calcium manganese oxide precursor powder obtained in step (4) with platinum powder in a certain stoichiometric ratio in an agate mortar and grinding for 1.5 h to obtain a mixed precursor powder; (6) The mixed precursor powder obtained in step (5) was pressed into a block in an automatic tablet press at a pressing pressure of 5 MPa for 20 min, and then placed in a muffle furnace and sintered at 1450 °C for 12 h to obtain La 1-x Ca x MnO3:Pt y Composite ceramic block of composite ceramic, wherein x = 0.33, y=0.05.

[0017] The lanthanum calcium manganese oxide and metal platinum multiphase composite ceramic La obtained in Example 1 0.67 Ca 0.33 MnO3:Pt 0.05 , see Figure 4 , 5 , 6. At 265.2 K, the TCR is 51.2% / K, and the maximum MR is 78.3% at 1 T magnetic field.

[0018] Comparative Example 1 The preparation method of a lanthanum calcium manganese oxide ceramic material of the present embodiment specifically comprises the following steps: (1) Preparation of La by combining sol-gel method and solid phase method 0.67 Ca 0.33 MnO3 ceramic target material, lanthanum nitrate hexahydrate, calcium nitrate tetrahydrate, and manganese nitrate tetrahydrate with a purity of not less than 99.9% are weighed according to the stoichiometric ratio of cations in the chemical formula, citric acid monohydrate is used as a complexing agent, methanol is used as a solvent, and the weighed raw materials are stirred on a magnetic stirrer at room temperature to completely dissolve them, and the weighing error is controlled within ±0.5 mg; (2) Ethylene glycol is used as a dispersant. After the raw materials in step (1) are completely dissolved, ethylene glycol is added to the mixed solution to allow it to be fully mixed with the solution, wherein the molar ratio of lanthanum calcium manganese oxide to ethylene glycol is 1:2; (3) After the mixed solution in step (2) is fully mixed, the solution is transferred to a magnetic heating stirrer at 88°C for heating and stirring. When the solution turns dark yellow and foaming is observed, the mixed solution is transferred to a constant temperature oven at 140°C for full foaming and drying for 12 h to obtain a dry gel.

[0019] (4) The dry gel in step (3) was placed in an agate mortar and ground for 0.7 h. The ground powder was placed in a muffle furnace and calcined at 500 °C for 8 h to remove organic matter and nitrate ions in the gel, thereby obtaining a black precursor powder. (5) The mixed precursor powder obtained in step (4) was pressed into a block in an automatic tablet press at a pressing pressure of 5 MPa for 20 min, and then placed in a muffle furnace and sintered at 1450 °C for 12 h to obtain La 0.67 Ca 0.33 MnO3 polycrystalline ceramics.

[0020] The La obtained in this comparative example 1 0.67 Ca 0.33 MnO3, see Figure 1 , 2 , 3. At 259.4 K, the TCR is 40.1% / K, and the maximum MR is 60.3% at 1 T magnetic field.

[0021] Example 2 In this embodiment, La 1-x Ca x MnO3:Pt y of x = 0.33, y = 0.1, and other step parameters are the same as those in Example 1.

[0022] The lanthanum calcium manganese oxide and metal platinum multiphase composite ceramic La obtained in Example 2 0.67 Ca 0.33 MnO3:Pt 0.1 ,See Figure 7 , 8 , 9, at 266.3 K, the TCR is 52.6% / K, and the maximum MR value is 80.7% under 1 T magnetic field.

[0023] Example 3 In this embodiment, La 1-x Ca x MnO3:Pt y of x = 0.33, y = 0.15, and other step parameters are the same as those in Example 1.

[0024] The La obtained in Example 3 0.67 Ca 0.33 MnO3:Pt 0.15 , see Figure 4 , 5 , 6. At 266.4 K, the TCR is 52.8% / K, and the maximum MR is 80.0% at 1 T magnetic field.

[0025] Example 4 The preparation method of a lanthanum calcium manganese oxide and metal platinum multiphase composite ceramic material of the present embodiment specifically comprises the following steps: (1) Weighing lanthanum nitrate hexahydrate, calcium nitrate tetrahydrate, and manganese nitrate tetrahydrate with a purity of not less than 99.9% according to the stoichiometric ratio of cations in the chemical formula, using citric acid monohydrate as a complexing agent and methanol as a solvent, and stirring the weighed raw materials on a magnetic stirrer at room temperature to completely dissolve them, and controlling the weighing error within ±0.5 mg; (2) Ethylene glycol is used as a dispersant. After the raw materials in step (1) are completely dissolved, ethylene glycol is added to the mixed solution to allow it to be fully mixed with the solution, wherein the molar ratio of lanthanum calcium manganese oxide to ethylene glycol is 1:2; (3) After the mixed solution in step (2) is fully mixed, the solution is transferred to a 70°C magnetic heating stirrer for heating and stirring. When the solution turns dark yellow and foaming is observed, the mixed solution is transferred to a 100°C constant temperature oven for full foaming and drying for 14 hours to obtain a dry gel.

[0026] (4) The dry gel in step (3) was placed in an agate mortar and ground for 0.5 h. The ground powder was placed in a muffle furnace and calcined at 400 °C for 10 h to remove organic matter and nitrate ions in the gel, thereby obtaining a black precursor powder. (5) mixing the lanthanum calcium manganese oxide precursor powder obtained in step (4) with platinum powder in a certain stoichiometric ratio in an agate mortar and grinding for 1 h to obtain a mixed precursor powder; (6) The mixed precursor powder obtained in step (5) was pressed into a block in an automatic tablet press at a pressure of 3 MPa for 20 min and then placed in a muffle furnace for sintering at 1400 °C for 10 h. x = 0.33, y = 0.05 to obtain the composite ceramic La 0.67 Ca 0.33 MnO3:Pt 0.05 Composite ceramic blocks.

[0027] Example 5 The method for preparing a Ag-doped nickelate ceramic for room temperature high-sensitivity infrared detection of the present embodiment specifically comprises the following steps: (1) Weighing lanthanum nitrate hexahydrate, calcium nitrate tetrahydrate, and manganese nitrate tetrahydrate with a purity of not less than 99.9% according to the stoichiometric ratio of cations in the chemical formula, using citric acid monohydrate as a complexing agent and methanol as a solvent, and stirring the weighed raw materials on a magnetic stirrer at room temperature to completely dissolve them, and controlling the weighing error within ±0.5 mg; (2) Ethylene glycol is used as a dispersant. After the raw materials in step (1) are completely dissolved, ethylene glycol is added to the mixed solution to allow it to be fully mixed with the solution, wherein the molar ratio of lanthanum calcium manganese oxide to ethylene glycol is 1:2; (3) After the mixed solution in step (2) is fully mixed, the solution is transferred to a magnetic heating stirrer at 100°C for heating and stirring. When the solution turns dark yellow and foaming is observed, the mixed solution is transferred to a constant temperature oven at 180°C for full foaming and drying for 7 hours to obtain a dry gel.

[0028] (4) The dry gel in step (3) was placed in an agate mortar and ground thoroughly for 1 h. The ground powder was placed in a muffle furnace and calcined at 700 °C for 5 h to remove organic matter and nitrate ions in the gel, thereby obtaining a black precursor powder. (5) mixing the lanthanum calcium manganese oxide precursor powder obtained in step (4) with platinum powder in a certain stoichiometric ratio in an agate mortar and grinding for 2 h to obtain a mixed precursor powder; (6) The mixed precursor powder obtained in step (5) was pressed into a block in an automatic tablet press at a pressure of 6 MPa for 30 min and then placed in a muffle furnace for sintering at 1550 °C for 16 h, x-0.4, y=0.2 to obtain La 0.6 Ca 0.4 MnO3:Pt 0.2 Composite ceramic blocks of composite ceramics.

[0029] The above description is only a specific implementation of the present application, so that those skilled in the art can understand or implement the present application. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present application. Therefore, the present application will not be limited to the embodiments shown herein, but will conform to the widest range consistent with the principles and novel features applied for herein.

Claims

1. A method for preparing a lanthanum calcium manganese oxide and metal platinum multiphase composite ceramic material, characterized in that: The steps include: (1) Weighing high-purity lanthanum nitrate hexahydrate, calcium nitrate tetrahydrate, and manganese nitrate tetrahydrate according to the stoichiometric ratio of cations in the chemical formula, using citric acid monohydrate as a complexing agent and methanol as a solvent, and stirring the weighed raw materials on a magnetic stirrer at room temperature to completely dissolve them; (2) Ethylene glycol is used as a dispersant. After the raw materials in step (1) are completely dissolved, ethylene glycol is added to the mixed solution to allow it to be fully mixed with the solution; (3) After the mixed solution in step (2) is fully mixed, the solution is transferred to a magnetic heating stirrer for heating and stirring. When the solution turns dark yellow and foaming is observed, the mixed solution is transferred to a constant temperature oven for full foaming and drying to obtain a dry gel.

2. (4) The dry gel in step (3) is placed in an agate mortar and ground thoroughly, and the ground powder is calcined in a muffle furnace to remove organic matter and nitrate ions in the gel to obtain a black precursor powder; (5) mixing the precursor powder obtained in step (4) with platinum powder in a certain stoichiometric ratio in an agate mortar and grinding them thoroughly to obtain a mixed precursor powder; (6) The mixed precursor powder obtained in step (5) is pressed into a block in an automatic tablet press, and then placed in a muffle furnace for high-temperature sintering to obtain La 1-x Ca x MnO3:Pt y Composite ceramic blocks.

3. The method for preparing a lanthanum calcium manganese oxide and metal platinum multiphase composite ceramic material according to claim 1, characterized in that: The purity of all raw materials in step (1) is not less than 99.9%, and the weighing error is controlled within ±0.5 mg; the chemical formula of the composite ceramic prepared in step (6) is La 1-x Ca x MnO3:Pt y , where 0 < x ≤ 0.4,0.05 ≤ y ≤ 0.

2.

4. The method for preparing a lanthanum calcium manganese oxide and metal platinum multiphase composite ceramic material according to claim 1, characterized in that: In step (2), the molar ratio of lanthanum calcium manganese oxide to ethylene glycol is 1:

2.

5. The method for preparing a lanthanum calcium manganese oxide and metal platinum multiphase composite ceramic material according to claim 1, characterized in that: In step (3), the mixed solution is heated to a reaction temperature of 70-100°C and the stirring speed is 300 r / min.

6. The method for preparing a lanthanum calcium manganese oxide and metal platinum multiphase composite ceramic material according to claim 1, characterized in that: In step (3), the oven temperature is set at 100-180°C and the drying time is 7-14 h under normal pressure and air atmosphere.

7. The method for preparing a lanthanum calcium manganese oxide and metal platinum multiphase composite ceramic material according to claim 1, characterized in that: The grinding time of step (4) is 0.5-1.0 h, the calcination temperature is 400-700 ° C in an air atmosphere, and the sintering holding time is 5-10 h.

8. The method for preparing a lanthanum calcium manganese oxide and metal platinum multiphase composite ceramic material according to claim 1, characterized in that: The grinding time in step (5) is 1-2 hours.

9. The method for preparing a lanthanum calcium manganese oxide and metal platinum multiphase composite ceramic material according to claim 1, characterized in that: In step (6), the setting parameters of the automatic tablet press are 3-6 MPa, the pressing time is about 20-30 min, the sintering temperature is 1400-1550 °C under normal pressure and air atmosphere, and the insulation time is 10-16 h.

Citation Information

Patent Citations

  • Low-temperature synthetic method of La&lt;1-x&gt;Ca&lt;x&gt;MnO3 nano-powder

    CN104211124A

  • Method for improving electrical performance of lanthanum-calcium-manganese-oxygen (LCMO) ceramic material

    CN106565242A

  • Method for preparing silver-doped lanthanum calcium manganese oxygen polycrystalline ceramic target

    CN110451961A

  • Preparation method of lanthanum-calcium-manganese-oxygen low-doped samarium nitrate

    CN111646798A

  • Nickel-doped lanthanum calcium manganese oxide polycrystalline ceramic target material