In-situ synthesized SiBCN / graphene composite material and preparation method thereof

Through in-situ synthesis method, graphene is uniformly dispersed in SiBCN ceramics, and the problems of uniform dispersion of materials at high temperatures and improved electromagnetic wave absorption performance are solved, achieving good electromagnetic absorption performance and thermal stability.

CN118993744APending Publication Date: 2024-11-22JIANGSU MOGUI NEW MATERIAL CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411102026.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-12
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

SiBCN ceramic materials are difficult to uniformly disperse graphene at high temperatures, and traditional preparation methods are difficult to simultaneously improve the electromagnetic wave absorption performance and thermal stability of the material.

Method used

In situ synthesis method, the H2 released during polyborsilane (PBSZ) pyrolysis is used as a carrier, and the graphene is uniformly dispersed in the precursor solution with water-soluble sugars, and the SiBCN ceramics are retained during low-temperature pyrolysis. Amorphous structure to avoid heat damage to graphene.

Benefits of technology

The uniform dispersion of graphene in SiBCN ceramic materials and high temperature stability are achieved, which improves the electromagnetic absorption performance of the material, and reduces the difficulty of preparation and environmental impact.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118993744A_ABST
    Figure CN118993744A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of ceramic compositions, and particularly relates to an in-situ synthesis SiBCN / graphene composite material and a preparation method thereof.The preparation method comprises the following steps that S1, raw materials are mixed and dissolved, PBSZ, water-soluble saccharides and nitrate are dissolved in o-xylene, and a raw material solution is prepared; s2, placing the raw material solution in a protective atmosphere, heating the raw material solution to a ceramization temperature of PBSZ, carrying out heat preservation, and carrying out an in-situ reaction to prepare a SiBCN / graphene composite material; wherein the ceramization temperature ranges from 1100 DEG C to 1400 DEG C, and the heating rate ranges from 1 DEG C / min to 10 DEG C / min; h2 released in the pyrolysis process of polyborosilane (PBSZ) is used as a carrier similar to CH4 transition in a CVD deposition process, and is matched with water-soluble saccharides as a carbon source to be uniformly dispersed in a precursor solution, so that graphene can uniformly grow in a matrix, an amorphous structure of SiBCN ceramic is also retained by subsequent low-temperature pyrolysis, and the graphene is protected from thermal damage.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of ceramic compositions, and specifically relates to a ceramic composition based on borides, nitrides or silicides, and in particular to an in-situ synthesized SiBCN / graphene composite material and a preparation method thereof. Background Art

[0002] SiBCN ceramics are multifunctional ceramics with excellent oxidation resistance, extremely high temperature stability and tunable electromagnetic properties. They can be synthesized by thermal decomposition of pre-ceramic polymers. For the sake of highly sensitive precision electronic equipment and human health, the development of high-performance electromagnetic wave absorption devices to eliminate the harmful effects of electromagnetic radiation has become a hot topic of research; in addition to the basic properties of carbon materials for absorbing electromagnetic waves, such as high conductivity and large aspect ratio, graphene also has other advantages, such as the two-dimensional (2D) structure determines that graphene has a high specific surface area. Therefore, graphene is always introduced into the matrix to enhance the electromagnetic wave absorption performance. However, the role of graphene in promoting the wave absorption performance of SiBCN ceramics has not yet been clarified.

[0003] Traditional carbon-based composite materials cannot resist the damage of high temperature and oxidation, and the amorphous structure of SiBCN also indicates its poor EMW absorption performance. In order to expand the application prospects of materials, many scientists have conducted a lot of valuable research. For example, the method of adding multi-walled carbon nanotubes (MWCNTs) or SiC particles to the SiBCN matrix and annealing at high temperature has been greatly improved, but it is worth noting that in these methods, the materials are limited by two shortcomings, including the introduction of MWCNTs into the SiBCN matrix, which is difficult to disperse evenly in the matrix, and the improvement of electromagnetic wave absorption performance is at the expense of destroying the amorphous structure, which also reduces the thermal stability of the material.

[0004] By introducing graphene oxide into SiBCN ceramics and preparing bulk materials through hot pressing, the mechanical properties and ablation resistance of SiBCN / graphene composites are significantly improved. However, the two most difficult problems to overcome in SiBCN / graphene composites are uniform dispersion in the matrix and damage under high temperature. The current preparation methods cannot solve these problems at the same time.

[0005] Therefore, how to achieve both uniform dispersion and high-temperature stability of graphene in SiBCN ceramic materials is a technical problem that urgently needs to be solved in this field.

[0006] It should be noted that the above information disclosed in this background technology section is only used to understand the background technology of the present application concept, and therefore, the above description is not considered to constitute information of the prior art. Summary of the invention

[0007] The embodiments of the present disclosure at least provide an in-situ synthesized SiBCN / graphene composite material and a preparation method thereof.

[0008] In a first aspect, an embodiment of the present disclosure provides a method for preparing an in-situ synthesized SiBCN / graphene composite material, comprising the following steps: step S1, mixing and dissolving raw materials, dissolving PBSZ, water-soluble sugars, and nitrates in o-xylene to prepare a raw material solution; step S2, placing the raw material solution in a protective atmosphere, heating it to the ceramicization temperature of PBSZ, keeping it warm and conducting an in-situ reaction to prepare a SiBCN / graphene composite material; wherein the ceramicization temperature ranges from 1100-1400°C, and the heating rate is 1°C / min-10°C / min.

[0009] In an optional embodiment, the weight proportions of the raw materials in step S1 are: 7-20 parts of PBSZ; 0.5-2 parts of water-soluble sugars; 2-5 parts of nitrates; and 70-90 parts of o-xylene.

[0010] In an optional embodiment, the mixed dissolution of raw materials in step S1 specifically includes: dissolving PBSZ, water-soluble sugars, and nitrates in o-xylene, heating to 60°C-80°C in a water bath and stirring well, and preparing a raw material solution after complete dissolution.

[0011] In an optional embodiment, the nitrate comprises Ni(NO 3 ) 2 ,Ni(NO 3 ) 2 、KNO 3 and Ca(NO 3 ) 2 Any one or more combinations of .

[0012] In an optional embodiment, the water-soluble sugar is a high-purity water-soluble sugar with a ignition residue of less than 0.05% at 800° C. / 5 h, including any one or more combinations of sucrose, glucose, fructose and maltose.

[0013] In an optional embodiment, the heat preservation and in-situ reaction in step S2 specifically include: heat preservation for 1.5-4.5 hours, and then cooling; the cooling includes any one of furnace cooling and water cooling.

[0014] In an optional embodiment, the protective atmosphere in step S2 includes any one of nitrogen, argon or a vacuum environment.

[0015] In a second aspect, an embodiment of the present disclosure also provides an in-situ synthesized SiBCN / graphene composite material prepared by the method described above, wherein the mass fraction of the graphene in the in-situ synthesized SiBCN / graphene composite material is 1 wt.%-5 wt.%; the mass fraction of the SiBCN is 95 wt.%-99 wt.%.

[0016] In an optional embodiment, the ratio of ID / IG of the in-situ synthesized SiBCN / graphene composite material is in the range of 0.5-1.

[0017] In an optional embodiment, the dielectric loss of the in-situ synthesized SiBCN / graphene composite material is not less than 0.24.

[0018] The beneficial effect of the present invention is that the in-situ synthesized SiBCN / graphene composite material and the preparation method thereof utilize the H released during the pyrolysis of polyborosilane (PBSZ) to 2 , as similar to CH in CVD deposition process 4 The transitional carrier, combined with water-soluble sugars as carbon sources, is evenly dispersed in the precursor solution, allowing graphene to grow evenly in the matrix. The subsequent low-temperature pyrolysis also retains the amorphous structure of the SiBCN ceramic, protecting the graphene from thermal damage. In addition, water-soluble sugars replace traditional resins and asphalt, which improves environmental friendliness while reducing the difficulty of preparation. The SiBCN / graphene composite material synthesized in one step can have good electromagnetic absorption properties.

[0019] Other features and advantages of the present invention will be described in the following description, and partly become apparent from the description, or understood by practicing the present invention. The purpose and other advantages of the present invention are realized and obtained by the structures particularly pointed out in the description, claims and drawings.

[0020] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, preferred embodiments are given below and described in detail with reference to the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0022] Figure 1XRD diagram of the phase composition of G / SiBCN and SiBCN pyrolysis samples after 1200°C pyrolysis provided in the embodiments of the present disclosure; Figure 2 Raman images of the structure and composition of G / SiBCN and SiBCN pyrolysis samples after 1200°C pyrolysis provided in the embodiments of the present disclosure; Figure 3 TEM image of G / SiBCN provided for the embodiments of the present disclosure; Figure 4 XPS fitting curves of SiBCN and G / SiBCN provided in the embodiments of the present disclosure; Figure 5 Graphs showing the dielectric properties and electromagnetic wave absorption properties of the two samples, G / SiBCN and SiBCN, provided in the embodiments of the present disclosure. DETAILED DESCRIPTION

[0023] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution of the present invention will be clearly and completely described below in conjunction with the accompanying drawings. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0024] As used herein, the phrases "in one embodiment," "according to one embodiment," "in some embodiments," and the like generally refer to the fact that the particular feature, structure, or characteristic following the phrase may be included in at least one embodiment of the present disclosure. Therefore, a particular feature, structure, or characteristic may be included in more than one embodiment of the present disclosure, so that these phrases do not necessarily refer to the same embodiment. As used herein, the terms "example," "exemplary," and the like are used to "serve as an example, instance, or illustration." Any implementation, aspect, or design described herein as "example" or "exemplary" is not necessarily to be construed as preferred or superior to other implementations, aspects, or designs. On the contrary, the use of the terms "example," "exemplary," and the like is intended to present concepts in a concrete manner.

[0025] Herein, example embodiments of the present disclosure will be described in more detail with reference to the accompanying drawings. As used herein, expressions such as "at least one of..." modify the entire list of elements when following a list of elements, rather than modifying individual elements in the list. For example, the expression "at least one of a, b, and c" should be understood to include only a, only b, only c, both a and b, both a and c, both b and c, or all of a, b, and c.

[0026] The terms used herein are only used to describe specific exemplary configurations and are not intended to be limited. As used herein, the singular articles "one", "an" and "the" may also be intended to include plural forms, unless it is clearly indicated above that this is not the case. The terms "comprise", "include" and "have" are inclusive, and therefore specify the presence of features, steps, operations, elements and / or components, but do not exclude the presence or addition of one or more other features, steps, operations, elements, components and / or combinations thereof. The method steps, processes and operations described herein should not be interpreted as necessarily requiring them to be performed in the specific order discussed or shown, unless specifically identified as an execution order. Additional or alternative steps may be adopted.

[0027] As an excellent modifying material, graphene is used to modify the mechanical and electrical properties of various materials. However, the high-temperature preparation of SiBCN ceramic materials will inevitably destroy the structural integrity of graphene, thus affecting the modification effect.

[0028] The defects existing in the above solutions are the results obtained by the inventor after practice and careful research. Therefore, the discovery process of the above problems and the solutions proposed by the present disclosure for the above problems below should be the contributions made by the inventor to the present disclosure during the disclosure process.

[0029] In the embodiments of the present disclosure, specifically, the SiBCN / graphene composite material may also be abbreviated as G / SiBCN.

[0030] The disclosed embodiment provides a method for preparing an in-situ synthesized SiBCN / graphene composite material, comprising the following steps: step S1, mixing and dissolving raw materials, dissolving PBSZ, water-soluble sugars, and nitrates in o-xylene to prepare a raw material solution; step S2, placing the raw material solution in a protective atmosphere, heating it to the ceramicization temperature of PBSZ, keeping the temperature and performing an in-situ reaction to prepare the SiBCN / graphene composite material; wherein the ceramicization temperature ranges from 1100 to 1400°C, and the heating rate is 1°C / min to 10°C / min.

[0031] In the embodiment of the present disclosure, specifically, the mass proportions of the raw materials in step S1 are: 7-20 parts of PBSZ; 0.5-2 parts of water-soluble sugars; 2-5 parts of nitrates; 70-90 parts of o-xylene; wherein the water-soluble sugars are used as carbon sources, polyborosilane (PBSZ) is used as boron source and silicon source, nitrate is used as nitrogen source, and o-xylene is used as solvent to form a mixed solvent.

[0032] In the embodiments of the present disclosure, specifically, in the mixed solution, the mass ratio of polyborosilane (PBSZ), water-soluble sugars, nitrates and o-xylene is 100:10-50:10-40:800-1000, preferably 100:10:10:800, 100:10:30:900, 100:20:30:900, 100:10:25:900, 100:10:25:1000, 100:10:30:1000 and 100:10:20:900.

[0033] In the disclosed embodiment, specifically, the mixed dissolution of raw materials in step S1 specifically includes: dissolving PBSZ, water-soluble sugars, and nitrates in o-xylene, heating to 60°C-80°C in a water bath and stirring well, and preparing a raw material solution after complete dissolution.

[0034] In the embodiment of the present disclosure, specifically, the nitrate includes Ni(NO 3 ) 2 ,Ni(NO 3 ) 2 、KNO 3 and Ca(NO 3 ) 2 Any one or more combinations of .

[0035] In the embodiments of the present disclosure, specifically, the water-soluble sugar is a high-purity water-soluble sugar with a ignition residue of less than 0.05% at 800°C / 5h, including any one or more combinations of sucrose, glucose, fructose and maltose, preferably analytically pure or chemically pure components.

[0036] In the embodiments of the present disclosure, specifically, the total heating time is preferably 10h, 15h, 20h, 25h, 30h, 35h, 40h, 45h, 50h, 55h, 60h, 65h, 70h, 75h, 80h, 85h, 90h, 95h and 100h; the heating temperature is preferably 1150℃, 1180℃, 1200℃, 1220℃, 1250℃ and 1300℃; the holding time is preferably 1h, 1.5h, 2.0h, 2.5h, 3.0h, 3.5h, 4.0h, 4.5h, 5.0h, 5.5h and 6.0h.

[0037] In the embodiment of the present disclosure, specifically, the heat preservation and in-situ reaction in step S2 specifically include: heat preservation for 1.5-4.5 hours, and then cooling; the cooling includes any one of furnace cooling and water cooling.

[0038] In the embodiments of the present disclosure, specifically, the protective atmosphere in step S2 includes any one of nitrogen, argon or a vacuum environment; wherein the purity of the nitrogen is preferably 99.8%, 99.9%, 99.98%, 99.99% and 99.998%; the purity of the argon is preferably 99.8%, 99.9%, 99.98%, 99.99% and or 99.998%.

[0039] In the embodiments disclosed herein, specifically, when the temperature is kept at 2 hours, a good reaction is basically achieved, and a SiBCN / graphene composite material is obtained. The preparation process is simple, the raw materials are green and cheap, and the overall cost is low.

[0040] The disclosed embodiment also provides an in-situ synthesized SiBCN / graphene composite material prepared by the method as described above, wherein the mass fraction of graphene in the in-situ synthesized SiBCN / graphene composite material is 1 wt.%-5wt.%; the mass fraction of SiBCN is 95 wt.%-99 wt.%.

[0041] In the embodiments of the present disclosure, specifically, the ratio of ID / IG of the in-situ synthesized SiBCN / graphene composite material is in the range of 0.5-1.

[0042] In the embodiments of the present disclosure, specifically, the dielectric loss of the in-situ synthesized SiBCN / graphene composite material is not less than 0.24.

[0043] Some embodiments of the present invention are described in detail below in conjunction with the accompanying drawings. In the absence of conflict, the following embodiments and features in the embodiments can be combined with each other.

[0044] Example 1: Weigh 10 g polyborosilane (PBSZ), 1 g analytically pure glucose monohydrate (C 6 H 12 O 6 ·H 2 O, theoretical carbon content 36.4%), 2.4g Ni(NO 3 ) 2 Put it in a 5000ml beaker, add 90g of o-xylene and stir evenly.

[0045] The mixed solution was poured into a quartz crucible, placed in a high-temperature furnace protected by argon gas and kept at 1200°C for 2 hours, and a black irregular powder-like substance was obtained after taking it out, which was the SiBCN / graphene composite material; See also Figure 1 and Figure 2From the analysis of XRD and Raman data, it can be seen that the samples pyrolyzed with sugar and pyrolyzed without sugar are represented by G / SiBCN and SiBCN, respectively. The G / SiBCN curve has a significant peak at 26.3 degrees, which is consistent with the (002) peak of graphene. In addition, it should be noted that both curves are typical amorphous characteristic curves, that is, the precursor remains amorphous below 1200°C. The Raman spectrum of SiBCN ceramics has no characteristic peaks. The G / SiBCN precursor has been transformed into a ceramic without residual carbon, and its Raman spectrum has representative free carbon peaks at both the disordered bond (D) and graphite (G) peaks. The ID / IG ratio of G / SiBCN is greater than 0.5 but less than 1, indicating that the defect density is very small. The morphology of the 2D peak is clear and symmetrical, and only one Lorentz peak can be fitted, proving that graphene is almost a single layer.

[0046] See also Figure 3 , from the TEM analysis, it can be seen that the bright white area in the bright field image is ceramic particles, the cotton-like area is graphene, and several graphene sheets overlap randomly to form a texture structure. This structure can increase the specific surface area of ​​the composite material and consume the energy of electromagnetic waves during transmission. The diffraction spots indicate that the graphene is a hexagonal structure. In addition, the stripes in the HRTEM image indicate that the graphene is three to four layers. It can be seen that even without a catalyst, the in-situ growth of graphene still has a good structure.

[0047] See also Figure 4 From the XPS analysis, we can see that the BNC peak can be observed, indicating that graphene generates a BCN structure through lattice doping. After in-situ growth of graphene, the chemical bond of the B element in SiBCN is transformed into a stronger binding state. The existence of the CBN bond indicates that graphene forms a stable chemical bond with the ceramic, rather than van der Waals force.

[0048] See also Figure 5 , from the analysis of electromagnetic wave absorption performance, it can be seen that pure SiBCN ceramics have extremely low dielectric constant and dielectric loss. The main reason is that the amorphous structure lacks grain boundaries. After the introduction of graphene, its dielectric properties have been significantly improved. The dielectric loss of G / SiBCN composite material reaches 0.54, which is 4 times that of bare SiBCN ceramics. Uniform graphene forms a large number of highly connected networks, which improves the overall conductivity. The electromagnetic wave absorption curves at different thicknesses are calculated here. Pure SiBCN ceramics have almost no absorption performance, while the bottom of the curve of G / SiBCN composite material gradually moves to high frequency as the thickness decreases. When the thickness is fixed at 2mm, the effective absorption band ranges from 13.1 to 17.8 GHz, almost covering the Ku band. When it reaches 3mm, the EMW increases from 8.2 GHz to 12.1 GHz, completely covering the X band.

[0049] In summary, the in-situ synthesized SiBCN / graphene composite material and the preparation method thereof of the present invention utilize the H released during the pyrolysis of polyborosilane (PBSZ) to 2 , as similar to CH in CVD deposition process 4 The transitional carrier, combined with water-soluble sugars as carbon sources, is evenly dispersed in the precursor solution, allowing graphene to grow evenly in the matrix. The subsequent low-temperature pyrolysis also retains the amorphous structure of the SiBCN ceramic, protecting the graphene from thermal damage. In addition, water-soluble sugars replace traditional resins and asphalt, which improves environmental friendliness while reducing the difficulty of preparation. The SiBCN / graphene composite material synthesized in one step can have good electromagnetic absorption properties.

[0050] Based on the above ideal embodiments of the present invention, the relevant staff can make various changes and modifications without departing from the technical concept of the present invention through the above description. The technical scope of the present invention is not limited to the contents of the specification, and its technical scope must be determined according to the scope of the claims.

Claims

1. A method for preparing an in-situ synthesized SiBCN / graphene composite material, characterized in that: The steps include: Step S1, mixing and dissolving raw materials, dissolving PBSZ, water-soluble sugars, and nitrates in o-xylene to prepare a raw material solution; Step S2, placing the raw material solution in a protective atmosphere, heating it to the ceramic temperature of PBSZ, keeping it warm and performing an in-situ reaction to prepare a SiBCN / graphene composite material; wherein The ceramicization temperature ranges from 1100 to 1400° C., and the heating rate is from 1° C. / min to 10° C. / min.

2. The method for preparing the in-situ synthesized SiBCN / graphene composite material according to claim 1, wherein: The mass proportions of the raw materials in step S1 are: 7-20 parts of PBSZ; 0.5-2 parts of water-soluble sugars; 2-5 parts of nitrates; and 70-90 parts of o-xylene.

3. The method for preparing the in-situ synthesized SiBCN / graphene composite material as claimed in claim 1, characterized in that: The mixed dissolution of raw materials in step S1 specifically includes: dissolving PBSZ, water-soluble sugars, and nitrates in o-xylene, heating to 60° C.-80° C. in a water bath, stirring thoroughly, and preparing a raw material solution after the mixture is completely dissolved.

4. The method for preparing the in-situ synthesized SiBCN / graphene composite material as claimed in claim 1, characterized in that: The nitrate includes any one or more combinations of Ni(NO3)2, Ni(NO3)2, KNO3 and Ca(NO3)2.

5. The method for preparing the in-situ synthesized SiBCN / graphene composite material as claimed in claim 1, characterized in that: The water-soluble sugar is a high-purity water-soluble sugar with a ignition residue of less than 0.05% at 800°C / 5h, including any one or more combinations of sucrose, glucose, fructose and maltose.

6. The method for preparing the in-situ synthesized SiBCN / graphene composite material according to claim 1, characterized in that: The step S2 of heat preservation and in-situ reaction specifically includes: heat preservation for 1.5-4.5 hours, and then cooling; The cooling includes any one of furnace cooling and water cooling.

7. The method for preparing the in-situ synthesized SiBCN / graphene composite material according to claim 1, characterized in that: The protective atmosphere in step S2 includes any one of nitrogen, argon or vacuum environment.

8. An in-situ synthesized SiBCN / graphene composite material prepared by the method according to any one of claims 1 to 7, characterized in that: The in-situ synthesized SiBCN / graphene composite material The mass fraction of the graphene is 1 wt.%-5 wt.%; The mass fraction of the SiBCN is 95 wt.%-99 wt.%.

9. The in-situ synthesized SiBCN / graphene composite material according to claim 8, characterized in that: The ID / IG ratio of the in-situ synthesized SiBCN / graphene composite material is in the range of 0.5-1.

10. The in-situ synthesized SiBCN / graphene composite material according to claim 8, characterized in that: The dielectric loss of the in-situ synthesized SiBCN / graphene composite material is not less than 0.24.

Citation Information

Patent Citations

  • Graphene-reinforced silicon-boron-carbon-nitrogen ceramic composite material and preparation method thereof

    CN104529468A

  • SiBCN composite ceramic powder and preparation method thereof

    CN109970451A

  • Graphene oxide modified SiBCN ceramic temperature sensor and preparation method thereof

    CN115745626A

  • Bulk compact amorphous SiBCN ceramic block and preparation method thereof

    CN117902903A

  • Reduced graphene-cobalt chromate composite composition for humidity sensor applications and its fabrication process and system

    US20230221273A1