Silicon carbide-magnesium aluminate spinel refractory product and preparation method thereof
Through the casting molding process of silicon carbide-magnesium aluminum spinel refractory products, the chromium resource shortage and the limitations of press molding process of refractory materials for water-coal slurry gasification furnaces are solved, and high-strength and slag corrosion resistance are achieved. Refractory material preparation, suitable for automated production.
Patent Information
- Application Number
- CN202411212245.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-08-30
AI Technical Summary
The existing refractory materials for water-coal slurry gasification furnaces have problems with chromium resources, high costs and chromium pollution. The press molding process has limitations on the size and shape of the product, low strength, and is not conducive to automated production.
Silicon carbide-magnesium aluminum spinel refractory products are used, by mixing materials such as silicon carbide, magnesium aluminum spinel powder, lightly flammed magnesium oxide powder, passivated metal aluminum powder and alumina micro powder, adding water reducing agent, and using casting molding The process is calcined in a nitrogen atmosphere to form refractory products with high strength, good resistance to slag corrosion and permeability.
It improves the bonding strength and corrosion resistance of refractory products, reduces production costs, adapts to production needs of complex shapes and large sizes, and has a simple process and low energy consumption, making it suitable for mechanized construction.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of new refractory materials, and in particular relates to a silicon carbide-magnesia alumina spinel refractory product and a preparation method thereof. Background Art
[0002] From the perspective of my country's fossil energy reserves, coal accounts for more than 90% of the total proven fossil energy resources, while oil and natural gas account for less than 10%. At present, direct combustion and thermal power generation are still the main ways of using coal in my country, which brings about problems such as low energy utilization rate and serious environmental pollution. Therefore, it is of great significance to achieve clean and efficient use of coal.
[0003] Coal gasification is the most effective means of clean and efficient utilization of coal. As a typical representative process, water-coal slurry gasification technology is the most widely used in China. Refractory materials for water-coal slurry gasification furnaces face harsh working environments such as high temperature (1300-1600℃), high pressure (2-6.5MPa), slag erosion, thermal erosion, air flow scouring, and rapid temperature fluctuations. Therefore, the refractory materials used need to have good high-temperature mechanical properties, thermal shock resistance, and resistance to slag erosion and permeability. At present, the most commonly used refractory material for domestic gasifiers is chromium-aluminum-zirconium (Cr2O3-Al2O3-ZrO2) bricks, and its raw materials and components are mainly Cr2O3. However, there are some disadvantages of chromium-containing refractories: on the one hand, due to the shortage of chromium resources in my country, the cost of raw materials is relatively high; on the other hand, there is the problem of chromium pollution. There is potential Cr in the preparation, use and after use. 6+ It is harmful to human body and environment. Therefore, the development of chromium-free refractory materials for water-coal slurry gasifier is urgent.
[0004] At present, the chromium-free treatment of refractory materials for water-coal slurry gasifiers is mostly in the laboratory stage, and the material selection mostly focuses on designing the chemical composition of the material for anti-coal slag erosion tests. After research and exploration, oxide-non-oxide composite materials have more excellent resistance to coal slag erosion and permeability, and are the development direction of chromium-free refractory materials for coal gasification. Based on this, the patent (CN 202010646418.5) discloses a silicon carbide-magnesium aluminum spinel-aluminum composite refractory material, which uses silicon carbide particles as aggregates, magnesium aluminum spinel fine powder or micropowder as a matrix, and adds coated metal aluminum powder to the matrix. A resin binder is used, and the green body is formed by pressing and then fired into refractory bricks in a carbon-buried atmosphere at 1500-1600°C. The silicon carbide-magnesium aluminum spinel-aluminum composite refractory material has good resistance to slag erosion and penetration, but the pressing and molding has great limitations on the size and shape of the product, and can only produce products with small size and simple shape. In addition, the strength of the pressed green body is low before drying, and the skin and corners are easy to peel off, and the integrity of the green body cannot be guaranteed. In addition, the pressing and molding has high labor intensity, large machine energy consumption, and low construction efficiency, which is not conducive to automated production. Summary of the invention
[0005] In view of the problems and shortcomings in the prior art, the object of the present invention is to provide a silicon carbide-magnesium aluminum spinel refractory product and a preparation method thereof.
[0006] To achieve the purpose of the invention, the technical solution adopted by the present invention is as follows:
[0007] The first aspect of the present invention provides a silicon carbide-magnesium aluminate spinel refractory product. The raw material composition of the silicon carbide-magnesium aluminate spinel refractory product is calculated by mass percentage: 50% to 70% of silicon carbide with a particle size of 0.1 to 3 mm, 10% to 30% of magnesium aluminate spinel powder with a particle size of 0.045 to 1 mm, 1% to 10% of a binder, 1% to 10% of alumina powder, 1% to 10% of passivated metal aluminum powder and 0.1% to 10% of an additive, plus 0.1% to 1% of a water reducer accounting for 0.1% to 1% of the total mass of the above raw materials; the binder is lightly burned magnesium oxide powder.
[0008] According to the above-mentioned silicon carbide-magnesium aluminate spinel refractory products, preferably, calculated by mass percentage, the raw material composition of the silicon carbide-magnesium aluminate spinel refractory products is: 63% silicon carbide with a particle size of 0.1-3mm, 18.2% magnesium aluminate spinel powder with a particle size of 0.045-1mm, 4% binder, 5% alumina powder, 9% passivation metal aluminum powder and 0.8% additives, plus 0.15% of the total mass of the above-mentioned raw materials The water reducer.
[0009] According to the above-mentioned silicon carbide-magnesium aluminum spinel refractory product, preferably, the preparation method of the passivated metal aluminum powder is: calcining the metal aluminum powder at 500-620° C. for 1-20 hours, and obtaining the passivated metal aluminum powder after cooling.
[0010] According to the above silicon carbide-magnesium aluminate spinel refractory product, preferably, the additive is lactate.
[0011] According to the above silicon carbide-magnesium aluminate spinel refractory product, preferably, the lactate is at least one of aluminum lactate and magnesium lactate; more preferably, the lactate is aluminum lactate.
[0012] According to the above-mentioned silicon carbide-magnesium alumina spinel refractory product, preferably, the alumina powder is calcined alumina powder or activated alumina powder; more preferably, the alumina powder is activated alumina powder; most preferably, the activated alumina powder is bimodal activated alumina powder.
[0013] According to the above-mentioned silicon carbide-magnesium aluminum spinel refractory products, preferably, the silicon carbide is fused silicon carbide, and the fused silicon carbide particles have a complete crystal structure, high density, and good resistance to coal slag corrosion and oxidation. More preferably, the purity of fused silicon carbide is ≥98.0%; because SiO2, Fe2O3, Na2O, K2O and other impurity phases in the silicon carbide raw material will form low-melting point substances at high temperatures, reducing the high-temperature mechanical properties and slag corrosion resistance of the refractory products, the present invention controls the purity of fused silicon carbide to be ≥98.0%, and the content of impurities such as SiO2, Fe2O3, Na2O, K2O in fused silicon carbide of this purity is very low, which can effectively reduce the formation of low-melting point substances during the high-temperature calcination of the castable, and reduce the influence of impurities on the high-temperature mechanical properties and slag corrosion resistance of the refractory products.
[0014] According to the above-mentioned silicon carbide-magnesium aluminate spinel refractory products, preferably, the purity w (Al2O3+MgO) of the magnesium aluminate spinel powder is ≥99.0%, and this purity can ensure that the prepared refractory products have good resistance to coal slag erosion; the mass fraction of Al2O3 in the magnesium aluminate spinel powder is ≥72.0%, and this setting can ensure that the MgO in the raw materials exists in a stable spinel phase, and during the firing process, no low-melting phase (Al2O3+MgO+SiO2) is generated.
[0015] According to the above silicon carbide-magnesium aluminum spinel refractory product, preferably, the particle size of the passivated metal aluminum powder is 0.048-0.11 mm, the particle size of the alumina powder is 2-4 μm, and the water reducer is a polycarboxylic acid water reducer or a naphthalene-based water reducer.
[0016] The second aspect of the present invention provides a method for preparing the silicon carbide-magnesium aluminum spinel refractory product according to the first aspect, comprising the following steps:
[0017] (1) mixing silicon carbide, magnesium aluminum spinel powder, a binder, alumina powder, passivation metal aluminum powder, an additive and a water reducing agent to obtain a mixture; adding water to the mixture and mixing to obtain a slurry;
[0018] (2) pouring the clay into a mold, curing at room temperature, demolding, and drying to obtain a blank;
[0019] (3) calcining the blank at 1000° C. to 1600° C. in a nitrogen atmosphere to obtain a silicon carbide-magnesium aluminum spinel refractory product.
[0020] According to the above preparation method, preferably, the drying temperature in step (2) is 110° C. and the drying time is 24 h.
[0021] Compared with the prior art, the present invention has the following positive and beneficial effects:
[0022] (1) The silicon carbide-magnesium aluminate spinel refractory product of the present invention adds metal aluminum powder that has been passivated to the matrix. During the casting process, on the one hand, the passivation layer on the surface of the passivated metal aluminum powder can effectively prevent the metal aluminum powder from reacting with free water in the castable to produce gas. On the other hand, the metal aluminum powder and the hydration product of light-burned magnesium oxide produce a synergistic effect to generate a dense magnesium aluminum hydrotalcite, which further prevents the hydration of the aluminum powder and avoids the expansion of the blank. Moreover, during the high-temperature calcination process, the metal aluminum reacts with N2 in the atmosphere in the form of liquid or gas to generate AlN with whisker-like, rod-like, sheet-like, etc. morphology, which forms a firm bond with the matrix on a microscopic scale, thereby improving the bonding strength of the material and improving the corrosion resistance and thermal shock resistance.
[0023] (2) The present invention calcines metal aluminum powder at 500-620°C for 1-20 hours, oxidizing its surface to form a dense aluminum oxide layer, and then obtains passivated metal aluminum powder after cooling. The passivated metal aluminum powder has a simple preparation process, a relatively uniform coating layer, and can be mass-produced. At the same time, it can avoid agglomeration during preparation such as aluminum sol coating, which causes the passivation layer to peel off when crushed, thereby affecting the passivation effect.
[0024] (3) The present invention uses light-burned magnesium oxide powder as a binder to prepare refractory products. At room temperature, the light-burned magnesium oxide powder generates hydrate [Mg(OH)2] through a hydration reaction, which solidifies and hardens to obtain strength. It can form high bonding strength by low-temperature drying, thereby providing higher demolding and drying strength, and avoiding partial peeling and pulverization during room temperature storage and transportation of the green body. The light-burned magnesium oxide powder can react with the active alumina powder in the matrix at high temperature to generate magnesium-aluminum spinel in situ, and dissolve the divalent and trivalent ions in the molten slag, which not only improves the bonding strength of the refractory products, but also greatly enhances the ability of the refractory products to resist slag erosion and penetration. Moreover, compared with phenolic resin binder, the present invention uses lightly burned magnesium oxide powder as a binder to avoid harmful gases and residual carbon generated by the decomposition of phenolic resin during high-temperature calcination, and solves the technical problem that metal aluminum reacts with C generated by the decomposition of phenolic resin to generate Al4C3 (Al4C3 is very easy to hydrate) during the high-temperature calcination of refractory products using phenolic resin as a binder, resulting in cracking and powdering of refractory products during storage and use, causing the refractory products to be scrapped or the service life to be greatly reduced. In addition, compared with calcium aluminate cement, a commonly used binder for castables, the present invention uses lightly burned magnesium oxide powder as a binder to avoid introducing CaO into the castable, and solves the technical problem that when calcium aluminate cement is used as a binder, CaO is introduced into the castable to reduce the slag erosion resistance and permeability of the refractory products.
[0025] (4) The refractory products of the present invention are prepared in the form of casting. After curing and demolding, the flexural strength of the prepared refractory products reaches 2.9-5.9 MPa at room temperature, the compressive strength is 11.1-23.6 MPa, and the demolding strength is high. Compared with the silicon carbide-magnesium aluminum spinel shaped products prepared by machine compression molding, the present invention can effectively reduce the cracking of the green body and improve the yield rate. In addition, compared with the pressing molding, the casting molding has a simple production process, high labor productivity, strong adaptability to the product shape and size, and is conducive to mechanized construction.
[0026] (5) During the preparation of the silicon carbide-magnesium aluminum spinel refractory product of the present invention, the green refractory product is calcined in a nitrogen atmosphere; compared with a carbon-buried atmosphere, a nitrogen atmosphere can prevent further oxidation of metal Al, resulting in a thicker passivation layer, making it difficult for molten Al to escape, and unable to fully participate in whisker formation and mechanical property improvement. In addition, under a carbon-buried atmosphere, the nitrogen atmosphere partial pressure decreases with increasing heating time, while under a circulating nitrogen atmosphere, the atmosphere partial pressure in the furnace is always consistent at each stage of heating, which is more conducive to the nitridation reaction of metal Al.
[0027] (6) The silicon carbide-magnesium aluminum spinel refractory product of the present invention has an apparent porosity of 18% to 22% after calcination and a bulk density of 2.6 g / cm 3 ~2.7g / cm 3The room temperature flexural strength reaches 5.4-18.3 MPa, and the room temperature compressive strength reaches 62.0-99.0 MPa. Therefore, the silicon carbide-magnesium aluminum spinel refractory product of the present invention has high strength, good resistance to slag erosion and permeability, and also has the advantages of convenient construction, long construction time during pouring, and low production energy consumption.
[0028] (7) The refractory product of the present invention contains an additive, and the additive is preferably lactate. Lactate can make Mg(OH)2 grow evenly on the surface of MgO particles, thereby preventing the MgO-bound castable from expanding in volume during the curing and drying process and forming cracks in the castable. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 This is a graph showing the volume change test results of green body samples prepared using the matrix part raw materials in the refractory product formulations of Example 1-1 and Comparative Example 1-1;
[0030] Figure 2 This is a scanning electron microscope secondary electron image of the refractory product prepared in Example 1 of the present invention. DETAILED DESCRIPTION
[0031] The following examples are only for further explanation of the present invention. It should be noted that all technical and scientific terms used in the present invention have the same meanings as in the technical field to which the present invention belongs unless otherwise specified. The experimental methods in the following examples without specifying specific conditions are all based on conventional techniques in the technical field, or according to the conditions recommended by the manufacturer; the reagents or instruments used without specifying the manufacturer are all conventional products that can be purchased commercially.
[0032] In order to enable those skilled in the art to more clearly understand the technical solution of the present invention, the technical solution of the present invention will be described in detail below in conjunction with specific embodiments.
[0033] Example 1: Discussion on types of aluminum powder
[0034] In order to study the effect of whether the metal aluminum powder in the refractory product is passivated on the performance of the prepared silicon carbide-magnesium aluminum spinel refractory product, the present invention carried out Example 1-1 and Comparative Example 1-1. The specific contents of Example 1-1 and Comparative Example 1-1 and Comparative Example 1-1 are as follows:
[0035] Example 1-1:
[0036] A silicon carbide-magnesium aluminum spinel refractory product, whose raw material composition is calculated by mass percentage: 63% of silicon carbide with a particle size of 0.1-3mm, 20.2% of magnesium aluminum spinel powder with a particle size of 0.045-1mm, 4% of a binder, 5% of alumina micropowder with a particle size of 2-4μm, 7% of passivated metal aluminum powder with a particle size of 0.048-0.11mm and 0.8% of an additive, plus a water reducer accounting for 0.15% of the total mass of the above raw materials; the binder is light-burned magnesium oxide powder, the additive is aluminum lactate, and the water reducer is a polycarboxylic acid water reducer; the preparation method of the passivated metal aluminum powder is: calcining the metal aluminum powder at 500-620°C for 1-20h, and obtaining the passivated metal aluminum powder after cooling.
[0037] The preparation method of the above silicon carbide-magnesium aluminum spinel refractory product comprises the following specific steps:
[0038] (1) mixing silicon carbide, magnesium aluminum spinel powder, a binder, alumina powder, passivation metal aluminum powder, an additive and a water reducing agent to obtain a mixture; adding water to the mixture and mixing to obtain a slurry;
[0039] (2) pouring the clay into a mold, curing at room temperature for 24 hours, then demolding, and then drying at 110° C. for 24 hours to obtain a blank;
[0040] (3) The blank is calcined at 1500° C. for 5 h in a flowing nitrogen atmosphere to obtain a silicon carbide-magnesium aluminate spinel refractory product.
[0041] Comparative Example 1-1:
[0042] A silicon carbide-magnesium aluminum spinel refractory product, whose raw material composition, calculated by mass percentage, is: 63% of silicon carbide with a particle size of 0.1-3mm, 20.2% of magnesium aluminum spinel powder with a particle size of 0.045-1mm, 4% of a binder, 5% of aluminum oxide micropowder with a particle size of 2-4μm, 7% of metal aluminum powder with a particle size of 0.048-0.11mm and 0.8% of an additive, plus a water reducer accounting for 0.15% of the total mass of the above raw materials; the binder is light-burned magnesium oxide powder, the additive is aluminum lactate, and the water reducer is a polycarboxylate water reducer.
[0043] The preparation method of the above silicon carbide-magnesium aluminum spinel refractory product comprises the following specific steps:
[0044] (1) mixing silicon carbide, magnesium aluminum spinel powder, a binder, alumina powder, metal aluminum powder, an additive and a water reducing agent uniformly to obtain a mixture; adding water to the mixture and mixing uniformly to obtain a slurry;
[0045] (2) pouring the clay into a mold, curing at room temperature for 24 hours, then demolding, and then drying at 110° C. for 24 hours to obtain a blank;
[0046] (3) The blank is calcined at 1500° C. for 5 h in a flowing nitrogen atmosphere to obtain a silicon carbide-magnesium aluminate spinel refractory product.
[0047] The demoulding strength test was performed on the blanks prepared in Example 1-1 and Comparative Example 1-1, and the mechanical properties of the silicon carbide-magnesium aluminum spinel refractory products prepared after calcining the blanks were tested. The demoulding strength test method is: the strength of the blank obtained after demoulding is tested according to GB / T3001-2007. The mechanical property test method after the green body is calcined is: the flexural strength and compressive strength of the refractory material after sintering at 1500°C are tested according to GB / T 3001-2007 and GB / T5702-2008, respectively, and the volume density and apparent porosity of the refractory material after sintering at 1500°C are tested according to GB / T2997-2000. The test results of the demoulding strength of the green body and the mechanical properties of the green body after calcining of Example 1-1 and Comparative Example 1-1 are shown in Table 1.
[0048] Table 1 shows the test results of the demoulding strength of the green body and the mechanical properties of the green body after calcination of Example 1-1 and Comparative Example 1-1.
[0049]
[0050] As shown in Table 1, compared with Comparative Example 1-1, the sample prepared in Example 1-1 has higher green and fired strength and lower apparent porosity. This is because the green sample prepared in Comparative Example 1-1 will undergo a large volume expansion during the curing process, the internal structure of the green body is destroyed, and obvious cracks are generated on the surface of the green body, resulting in poor performance of the product prepared in Comparative Example 1-1. This shows that the use of passivated metal aluminum powder in the present invention can improve the physical properties of silicon carbide-magnesium aluminum spinel refractory products.
[0051] Since the metal aluminum powder reacts with water to generate gas, the volume expansion of the castable occurs. In order to study the effect of whether the metal aluminum powder is passivated on the volume expansion of the castable blank, the present invention further adopts the matrix raw materials in Example 1-1 and Comparative Example 1-1 (in terms of mass percentage, the composition is: 27% silicon carbide with a particle size of 0.1 to 0.5 mm, 27.6% magnesium aluminum spinel powder with a particle size of 0.045 mm, 10.8% binder, and alumina with a particle size of 2 to 4 μm). The green sample was prepared by weighing the raw materials according to the composition of the matrix raw materials, putting them in a plastic cup, adding water and stirring them evenly, and curing them at room temperature for 24 hours to obtain the green sample. The volume change of the green sample was observed by taking photos and recording. The volume change test results of the green sample are shown in FIG. Figure 1 shown.
[0052] Depend on Figure 1 It can be seen that compared with Example 1-1, the green body sample prepared in Comparative Example 1-1 has serious expansion. This is because the metal aluminum powder in Comparative Example 1-1 has not been passivated, and reacts with water in large quantities during the pouring process, generating a large amount of H2, which causes the green body to expand; the matrix sample prepared in Example 1 has basically no expansion. This shows that the use of passivated metal aluminum powder in the present invention can reduce the reaction between the metal aluminum powder and water during the pouring process, avoid a large volume expansion, and thus improve the volume stability of silicon carbide-magnesium aluminum spinel refractory products.
[0053] Example 2: Discussion on the dosage of passivated aluminum powder
[0054] In order to study the effect of the amount of passivation metal aluminum powder in refractory products on the performance of the prepared silicon carbide-magnesium aluminum spinel refractory products, the present invention carried out Examples 2-1 to 2-3 and Comparative Examples 2-1 to 2-2. The specific contents of Examples 2-1 to 2-3 and Comparative Examples 2-1 to 2-2 are as follows:
[0055] Example 2-1:
[0056] A silicon carbide-magnesium aluminum spinel refractory product, whose raw material composition is calculated by mass percentage: 63% of silicon carbide with a particle size of 0.1-3mm, 24.2% of magnesium aluminum spinel powder with a particle size of 0.045-1mm, 4% of a binder, 5% of alumina micropowder with a particle size of 2-4μm, 3% of passivated metal aluminum powder with a particle size of 0.048-0.11mm and 0.8% of an additive, plus a water reducer accounting for 0.15% of the total mass of the above raw materials; the binder is light-burned magnesium oxide powder, the additive is aluminum lactate, and the water reducer is a polycarboxylic acid water reducer; the preparation method of the passivated metal aluminum powder is: calcining the metal aluminum powder at 500-620°C for 1-20h, and obtaining the passivated metal aluminum powder after cooling.
[0057] The preparation method of the above silicon carbide-magnesium aluminum spinel refractory product is the same as that of Example 1-1.
[0058] Example 2-2:
[0059] A silicon carbide-magnesium aluminum spinel refractory product, whose raw material composition is calculated by mass percentage: 63% of silicon carbide with a particle size of 0.1-3mm, 22.2% of magnesium aluminum spinel powder with a particle size of 0.045-1mm, 4% of a binder, 5% of alumina micropowder with a particle size of 2-4μm, 5% of passivated metal aluminum powder with a particle size of 0.048-0.11mm and 0.8% of an additive, plus a water reducer accounting for 0.15% of the total mass of the above raw materials; the binder is light-burned magnesium oxide powder, the additive is aluminum lactate, and the water reducer is a polycarboxylic acid water reducer; the preparation method of the passivated metal aluminum powder is: calcining the metal aluminum powder at 500-620°C for 1-20h, and obtaining the passivated metal aluminum powder after cooling.
[0060] The preparation method of the above silicon carbide-magnesium aluminum spinel refractory product is the same as that of Example 1-1.
[0061] Embodiment 2-3:
[0062] A silicon carbide-magnesium aluminum spinel refractory product, whose raw material composition is calculated by mass percentage: 63% of silicon carbide with a particle size of 0.1-3mm, 18.2% of magnesium aluminum spinel powder with a particle size of 0.045-1mm, 4% of a binder, 5% of alumina micropowder with a particle size of 2-4μm, 9% of passivated metal aluminum powder with a particle size of 0.048-0.11mm and 0.8% of an additive, plus a water reducer accounting for 0.15% of the total mass of the above raw materials; the binder is light-burned magnesium oxide powder, the additive is aluminum lactate, and the water reducer is a polycarboxylic acid water reducer; the preparation method of the passivated metal aluminum powder is: calcining the metal aluminum powder at 500-620°C for 1-20h, and obtaining the passivated metal aluminum powder after cooling.
[0063] The preparation method of the above silicon carbide-magnesium aluminum spinel refractory product is the same as that of Example 1-1.
[0064] Comparative Example 2-1:
[0065] A silicon carbide-magnesium aluminum spinel refractory product, whose raw material composition is calculated by mass percentage: 63% of silicon carbide with a particle size of 0.1-3mm, 14.2% of magnesium aluminum spinel powder with a particle size of 0.045-1mm, 4% of a binder, 5% of alumina micropowder with a particle size of 2-4μm, 13% of passivated metal aluminum powder with a particle size of 0.048-0.11mm and 0.8% of an additive, plus a water reducer accounting for 0.15% of the total mass of the above raw materials; the binder is light-burned magnesium oxide powder, the additive is aluminum lactate, and the water reducer is a polycarboxylic acid water reducer; the preparation method of the passivated metal aluminum powder is: calcining the metal aluminum powder at 500-620°C for 1-20h, and obtaining the passivated metal aluminum powder after cooling.
[0066] The preparation method of the above silicon carbide-magnesium aluminum spinel refractory product is the same as that of Example 1-1.
[0067] Comparative Example 2-2:
[0068] A silicon carbide-magnesium aluminum spinel refractory product, whose raw material composition is calculated by mass percentage: 63% of silicon carbide with a particle size of 0.1-3mm, 27.2% of magnesium aluminum spinel powder with a particle size of 0.045-1mm, 4% of a binder, 5% of alumina micropowder with a particle size of 2-4μm, 0% of passivated metal aluminum powder with a particle size of 0.048-0.11mm and 0.8% of an additive, plus a water reducer accounting for 0.15% of the total mass of the above raw materials; the binder is light-burned magnesium oxide powder, the additive is aluminum lactate, and the water reducer is a polycarboxylic acid water reducer; the preparation method of the passivated metal aluminum powder is: calcining the metal aluminum powder at 500-620°C for 1-20h, and obtaining the passivated metal aluminum powder after cooling.
[0069] The preparation method of the above silicon carbide-magnesium aluminum spinel refractory product is the same as that of Example 1-1.
[0070] The demoulding strength of the refractory product blanks (green blanks) prepared in Examples 2-1 to 2-3 and Comparative Examples 2-1 to 2-2 was tested, and the mechanical properties of the green blanks after calcination were also tested. The test results are shown in Table 2.
[0071] Table 2 shows the test results of the demoulding strength of the green body and the mechanical properties of the green body after calcination of Examples 2-1 to 2-3 and Comparative Examples 2-1 to 2-2.
[0072]
[0073] It can be seen from Table 2 that with the increase of the amount of passivation metal aluminum powder added, the green and fired physical properties of the prepared silicon carbide-magnesium aluminum spinel refractory products first increase and then decrease. When the amount of passivation metal aluminum powder added is 9%, the silicon carbide-magnesium aluminum spinel refractory products have relatively excellent green and fired physical properties. This shows that adding 9% passivation metal aluminum powder is more conducive to the preparation of high-performance silicon carbide-magnesium aluminum spinel refractory products.
[0074] Example 3: Discussion on types of additives
[0075] In order to study the influence of the type of additives in refractory products on the performance of the prepared silicon carbide-magnesium aluminum spinel refractory products, the present invention carried out Example 3-1 and Comparative Example 3-1. The specific contents of Example 3-1 and Comparative Example 3-1 are as follows:
[0076] Example 3-1:
[0077] A silicon carbide-magnesium aluminum spinel refractory product, whose raw material composition is calculated by mass percentage: 63% of silicon carbide with a particle size of 0.1-3mm, 18.2% of magnesium aluminum spinel powder with a particle size of 0.045-1mm, 4% of a binder, 5% of alumina micropowder with a particle size of 2-4μm, 9% of passivated metal aluminum powder with a particle size of 0.048-0.11mm and 0.8% of an additive, plus a water reducer accounting for 0.15% of the total mass of the above raw materials; the binder is light-burned magnesium oxide powder, the additive is magnesium lactate, and the water reducer is a polycarboxylic acid water reducer; the preparation method of the passivated metal aluminum powder is: calcining the metal aluminum powder at 500-620°C for 1-20h, and obtaining the passivated metal aluminum powder after cooling.
[0078] The preparation method of the above silicon carbide-magnesium aluminum spinel refractory product is the same as that of Example 1-1.
[0079] Comparative Example 3-1:
[0080] A silicon carbide-magnesium aluminum spinel refractory product, whose raw material composition is calculated by mass percentage: 63% of silicon carbide with a particle size of 0.1-3mm, 19% of magnesium aluminum spinel powder with a particle size of 0.045-1mm, 4% of binder, 5% of aluminum oxide micropowder with a particle size of 2-4μm, 9% of passivated metal aluminum powder with a particle size of 0.048-0.11mm and 0% of additives, plus a water reducer accounting for 0.15% of the total mass of the above raw materials; the binder is light-burned magnesium oxide powder, and the water reducer is a polycarboxylic acid water reducer; the preparation method of the passivated metal aluminum powder is: calcining the metal aluminum powder at 500-620°C for 1-20h, and obtaining the passivated metal aluminum powder after cooling.
[0081] The preparation method of the above silicon carbide-magnesium aluminum spinel refractory product is the same as that of Example 1-1.
[0082] The demoulding strength of the refractory product blanks (green blanks) prepared in Example 3-1 and Comparative Example 3-1 was tested, and the mechanical properties of the green blanks after calcination were tested. The test results are shown in Table 3.
[0083] Table 3 shows the test results of the demoulding strength of the green body and the mechanical properties of the green body after calcination in Example 3-1 and Comparative Example 3-1.
[0084]
[0085] As can be seen from Table 3, the physical properties of the green and fired silicon carbide-magnesium aluminum spinel refractory products prepared by Example 3-1 and Example 2-3 are relatively close, and both are better than Comparative Example 3-1. This is because Mg(OH)2 of different particle sizes is generated on the surface of MgO particles during the hydration of light-burned magnesium oxide, resulting in microcracks in the castable body, which leads to poor physical properties of Comparative Example 3-1. This shows that the addition of lactate is more conducive to the preparation of high-performance silicon carbide-magnesium aluminum spinel refractory products.
[0086] Example 4: Experiment on the types of binding agents
[0087] In order to study the influence of the type of binder on the performance of the prepared silicon carbide-magnesium aluminum spinel refractory products, the present invention carried out comparative example 4-1, and the specific content of comparative example 4-1 is as follows.
[0088] Comparative Example 4-1:
[0089] A silicon carbide-magnesium aluminum spinel refractory product, the raw material composition of which is calculated by mass percentage: 63% of silicon carbide with a particle size of 0.1-3mm, 23.0% of magnesium aluminum spinel powder with a particle size of 0.045-1mm, 5% of aluminum oxide micropowder with a particle size of 2-4μm and 9% of metal aluminum powder with a particle size of 0.048-0.11mm, plus a binder accounting for 4% of the total mass of the above raw materials; the binder is phenolic resin
[0090] The demoulding strength of the refractory product blanks (green blanks) prepared in Example 2-3 and Comparative Example 4-1 was tested, and the mechanical properties of the green blanks after calcination were also tested. The test results are shown in Table 4.
[0091] Table 4 shows the test results of the demoulding strength of the green body and the mechanical properties of the green body after calcination in Example 2-3 and Comparative Example 4-1.
[0092]
[0093] As can be seen from Table 4, the green strength of Example 2-3 is significantly higher than that of Comparative Example 4-1, and the physical properties of Example 4-1 after firing at 1500°C are slightly lower than those of Comparative Example 4-1. This shows that the silicon carbide-magnesium aluminum spinel refractory product prepared by casting with lightly burned magnesium oxide powder as a binder in the present invention has relatively excellent green strength, can ensure the integrity of the sample before drying, and also avoids partial peeling and pulverization during storage and transportation of the green body at room temperature; and when lightly burned magnesium oxide powder is used as a binder, silicon carbide-magnesium aluminum spinel refractory products with good mechanical properties can be prepared by casting, which is simple in production process, high in labor productivity, strong in adaptability to product shape and size, and more energy-saving and environmentally friendly compared to press molding.
[0094] Example 5: Discussion on the dosage of binder
[0095] In order to study the effect of the amount of binder on the performance of the prepared silicon carbide-magnesium aluminum spinel refractory products, the present invention carried out Examples 5-1 to 5-4. The specific contents of Examples 5-1 to 5-4 are as follows:
[0096] Example 5-1:
[0097] A silicon carbide-magnesium aluminum spinel refractory product, whose raw material composition is calculated by mass percentage: 63% of silicon carbide with a particle size of 0.1-3mm, 21.8% of magnesium aluminum spinel powder with a particle size of 0.045-1mm, 1% of a binder, 5% of alumina micropowder with a particle size of 2-4μm, 9% of passivated metal aluminum powder with a particle size of 0.048-0.11mmμm and 0.2% of an additive, and a water reducer accounting for 0.15% of the total mass of the above raw materials; the binder is light-burned magnesium oxide powder, and the water reducer is a polycarboxylic acid water reducer; the preparation method of the passivated metal aluminum powder is: calcining the metal aluminum powder at 500-620°C for 1-20h, and obtaining the passivated metal aluminum powder after cooling.
[0098] The preparation method of the above silicon carbide-magnesium aluminum spinel refractory product is the same as that of Example 1-1.
[0099] Example 5-2:
[0100] A silicon carbide-magnesium aluminum spinel refractory product, whose raw material composition is calculated by mass percentage: 63% of silicon carbide with a particle size of 0.1-3mm, 19.4% of magnesium aluminum spinel powder with a particle size of 0.045-1mm, 3% of a binder, 5% of alumina micropowder with a particle size of 2-4μm, 9% of passivated metal aluminum powder with a particle size of 0.048-0.11mm and 0.6% of an additive, plus a water reducer accounting for 0.15% of the total mass of the above raw materials; the binder is light-burned magnesium oxide powder, and the water reducer is a polycarboxylic acid water reducer; the preparation method of the passivated metal aluminum powder is: calcining the metal aluminum powder at 500-620°C for 1-20h, and obtaining the passivated metal aluminum powder after cooling.
[0101] The preparation method of the above silicon carbide-magnesium aluminum spinel refractory product is the same as that of Example 1-1.
[0102] Example 5-3:
[0103] A silicon carbide-magnesium aluminum spinel refractory product, whose raw material composition is calculated by mass percentage: 63% of silicon carbide with a particle size of 0.1-3mm, 17% of magnesium aluminum spinel powder with a particle size of 0.045-1mm, 5% of binder, 5% of aluminum oxide micropowder with a particle size of 2-4μm, 9% of passivated metal aluminum powder with a particle size of 0.048-0.11mm and 1% of additives, plus a water reducer accounting for 0.15% of the total mass of the above raw materials; the binder is light-burned magnesium oxide powder, and the water reducer is a polycarboxylic acid water reducer; the preparation method of the passivated metal aluminum powder is: calcining the metal aluminum powder at 500-620°C for 1-20h, and obtaining the passivated metal aluminum powder after cooling.
[0104] The preparation method of the above silicon carbide-magnesium aluminum spinel refractory product is the same as that of Example 1-1.
[0105] Example 5-4:
[0106] A silicon carbide-magnesium aluminum spinel refractory product, whose raw material composition is calculated by mass percentage: 63% of silicon carbide with a particle size of 0.1-3mm, 14.6% of magnesium aluminum spinel powder with a particle size of 0.045-1mm, 7% of binder, 5% of aluminum oxide micropowder with a particle size of 2-4μm, 9% of passivated metal aluminum powder with a particle size of 0.048-0.11mm and 1.4% of additives, plus a water reducer accounting for 0.15% of the total mass of the above raw materials; the binder is light-burned magnesium oxide powder, and the water reducer is a polycarboxylic acid water reducer; the preparation method of the passivated metal aluminum powder is: calcining the metal aluminum powder at 500-620°C for 1-20h, and obtaining the passivated metal aluminum powder after cooling.
[0107] The preparation method of the above silicon carbide-magnesium aluminum spinel refractory product is the same as that of Example 1-1.
[0108] The demoulding strength of the refractory product blanks (green blanks) prepared in Examples 5-1 to 5-4 was tested, and the mechanical properties of the green blanks after calcination were also tested. The test results are shown in Table 5.
[0109] Table 5 shows the test results of the demoulding strength of the green body and the mechanical properties of the green body after calcination in Examples 5-1 to 5-4.
[0110]
[0111] It can be seen from Table 5 that with the increase of the amount of light-burned magnesium oxide powder added as a binder, the green and fired physical properties of the prepared silicon carbide-magnesium aluminum spinel refractory products first increase and then decrease. When the amount of light-burned magnesium oxide powder added is 4%, the silicon carbide-magnesium aluminum spinel refractory products have relatively excellent green and fired physical properties. This shows that adding 4% light-burned magnesium oxide powder is more conducive to the preparation of high-performance silicon carbide-magnesium aluminum spinel refractory products.
[0112] Example 6: Discussion of Calcination Gas Atmosphere
[0113] In order to study the influence of the calcining gas atmosphere of refractory products on the performance of the prepared silicon carbide-magnesium aluminum spinel refractory products, the present invention conducted comparative example 6-1. The specific contents of comparative example 6-1 are as follows:
[0114] Comparative Example 6-1:
[0115] A silicon carbide-magnesium aluminum spinel refractory product, whose raw material composition is calculated by mass percentage: 63% of silicon carbide with a particle size of 0.1-3mm, 18.2% of magnesium aluminum spinel powder with a particle size of 0.045-1mm, 4% of a binder, 5% of alumina micropowder with a particle size of 2-4μm, 9% of passivated metal aluminum powder with a particle size of 0.048-0.11mm and 0.8% of an additive, plus a water reducer accounting for 0.15% of the total mass of the above raw materials; the binder is light-burned magnesium oxide powder; the water reducer is a polycarboxylic acid water reducer; the preparation method of the passivated metal aluminum powder is: calcining the metal aluminum powder at 500-620°C for 1-20h, and obtaining the passivated metal aluminum powder after cooling.
[0116] The preparation method of the silicon carbide-magnesium aluminum spinel refractory product in this embodiment comprises the following specific steps:
[0117] (1) mixing silicon carbide, magnesium aluminum spinel powder, a binder, alumina powder, passivation metal aluminum powder, an additive and a water reducing agent to obtain a mixture; adding water to the mixture and mixing to obtain a slurry;
[0118] (2) pouring the clay into a mold, curing at room temperature for 24 hours, then demolding, and then drying at 110° C. for 24 hours to obtain a blank;
[0119] (3) calcining the blank at 1500° C. for 5 h in a flowing carbon atmosphere to obtain a silicon carbide-magnesium aluminum spinel refractory product.
[0120] The demoulding strength of the refractory product blanks (green blanks) prepared in Example 2-3 and Comparative Example 6-1 was tested, and the mechanical properties of the green blanks after calcination were tested. The test results are shown in Table 6.
[0121] Table 6 shows the test results of the demoulding strength of the green body and the mechanical properties of the green body after calcination in Example 2-3 and Comparative Example 6-1.
[0122]
[0123] As can be seen from Table 6, the physical properties of Example 2-3 after firing at 1500°C are significantly higher than those of Comparative Example 6-1, which shows that it is more conducive to the preparation of high-performance silicon carbide-magnesium aluminum spinel refractory products under a circulating nitrogen atmosphere. The reason is that because the partial pressure of the atmosphere in the furnace is always consistent at each stage of heating under a circulating nitrogen atmosphere, it is more conducive to the nitridation reaction of the metal Al powder to generate AlN with whisker-like, rod-like, and sheet-like morphologies. The silicon carbide-magnesium aluminum spinel refractory products prepared in Example 2-3 of the present invention were analyzed using a scanning electron microscope, and the microscopic morphology of the fracture is as follows: Figure 2 As shown. Figure 2 It can be seen that there are a large number of flake AlN interspersed in the matrix around the aluminum shell, forming a strong bond with the matrix on a microscopic scale, thereby improving the bonding strength of the material and thus improving the physical properties of the refractory product.
[0124] Finally, it should be noted that the above embodiments are only preferred embodiments of the present invention, and are not intended to limit the present invention in other forms. Any technician familiar with the profession may use the above technical content as inspiration to make changes or modifications. This is an equivalent embodiment of equivalent changes. However, any simple modification, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention without departing from the technical concept of the present invention still fall within the scope of protection of the claims of the present invention.
Claims
1. A silicon carbide-magnesia alumina spinel refractory product, characterized in that: Calculated by mass percentage, the raw material composition of the silicon carbide-magnesium aluminate spinel refractory product is: 50% to 70% silicon carbide with a particle size of 0.1 to 3 mm, 10% to 30% magnesium aluminate spinel powder with a particle size of 0.045 to 1 mm, 1% to 10% binder, 1% to 10% alumina powder, 1% to 10% passivated metal aluminum powder and 0.1% to 10% additives, plus 0.1% to 1% of a water reducer accounting for the total mass of the above raw materials; the binder is lightly burned magnesium oxide powder.
2. The silicon carbide-magnesium aluminum spinel refractory product according to claim 1, characterized in that: The preparation method of the passivated metal aluminum powder is as follows: calcining the metal aluminum powder at 500-620° C. for 1-20 hours, and obtaining the passivated metal aluminum powder after cooling.
3. The silicon carbide-magnesium aluminum spinel refractory product according to claim 1 or 2, characterized in that: The additive is lactate.
4. The silicon carbide-magnesium aluminum spinel refractory product according to claim 3, characterized in that: The lactate is at least one of aluminum lactate and magnesium lactate.
5. The silicon carbide-magnesium aluminum spinel refractory product according to claim 4, characterized in that: The alumina powder is calcined alumina powder or activated alumina powder.
6. The silicon carbide-magnesium aluminum spinel refractory product according to claim 5, characterized in that: The silicon carbide is fused silicon carbide, and the purity of the fused silicon carbide is ≥98.0%; the purity of the magnesia-alumina spinel powder is ≥99.0%, and the mass fraction of Al2O3 in the magnesia-alumina spinel powder is ≥72.0%.
7. The silicon carbide-magnesium aluminum spinel refractory product according to claim 6, characterized in that: The particle size of the passivated metal aluminum powder is 0.048-0.11 mm, the particle size of the aluminum oxide powder is 2-4 μm, and the water reducer is a polycarboxylic acid water reducer or a naphthalene water reducer.
8. The method for preparing the silicon carbide-magnesium aluminum spinel refractory product according to any one of claims 1 to 7, characterized in that: The following steps are involved: (1) Silicon carbide, magnesium aluminum spinel powder, binder, aluminum oxide powder, passivation metal aluminum powder, additives and water reducing agent are mixed uniformly to obtain a mixture; water is added to the mixture and mixed uniformly to obtain a slurry; (2) pouring the clay into a mold, curing at room temperature, demolding, and drying to obtain a blank; (3) calcining the blank at 1000° C. to 1600° C. in a nitrogen atmosphere to obtain a silicon carbide-magnesium aluminate spinel refractory product.
Citation Information
Patent Citations
Silicon carbide-magnesium aluminum spinel composite refractory material
CN107879753A
Preparation method of SiC-MgAl2O4-(Al2O3) x (AlN) 1-x multiphase refractory material
CN115073193A
Anti-hydration magnesia spinel brick and preparation method thereof
CN116102337A
A hydrotalcite structured catalyst using al as a substrate and a preparation method thereof
WO2007065323A1