Aerogel atomizing core, preparation method thereof and electronic cigarette

Silicon nitride fiber aerogel atomization core is prepared by using slurry sintering and chemical vapor phase impregnation methods of silicon nitride fiber aerosol in the electronic cigarette atomization core, which solves the problem of small pore size and slow oil conduction in the traditional method. Problem, high-efficiency atomization performance and low environmental pollution have been achieved.

CN118993758APending Publication Date: 2024-11-22SHENZHEN BAUHINIA FUTURE TECHNOLOGY CO LTD

Patent Information

Application Number
CN202411193352.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-28
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The traditional aerogel atomization core preparation method has problems such as small pore size, slow oil conduction, insufficient atomization amount, insufficient strength, and easy powder loss.

Method used

By molding the slurry containing a silicon source, a carbon source and a thickener, the silicon nitride fiber aerogel matrix is ​​sintered to form a silicon nitride fiber aerogel matrix, and carbon is formed on the surface and inside of the silicon nitride fiber aerogel matrix by chemical vapor phase impregnation method. Coating, prepare aerogel atomized core.

Benefits of technology

The prepared aerogel atomized core has excellent atomization performance of high porosity, high pore size, and large oil conduction, which improves the use effect of electronic cigarettes and has low environmental pollution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118993758A_ABST
    Figure CN118993758A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of electronic cigarettes, in particular to an aerogel atomizing core, a preparation method thereof and an electronic cigarette. The preparation method of the aerogel atomizing core comprises the following steps: carrying out molding treatment on slurry containing a silicon source, a carbon source and a thickening agent to prepare a green body; carrying out sintering treatment on the green body to prepare a silicon nitride fiber aerogel matrix; carbon coatings are formed on the surface and inside the silicon nitride fiber aerogel matrix through a chemical vapor impregnation method, and inorganic fiber aerogel is prepared; and forming a heating layer on the inorganic fiber aerogel to prepare the aerogel atomizing core. According to the preparation method provided by the invention, the use of a large amount of organic solvent can be avoided, the environmental pollution is extremely low, and the prepared aerogel atomizing core has the advantages of high mechanical strength, high porosity, large aperture and fast oil guide, and shows excellent oil guide and atomization performance, so that the use effect of the electronic cigarette is effectively improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of electronic cigarettes, and in particular to an aerogel atomization core, a preparation method thereof, and an electronic cigarette. Background Art

[0002] Electronic cigarettes are electronic products that produce aerosols with a specific smell by atomizing the e-liquid through heating. They are favored by consumers because of their advantages such as no second-hand smoke, no smoke odor, and can reduce the intake of harmful substances. Electronic cigarettes include components such as the smoke pipe for holding the e-liquid, the mouthpiece, the atomizer core, and the power supply. As the core component of the electronic cigarette, the performance of the atomizer core directly affects the use effect of the electronic cigarette.

[0003] At present, the main material of atomizer core is organic cotton, but organic cotton is easy to decompose at high temperature, producing harmful substances, which affects the health of users. It is necessary to find a high temperature resistant, non-toxic and efficient atomizer core material. Aerogel materials are widely used in heat insulation, sound absorption, adsorption and other fields due to their high porosity, low density, high specific surface area and other characteristics. It is an ideal material for preparing atomizer core. However, aerogel atomizer cores prepared by traditional methods have various problems such as small pore size, slow oil conduction, insufficient atomization volume, insufficient strength, and easy powder loss. Summary of the invention

[0004] Based on this, there is a need for an aerogel atomization core and a preparation method thereof and an electronic cigarette to solve various problems of aerogel atomization core prepared by traditional methods, such as small pore size, slow oil conduction, insufficient atomization amount, insufficient strength, easy powder loss, etc.

[0005] The above-mentioned purpose of the present application is achieved through the following technical solutions:

[0006] In a first aspect of the present application, a method for preparing an aerogel atomization core is provided, comprising the following steps:

[0007] Performing molding treatment on the slurry containing the silicon source, the carbon source and the thickener to prepare a green body;

[0008] Sintering the green body to prepare a silicon nitride fiber aerogel matrix;

[0009] Forming a carbon coating on the surface and inside of the silicon nitride fiber aerogel matrix by chemical vapor impregnation to prepare an inorganic fiber aerogel;

[0010] A heating layer is formed on the inorganic fiber aerogel to prepare an aerogel atomization core.

[0011] In one embodiment, the green body is sintered, comprising the following steps:

[0012] In a nitrogen atmosphere, the green body is subjected to a sintering treatment to cause a carbothermal reduction reaction between the silicon source and the carbon source and to generate silicon nitride nanofibers in situ, thereby preparing an intermediate;

[0013] The intermediate is subjected to secondary sintering treatment in an air atmosphere to prepare the silicon nitride fiber aerogel matrix.

[0014] In one embodiment, the sintering temperature of the primary sintering treatment is 1400° C. to 1700° C., and the holding time is 0.5 h to 24 h.

[0015] In one of the embodiments, the sintering temperature of the secondary sintering treatment is 600° C. to 1100° C., and the holding time is 0.1 h to 6 h.

[0016] In one embodiment, the silicon source includes one or more of silicon powder, silicon carbide powder, silicon nitride powder, silicon dioxide powder, molybdenum disilicide powder and silica sol.

[0017] In one embodiment, the carbon source includes one or more of carbon powder, graphite powder and carbon fiber.

[0018] In one embodiment, the thickener includes one or more of sol, cellulose, cellulose derivatives, starch and polymethyl methacrylate.

[0019] In one embodiment, the molar ratio of silicon to carbon in the slurry is 1:(1-10).

[0020] In one embodiment, the molding process includes one or more of a normal temperature pressure molding process, a hot die casting molding process, and an injection molding process.

[0021] In one embodiment, the chemical vapor impregnation method comprises the following steps:

[0022] In an atmosphere containing volatile organic matter, the silicon nitride fiber aerogel matrix is ​​subjected to a chemical vapor impregnation treatment to form a carbon coating on the surface and inside of the silicon nitride fiber aerogel matrix.

[0023] In one embodiment, the volatile organic compounds include one or more of methane, ethane, propane, ethylene, acetylene and propylene.

[0024] In one embodiment, the atmosphere containing volatile organic compounds further contains a carrier gas, and the flow ratio of the volatile organic compounds to the carrier gas is 1:(0.5~5.0).

[0025] In one embodiment, the conditions of the chemical vapor impregnation treatment include: pressure of 100Pa~10000Pa, temperature of 600℃~1300℃, and time of 0.5h~12h.

[0026] In one embodiment, the thickness of the carbon coating is 1 nm to 500 nm.

[0027] In a second aspect of the present application, an aerogel atomization core is provided, which is prepared by the method for preparing an aerogel atomization core as described above.

[0028] In one embodiment, the porosity of the aerogel atomization core is 50% to 98%.

[0029] In one embodiment, the pore size of the aerogel atomization core is 5 μm to 50 μm.

[0030] In one embodiment, the volume density of the aerogel atomization core is 5 mg / cm 3 ~5000mg / cm 3 .

[0031] In a third aspect of the present application, an electronic cigarette is provided, comprising the aerogel atomization core as described above.

[0032] This application has at least the following beneficial effects:

[0033] The present application forms a slurry containing a silicon source, a carbon source and a thickener to obtain a green body, and adopts an inorganic fiber growth technology so that the silicon source and the carbon source in the green body generate a large amount of silicon nitride nanofibers in situ during the high-temperature sintering process, thereby forming a silicon nitride fiber aerogel matrix with a three-dimensional porous network structure. At the same time, a carbon coating is formed on the surface and inside of the silicon nitride fiber aerogel matrix by chemical vapor impregnation treatment, which can increase the diameter of the silicon nitride nanofibers, and form fixed nodes between the silicon nitride nanofibers, thereby achieving the effect of enhancing mechanical strength. Compared with the traditional method, the preparation method of the aerogel atomization core provided by the present application can not only avoid the use of a large amount of organic solvents, and the environmental pollution is extremely low, and the aerogel atomization core obtained has the advantages of high mechanical strength, high porosity, large pore size, and fast oil conduction, showing excellent atomization performance, thereby effectively improving the use effect of electronic cigarettes. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] In order to more clearly illustrate the technical solutions in the embodiments of the present application and to more completely understand the present application and its beneficial effects, the following is a brief introduction to the drawings required for the description of the embodiments. Obviously, the drawings described below are only some embodiments of the present application, and those skilled in the art can obtain other drawings based on these drawings without creative work.

[0035] Figure 1 Schematic diagram of a process for preparing an aerogel atomization core in one embodiment;

[0036] Figure 2 This is the SEM image of the aerogel atomization core prepared in Example 1. DETAILED DESCRIPTION

[0037] In order to facilitate the understanding of the present application, the present application is further described in detail below in conjunction with specific embodiments. However, the present application can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the understanding of the disclosure of the present application more thorough and comprehensive.

[0038] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which this application belongs. The terms used herein in the specification of this application are only for the purpose of describing specific embodiments and are not intended to limit this application.

[0039] In the present application, the meaning of "and / or" includes any and all combinations of one or more related listed items. "At least one" means more than one, such as one, two and more than two. "Multiple" or "several" means at least two, such as two, three, etc., and "multi-layer" means at least two layers, such as two layers, three layers, etc., unless otherwise clearly and specifically defined. In the description of the present application, "several" means at least one, such as one, two, etc., unless otherwise clearly and specifically defined.

[0040] When a numerical range is disclosed in this application, the above range is considered to be continuous and includes the minimum and maximum values ​​of the range, as well as every value between such minimum and maximum values. Further, when a range refers to an integer, every integer between the minimum and maximum values ​​of the range is included. In addition, when multiple ranges are provided to describe features or characteristics, the ranges can be combined. In other words, unless otherwise indicated, all ranges disclosed in this application should be understood to include any and all subranges included therein.

[0041] Unless otherwise specified, all steps of the present application may be performed sequentially or randomly. For example, the method includes steps (a) and (b), which means that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may also include step (c), which means that step (c) may be added to the method in any order. For example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.

[0042] In this application, "above" or "below" includes the number itself. For example, "1 below" includes 1.

[0043] The temperature parameters in this application, unless otherwise specified, are allowed to be either constant temperature treatment or to vary within a certain temperature range. It should be understood that the constant temperature treatment allows the temperature to fluctuate within the accuracy range controlled by the instrument. Fluctuations within the range of ±5°C, ±4°C, ±3°C, ±2°C, and ±1°C are allowed.

[0044] In the present application, room temperature refers to indoor temperature, normal temperature or general temperature. Generally speaking, the range of room temperature can be any one of the following temperature intervals: 23°C ± 2°C, 25°C ± 5°C or 20°C ± 5°C.

[0045] Inorganic fiber aerogel material is an aerogel material that uses inorganic nanofibers as building blocks and forms a three-dimensional porous network structure by overlapping inorganic nanofibers. It is considered to be an ideal atomizer core material due to its excellent mechanical properties and chemical stability. However, the traditional method of preparing aerogel atomizer cores usually requires the use of a large amount of organic solvents, which is not only costly but also causes serious pollution to the environment. It has been reported that physical or chemical methods are used to mix ethyl orthosilicate with anhydrous ethanol and water, and the sol-gel method and supercritical drying method are used to prepare silica aerogel atomizer cores. The aerogel material prepared by this method is easy to break, very difficult to assemble, and easy to fall off. In addition, its pore size is nanometer-scale. Although the porosity is high and the oil absorption is high, the small pore size makes the oil conduction speed very slow, which will lead to a serious lack of smoke.

[0046] Based on this, in the first aspect of the present application, a method for preparing an aerogel atomization core is provided to solve various problems of aerogel atomization core prepared by traditional methods, such as small pore size, slow oil conduction, insufficient atomization amount, insufficient strength, and easy powder loss.

[0047] See also Figure 1 , which is a schematic flow chart of a method for preparing an aerogel atomizer core in an embodiment. In some embodiments, the method for preparing an aerogel atomizer core comprises the following steps:

[0048] S100: forming a slurry containing a silicon source, a carbon source and a thickener to prepare a green body;

[0049] S200: sintering the green body to prepare a silicon nitride fiber aerogel matrix;

[0050] S300: Forming a carbon coating on the surface and inside of a silicon nitride fiber aerogel matrix by chemical vapor impregnation treatment to prepare an inorganic fiber aerogel;

[0051] S400: forming a heating layer on the inorganic fiber aerogel to prepare an aerogel atomization core.

[0052] The present application forms a slurry containing a silicon source, a carbon source and a thickener to obtain a green body, and adopts an inorganic fiber growth technology so that the silicon source and the carbon source in the green body generate a large amount of silicon nitride nanofibers in situ during the high-temperature sintering process, thereby forming a silicon nitride fiber aerogel matrix with a three-dimensional porous network structure. At the same time, a carbon coating is formed on the surface and inside of the silicon nitride fiber aerogel matrix by chemical vapor impregnation treatment, which can increase the diameter of the silicon nitride nanofibers, and form fixed nodes between the silicon nitride nanofibers, thereby achieving the effect of enhancing mechanical strength. Compared with the traditional method, the preparation method of the aerogel atomization core provided by the present application can not only avoid the use of a large amount of organic solvents, and the environmental pollution is extremely low, and the aerogel atomization core obtained has the advantages of high mechanical strength, high porosity, large pore size, and fast oil conduction, showing excellent atomization performance, thereby effectively improving the use effect of electronic cigarettes.

[0053] The following is an explanation of the preparation method of the aerogel atomization core in a step-by-step manner.

[0054] S100: forming a slurry containing a silicon source, a carbon source and a thickener to prepare a green body.

[0055] Optionally, the silicon source includes one or more of silicon (Si) powder, silicon carbide (SiC) powder, silicon nitride (Si3N4) powder, silicon dioxide (SiO2) powder, molybdenum disilicide (MoSi2) powder and silica sol, and may further be silicon powder.

[0056] Optionally, the carbon source includes one or more of carbon powder, graphite powder and carbon fiber, and may further be carbon powder.

[0057] Optionally, the thickener includes one or more of sol, cellulose, cellulose derivatives, starch and polymethyl methacrylate (PMMA), and further optionally cellulose.

[0058] It can be understood that the sol includes one or more of silica sol, aluminum sol, titanium sol and zirconium sol, wherein the silica sol can be used as both a silicon source and a thickener. Cellulose derivatives refer to the product of esterification or etherification of hydroxyl groups in cellulose molecules, which can be divided into three categories: cellulose ether, cellulose ester and cellulose ether ester. Common cellulose derivatives include: methyl cellulose, ethyl cellulose, hydroxyethyl cellulose, hydroxypropyl cellulose, hydroxypropyl methyl cellulose, carboxymethyl cellulose, nitrocellulose, cellulose acetate, cellulose acetate phthalate, cellulose acetate butyrate, cellulose sulfonate, cellulose nitrate, cellulose acetate, cellulose acetate butyrate and cellulose xanthate. Cellulose, cellulose derivatives, starch and PMMA are mainly used as thickeners and can also be used as carbon sources.

[0059] In the present application, silicon source is selected from silicon powder, silicon carbide powder and other raw materials, carbon source is selected from carbon powder, graphite powder and other raw materials, thickener is selected from cellulose, starch and other raw materials, and the price of all raw materials is low, which is conducive to reducing the production cost of aerogel atomization core.

[0060] Optionally, the particle sizes of the silicon source, the carbon source and the thickener are each independently 10 mesh to 200 mesh, for example, 10 mesh, 20 mesh, 40 mesh, 60 mesh, 80 mesh, 100 mesh, 120 mesh, 140 mesh, 160 mesh, 180 mesh or 200 mesh.

[0061] It can be understood that mesh number is a unit for measuring particle size, 10 mesh corresponds to a pore size of about 2000 μm, and 200 mesh corresponds to a pore size of about 74 μm, that is, the particle sizes of the silicon source, the carbon source and the thickener are each independently 74 μm to 2000 μm, for example, 74 μm, 100 μm, 150 μm, 200 μm, 400 μm, 600 μm, 800 μm, 1000 μm, 1200 μm, 1400 μm, 1600 μm, 1800 μm or 2000 μm.

[0062] Optionally, the molar ratio of silicon to carbon in the green body is 1:(1-10), such as 1:1, 1:2, 1:3, 1:4, 1:5, 1:6, 1:7, 1:8, 1:9 or 1:10, and can further be 1:(5-10).

[0063] During the sintering process, if the reaction conditions are not controlled properly, part of the carbon source will undergo side reactions and cause loss, resulting in the inability of the silicon powder to fully react. Therefore, appropriately increasing the amount of carbon source can compensate for the loss of carbon source and the inadequate reaction of the silicon source.

[0064] Optionally, the dispersion medium in the slurry includes one or more of water, methanol, ethanol and isopropanol, and can further be water. The water can be one or more of tap water, deionized water, pure water, ultrapure water, distilled water and reverse osmosis water. The use of tap water is conducive to reducing costs, and the use of deionized water or pure water is conducive to improving the quality of the aerogel material.

[0065] Optionally, the solid content of the slurry is 50% to 90%, for example 50%, 55%, 60%, 65%, 70%, 75%, 80%, 85% or 90%.

[0066] Optionally, the solid content of the green body is 60% to 99%, for example 60%, 65%, 70%, 75%, 80%, 85%, 90%, 95% or 99%.

[0067] Optionally, the molding process includes one or more of a normal temperature pressure molding process, a hot die casting molding process and an injection molding process, and further optionally a normal temperature pressure molding process.

[0068] S200: Sintering the green body to prepare a silicon nitride fiber aerogel matrix.

[0069] Optionally, the green body is subjected to a sintering process, comprising the following steps:

[0070] S210: performing a sintering treatment on the green body in a nitrogen atmosphere to cause a carbothermal reduction reaction between the silicon source and the carbon source and to generate silicon nitride nanofibers in situ, thereby preparing an intermediate;

[0071] S220: performing secondary sintering treatment on the intermediate in an air atmosphere to prepare a silicon nitride fiber aerogel matrix.

[0072] The present application uses a primary sintering treatment in a nitrogen atmosphere to generate silicon-containing gas and carbon-containing gas from the silicon source and carbon source in the green body at high temperature, and a carbon thermal reduction reaction occurs between the silicon-containing gas and the carbon-containing gas, thereby generating a large number of Si3N4 nanofibers in situ, and then the Si3N4 nanofibers overlap each other to form an intermediate with a three-dimensional porous network structure. Through a secondary sintering treatment in an air atmosphere, the residual unreacted raw materials (such as excess carbon source or thickener) in the intermediate can be removed, thereby obtaining a pure Si3N4 fiber aerogel matrix.

[0073] Optionally, the sintering temperature of the primary sintering process is 1400°C to 1700°C, and the holding time is 0.5h to 24h. As an example, the sintering temperature of the primary sintering process may be 1400°C, 1450°C, 1500°C, 1550°C, 1600°C, 1650°C or 1700°C, and the holding time may be 0.5h, 1h, 2h, 4h, 6h, 8h, 10h, 12h, 14h, 16h, 18h, 20h, 22h or 24h.

[0074] Optionally, the sintering temperature of the secondary sintering treatment is 600°C to 1100°C, and the holding time is 0.1h to 6h. As an example, the sintering temperature of the secondary sintering treatment may be 600°C, 650°C, 700°C, 750°C, 800°C, 850°C, 900°C, 950°C, 1000°C, 1050°C or 1100°C, and the holding time may be 0.1h, 0.5h, 1h, 1.5h, 2h, 2.5h, 3h, 3.5h, 4h, 4.5h, 5h, 5.5h or 6h.

[0075] Optionally, the silicon nitride nanofibers in the silicon nitride fiber aerogel matrix meet the following conditions: (1) a diameter of 50 nm to 500 nm, for example, 50 nm, 100 nm, 150 nm, 200 nm, 250 nm, 300 nm, 350 nm, 400 nm, 450 nm or 500 nm, and further optionally 198 nm to 230 nm; (2) a length ≥ 10 μm, for example, 10 μm, 15 μm, 20 μm, 25 μm, 30 μm, 35 μm, 40 μm, 45 μm, 50 μm or 100 μm, and further optionally 12 μm to 36 μm.

[0076] Optionally, the volume density of the silicon nitride fiber aerogel matrix is ​​1000 mg / cm 3 ~10000mg / cm 3 , for example 1000mg / cm 3 、2000mg / cm 3 、3000mg / cm 3 、4000mg / cm 3 , 5000mg / cm 3 、6000mg / cm 3 、7000mg / cm 3 、8000mg / cm 3 , 9000mg / cm 3 or 10000mg / cm 3 .

[0077] Compared with aerogel materials prepared by traditional methods, the silicon nitride fiber aerogel matrix prepared by molding and sintering processes in the present application not only has high porosity and large pore size, but also has higher strength.

[0078] S300: Forming a carbon coating on the surface and inside of a silicon nitride fiber aerogel matrix through chemical vapor impregnation treatment to prepare an inorganic fiber aerogel.

[0079] Optionally, the chemical vapor impregnation method includes the following steps: performing chemical vapor impregnation treatment on the silicon nitride fiber aerogel matrix in an atmosphere containing volatile organic matter to form a carbon coating on the surface and inside of the silicon nitride fiber aerogel matrix.

[0080] It can be understood that Chemical Vapor Infiltration (CVI) is an important process for surface modification of materials. In CVI treatment, a gaseous precursor containing the target element is introduced into the reaction chamber. Under certain temperature and pressure conditions, the gaseous precursor is deposited on the surface or in the pores of the material through chemical reaction, thereby improving the strength and toughness of the material.

[0081] It can be understood that volatile organic compounds (VOCs) refer to organic compounds with high vapor pressure and volatile properties at normal temperature and pressure. During the CVI process, volatile organic compounds will decompose and deposit on the surface and inside of the silicon nitride fiber aerogel matrix to form a carbon coating, thereby effectively enhancing the mechanical strength of the inorganic fiber aerogel. In addition, compared with the low-density aerogel material prepared by traditional methods, the silicon nitride fiber aerogel matrix of the present application has high-density silicon nitride nanofibers. After being strengthened by CVI, a more significant strengthening effect can be achieved, and the mechanical strength of the inorganic fiber aerogel is higher.

[0082] Optionally, the volatile organic matter includes one or more of methane, ethane, propane, ethylene, acetylene and propylene, and may further be methane.

[0083] Optionally, the atmosphere containing volatile organic compounds further contains a carrier gas, and the carrier gas includes one or more of helium, neon, argon and xenon, and may further be argon.

[0084] The flow ratio of volatile organic compounds to carrier gas is 1:(0.5-5.0), such as 1:0.5, 1:1, 1:1.5, 1:2, 1:2.5, 1:3, 1:3.5, 1:4, 1:4.5 or 1:5. The flow rate of volatile organic compounds is 0.001 mL / min-1 mL / min, and the flow rate of carrier gas is 0.1 mL / min-1000 mL / min.

[0085] Optionally, the conditions for the chemical vapor impregnation treatment include: (1) the pressure is 100Pa~10000Pa, for example, 100Pa, 200Pa, 500Pa, 1000Pa, 5000Pa or 8000Pa, and can be further selected as 1000Pa; (2) the temperature is 600℃~1300℃, for example, 600℃, 650℃, 700℃, 750℃, 800℃, 850℃, 900℃, 950℃, 1200℃ or 1300℃; (3) the time is 0.5h~12h, for example, 0.5h, 1h, 1.5h, 2h, 2.5h, 3h, 5h or 10h.

[0086] Optionally, the thickness of the carbon coating is 100 nm to 1000 nm, for example, 100 nm, 200 nm, 300 nm, 400 nm, 500 nm, 600 nm, 700 nm, 800 nm, 900 nm or 1000 nm, and further optionally 407 nm to 672 nm.

[0087] S400: forming a heating layer on the inorganic fiber aerogel to prepare an aerogel atomization core.

[0088] Optionally, the method of forming the heating layer on the inorganic fiber aerogel includes printing a resistor paste, sputtering a resistor layer, or laminating a heating mesh.

[0089] In a second aspect of the present application, an aerogel atomization core is provided, which is prepared by the method for preparing an aerogel atomization core as described above.

[0090] Optionally, the porosity of the aerogel atomization core is 50% to 98%, for example, 50%, 55%, 60%, 65%, 70%, 75%, 80%, 85%, 90%, 95% or 98%, and further optionally 78.9% to 85.9%.

[0091] Optionally, the pore size of the aerogel atomization core is 5 μm to 50 μm, such as 5 μm, 10 μm, 15 μm, 20 μm, 25 μm, 30 μm, 35 μm, 40 μm, 45 μm or 50 μm, and can further be 6 μm to 23 μm.

[0092] Optionally, the volume density of the aerogel atomization core is 5 mg / cm 3 ~5000mg / cm 3 , for example 5mg / cm 3 、50mg / cm 3 、100mg / cm 3 、200mg / cm 3 , 500mg / cm 3 、1000mg / cm 3 、2000mg / cm3 、3000mg / cm 3 、4000mg / cm 3 or 5000mg / cm 3 , further optional to 390mg / cm 3 ~710mg / cm 3 .

[0093] Optionally, the compressive strength of the aerogel atomization core is 0.1 MPa to 100 MPa, for example, 0.1 MPa, 1 MPa, 5 MPa, 10 MPa, 20 MPa, 30 MPa, 40 MPa, 50 MPa, 60 MPa, 70 MPa, 80 MPa, 90 MPa or 100 MPa, and can further be 4 MPa to 6 MPa.

[0094] The aerogel atomization core provided in the present application has the characteristics of high porosity, large pore size and uniform pore size distribution. Its porosity is adjustable in the range of 50% to 98%, and its pore size is adjustable in the range of 5μm to 50μm. It has high mechanical strength and can show excellent oil conduction performance, atomization performance and safety performance, thereby effectively improving the user experience. In addition, the aerogel atomization core can also be made into blocks, films, fibers or other preset shapes to meet different application requirements. In general, the aerogel atomization core of the present application has the advantages of excellent product performance, simple preparation process, low cost, strong environmental protection and diversified product shapes.

[0095] In a third aspect of the present application, an electronic cigarette is provided, comprising the aerogel atomization core as described above.

[0096] The following is further described in conjunction with specific embodiments and comparative examples. The raw materials involved in the following specific embodiments and comparative examples, unless otherwise specified, can all be commercially available, the instruments used, unless otherwise specified, can all be commercially available, and the processes involved, unless otherwise specified, are all routinely selected by those skilled in the art.

[0097] Example 1

[0098] The preparation method of the aerogel atomization core of this embodiment is as follows:

[0099] (1) Preparation of green body: Under the conditions of argon protection, pressure of 1 atm, and temperature of 25°C, a silicon source, a carbon source, a thickener, and deionized water were mixed at a mixing speed of 500 rpm for 30 min to obtain a slurry; the slurry was subjected to pressure molding treatment at room temperature to obtain a green body with a solid content of 76%.

[0100] Among them, the silicon source is silicon powder with a purity of 99.9% and a particle size of 100 mesh;

[0101] The carbon source is carbon powder with a purity of 99.9% and a particle size of 200 meshes;

[0102] The thickener is cellulose with a purity of 99.9% and a particle size of 200 mesh;

[0103] The resistivity of deionized water is 18.2 MΩ·cm;

[0104] The mass ratio of the silicon source, the carbon source, the thickener and the deionized water is 1:5:2:2.5, and the molar ratio of the carbon element to the silicon element is 1:5.

[0105] (2) Primary sintering treatment: The green body is placed in a high-temperature furnace and nitrogen is introduced for protection. The temperature is raised to 1500°C at a heating rate of 5°C / min and kept at this temperature for 2 h. The silicon source, carbon source and thickener in the green body undergo carbon thermal reduction reaction and Si3N4 nanofibers are grown in situ. The intermediate is obtained after cooling in the furnace.

[0106] (3) Secondary sintering treatment: The intermediate is placed in a muffle furnace and heated to 800 °C at a heating rate of 5 °C / min in an air atmosphere. The temperature is kept at this temperature for 2 h to remove the unreacted carbon source and other raw materials remaining in the intermediate. After cooling in the furnace, a silicon nitride fiber aerogel matrix is ​​obtained.

[0107] (4) Chemical vapor impregnation treatment: The silicon nitride fiber aerogel substrate is placed in a chemical vapor impregnation furnace, with methane as the precursor and a methane flow rate of 0.01 mL / min, and argon as the carrier gas and an argon flow rate of 10 mL / min. Chemical vapor impregnation is carried out for 2 hours at a temperature of 800 °C and a pressure of 1 atm to form a carbon coating on the surface and inside of the silicon nitride fiber aerogel substrate. After cooling in the furnace, the substrate is taken out to obtain an inorganic fiber aerogel.

[0108] (5) Preparation of aerogel atomizer core: Cut the inorganic aerogel fiber into a rectangular shape with a length of 9 mm, a width of 4 mm, and a thickness of 2 mm, and then print the heating circuit on the surface of the rectangular shape or attach the heating electrode to obtain the aerogel atomizer core.

[0109] Example 2

[0110] The difference between this embodiment and embodiment 1 is that the carbon source is graphite powder with a purity of 99.9% and a particle size of 200 meshes.

[0111] Example 3

[0112] The difference between this embodiment and embodiment 1 is that the silicon source is silicon carbide powder with a purity of 99.9% and a particle size of 100 mesh.

[0113] Example 4

[0114] The difference between this embodiment and embodiment 1 is that starch is used as the thickener with a purity of 99.9% and a particle size of 200 meshes.

[0115] Example 5

[0116] The difference between this embodiment and embodiment 1 is that the mass ratio of the silicon source, the carbon source, the thickener and the deionized water is 1:3:1:0.5, and the molar ratio of the carbon element to the silicon element is 1:3.

[0117] Example 6

[0118] The difference between this embodiment and embodiment 1 is that the temperature of the primary sintering treatment in step (2) is 1700° C. and the temperature is maintained for 0.5 h.

[0119] Example 7

[0120] The difference between this embodiment and embodiment 1 is that the temperature of the primary sintering treatment in step (2) is 1400° C. and the temperature is kept for 20 hours.

[0121] Example 8

[0122] The difference between this embodiment and embodiment 1 is that the temperature of the chemical vapor impregnation treatment in step (4) is 1000° C. and the temperature is maintained for 0.5 h.

[0123] Comparative Example 1

[0124] The present comparative example adopts the traditional method to prepare the aerogel matrix, and the specific steps are as follows: ethyl orthosilicate is mixed with anhydrous ethanol and water in a certain proportion, stirred evenly, hydrolyzed with acid, and then alkali is added to obtain silica gel, which is then supercritically dried to obtain the silica aerogel matrix.

[0125] After the silica aerogel substrate is prepared, chemical vapor impregnation treatment is performed according to step (4) of Example 1 and a heating layer is prepared according to step (5) to obtain an aerogel atomization core.

[0126] Comparative Example 2

[0127] The preparation method of the aerogel atomization core of this comparative example is as follows:

[0128] (1) Preparation of slurry: The slurry was prepared according to step (1) of Example 1 without performing a forming process.

[0129] (2) Sintering treatment: performing a primary sintering treatment according to step (2) of Example 1, and performing a secondary sintering treatment according to step (3) of Example 1 to obtain silicon nitride fiber powder;

[0130] (3) Molding process: Pour the silicon nitride fiber powder into a mold and use a press to press at room temperature to obtain a silicon nitride fiber aerogel matrix.

[0131] (4) Chemical vapor impregnation treatment: the same as step (4) of Example 1.

[0132] (5) Preparation of aerogel atomization core: the same as step (5) of Example 1.

[0133] Comparative Example 3

[0134] The difference between this comparative example and Example 1 is that the chemical vapor impregnation treatment in step (4) is not performed.

[0135] Comparative Example 4

[0136] The difference between this comparative example and Example 1 is that no thickener is added in step (1).

[0137] Test Case

[0138] The aerogel atomization cores prepared in each embodiment and each comparative example were tested as follows:

[0139] (1) Morphological characterization: The microscopic morphology of the silicon nitride fiber aerogel matrix and the aerogel atomizer core was observed using a scanning electron microscope (SEM), and the length and diameter of the silicon nitride nanofibers in the silicon nitride fiber aerogel matrix and the length and diameter of the silicon nitride nanofibers in the aerogel atomizer core were recorded. The thickness of the carbon coating was calculated. The results are shown in Tables 1 and Figure 2 .

[0140] (2) Bulk density and porosity: The bulk density and porosity of the aerogel atomizer core were measured using a density and porosity tester, and the results are shown in Table 2. The porosity test method refers to the national standard JIS R1634-1998, and the porosity of the aerogel atomizer core is measured according to the Archimedes drainage method.

[0141] (3) Pore diameter: Using a pore diameter tester, the aerogel atomizer core is first evacuated and then placed in a tooling. Argon gas is passed through the core and the pore diameter of the aerogel atomizer core is calculated by the system by monitoring the gas pressure and the amount of gas passing through the sample. The results are shown in Table 2.

[0142] (4) Mechanical strength: Referring to the national standard GB / T 1041-2008, the compressive stress-strain curve of the aerogel atomizer core was measured using a mechanical testing machine, and the compressive strength of the aerogel atomizer core was calculated. The results are shown in Table 2.

[0143] (5) Liquid conduction performance: An internal standard test was performed using cigarette oil. A mixed solvent of propylene glycol (PG) and glycerol (VG) was placed in a container at a volume ratio of 1:1. A sponge was placed in the container with the height of the sponge higher than the liquid level. The porous substrate was placed parallel to the sponge and timing was started until the cigarette oil rose from the bottom surface of the sample to the upper plane of the sample through capillary action. The time taken for the cigarette oil to reach the upper plane from the bottom surface of the sample was tested. Three samples were used for each embodiment formula and the average value was calculated.

[0144] (6) Atomization performance: The total particulate matter (TPM) generated by the aerogel atomizer core during the atomization process was measured using an oil conduction test device and an absorption resistance meter. The results are shown in Table 2. The higher the TPM value, the better the atomization performance of the aerogel atomizer core.

[0145] Depend on Figure 2 As shown in Table 1, compared with Comparative Examples 1 to 4, in the aerogel atomizer cores prepared in Examples 1 to 8, the silicon nitride nanofibers before and after CVI treatment have a larger diameter, and the thickness of the obtained carbon coating is also significantly higher, which is beneficial to improving the mechanical strength and safety of the aerogel atomizer core.

[0146] It can be seen from Table 2 that, compared with Comparative Examples 1 to 4, the aerogel atomization cores prepared in Examples 1 to 8 have higher porosity, larger pore size, higher volume density and higher compression strength, and exhibit excellent oil conduction performance and atomization performance.

[0147] Table 1. Silicon nitride nanofibers in aerogel atomizer core

[0148]

[0149] Table 2. Performance of aerogel atomizer core

[0150]

[0151] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0152] The above-described embodiments only express several implementation methods of the present application, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of protection of the present application. It should be pointed out that, for a person of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present application, and these all belong to the scope of protection of the present application. Therefore, the scope of protection of the present application shall be subject to the attached claims.

Claims

1. A method for preparing an aerogel atomization core, characterized in that: The following steps are involved: Performing molding treatment on the slurry containing the silicon source, the carbon source and the thickener to prepare a green body; Sintering the green body to prepare a silicon nitride fiber aerogel matrix; Forming a carbon coating on the surface and inside of the silicon nitride fiber aerogel matrix by chemical vapor impregnation to prepare an inorganic fiber aerogel; A heating layer is formed on the inorganic fiber aerogel to prepare an aerogel atomization core.

2. The method for preparing the aerogel atomization core according to claim 1, characterized in that: The green compact is sintered, comprising the following steps: In a nitrogen atmosphere, the green body is subjected to a sintering treatment to cause a carbothermal reduction reaction between the silicon source and the carbon source and to generate silicon nitride nanofibers in situ, thereby preparing an intermediate; The intermediate is subjected to secondary sintering treatment in an air atmosphere to prepare the silicon nitride fiber aerogel matrix.

3. The method for preparing the aerogel atomization core according to claim 2, characterized in that: The sintering temperature of the primary sintering treatment is 1400° C. to 1700° C., and the heat preservation time is 0.5 h to 24 h.

4. The method for preparing the aerogel atomization core according to claim 2, characterized in that: The sintering temperature of the secondary sintering treatment is 600° C. to 1100° C., and the heat preservation time is 0.1 h to 6 h.

5. The method for preparing the aerogel atomization core according to any one of claims 1 to 4, characterized in that: One or more of the following conditions are met: (1) The silicon source includes one or more of silicon powder, silicon carbide powder, silicon nitride powder, silicon dioxide powder, molybdenum disilicide powder and silica sol; (2) The carbon source includes one or more of carbon powder, graphite powder and carbon fiber; (3) The thickener includes one or more of sol, cellulose, cellulose derivatives, starch and polymethyl methacrylate; (4) The molar ratio of silicon to carbon in the slurry is 1:(1-10); (5) The molding process includes one or more of room temperature pressure molding process, hot die casting molding process and injection molding process.

6. The method for preparing the aerogel atomization core according to any one of claims 1 to 4, characterized in that: The chemical vapor impregnation method comprises the following steps: In an atmosphere containing volatile organic matter, the silicon nitride fiber aerogel matrix is ​​subjected to a chemical vapor impregnation treatment to form a carbon coating on the surface and inside of the silicon nitride fiber aerogel matrix.

7. The method for preparing the aerogel atomization core according to claim 6, characterized in that: One or more of the following conditions are met: (1) The volatile organic compounds include one or more of methane, ethane, propane, ethylene, acetylene and propylene; (2) The atmosphere containing volatile organic compounds further contains a carrier gas, and the flow ratio of the volatile organic compounds to the carrier gas is 1:(0.5-5.0); (3) The conditions of the chemical vapor impregnation treatment include: pressure of 100Pa~10000Pa, temperature of 600℃~1300℃, and time of 0.5h~12h; (4) The thickness of the carbon coating is 1 nm to 500 nm.

8. An aerogel atomization core, characterized in that: The aerogel atomization core is prepared by the preparation method of the aerogel atomization core according to any one of claims 1 to 7.

9. The aerogel atomization core according to claim 8, characterized in that: One or more of the following conditions are met: (1) The porosity of the aerogel atomization core is 50% to 98%; (2) The pore size of the aerogel atomization core is 5 μm to 50 μm; (3) The volume density of the aerogel atomization core is 5 mg / cm 3 ~5000mg / cm 3 .

10. An electronic cigarette, characterized in that: Comprising the aerogel atomization core as described in claim 8 or 9.

Citation Information

Patent Citations

  • Silicon nitride nanoribbon aerogel and preparation method thereof

    CN109704781A

  • 3D printing silicon nitride fiber aerogel and preparation method and application thereof

    CN113754446A

  • High-temperature-resistant light-weight high-strength porous ceramic and preparation method thereof

    CN114276163A

  • High-temperature-resistant composite component aerogel material and preparation method thereof

    CN115246745A

  • Atomizing core, atomizer, aerosol generating device and atomizing core preparation method

    CN116807067A

Cited By

  • Aerogel atomization core, preparation method therefor and electronic cigarette

    WO2026046287A1