Isopyrazine compound, preparation method and application of isopyrazine compound in preparation of flexible binder-free zinc ion battery positive electrode material

By combining isofluoroazine compounds with MXene, a binder-free flexible zinc-ion battery cathode material was prepared, solving the problems of insufficient conductivity and flexibility. This resulted in a high-performance and safe zinc-ion battery cathode material suitable for flexible energy storage devices.

CN118994174AActive Publication Date: 2024-11-22XIAMEN UNIV

Patent Information

Application Number
CN202411076076.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-07
Publication Date
2024-11-22
Estimated Expiration
2044-08-07

AI Technical Summary

Technical Problem

In existing flexible energy storage devices, the flammability and toxicity of organic electrolytes pose safety hazards, and the conductivity and flexibility of traditional aqueous zinc-ion battery cathode materials are insufficient, making it difficult to meet the requirements of high performance and safety.

Method used

A binder-free flexible zinc-ion battery cathode material was prepared by combining isofluoroazine compounds with MXene. The pseudocapacitive properties of MXene and the isofluoroazine framework structure were used to improve conductivity and flexibility, and PVA hydrogel electrolyte was used to improve stress-strain capacity during cycling.

Benefits of technology

A high-performance, low-cost, and environmentally friendly flexible zinc-ion battery cathode material has been developed, exhibiting excellent electrochemical performance and cycle stability. It can stably cycle for over 30,000 cycles at high current density while maintaining a coulombic efficiency of 100%.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118994174A_ABST
    Figure CN118994174A_ABST
Patent Text Reader

Abstract

The invention discloses an isoxazine compound, a preparation method and application of the isoxazine compound in preparation of a flexible binder-free zinc ion battery positive electrode material, a binder-free organic positive electrode material BMBF is prepared by compounding MXene (Ti3C2Tx) and small molecules with an isoxazine skeleton structure, and the problems of poor intrinsic conductivity and high solubility of organic molecules are solved. And meanwhile, extra capacity is provided by utilizing the pseudocapacitance characteristic of MXene. The used small organic molecules are synthesized in one step by using the alloxan monohydrate through a simple Schiff base reaction, so that the cost is reduced, and the preparation process is simplified. The prepared aqueous zinc ion battery shows excellent electrochemical performance, including relatively high specific capacity, excellent cycling stability and rate capability. The button cell can stably circulate more than 30,000 circles under the current density of 3Ag <-1 >, and the coulombic efficiency of about 100% is always maintained.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to an isoalloxazine compound, a preparation method and application thereof in preparing a positive electrode material of a flexible binder-free zinc ion battery, belonging to the technical field of flexible zinc ion battery preparation. Background Art

[0002] In recent years, the rapid development of science and technology has significantly promoted the advancement of flexible energy storage technology and injected new vitality into the innovation of portable and wearable devices. With the rapid growth of market demand for portable devices, a variety of products such as small and exquisite smart watches, medical testing equipment that fits closely to the skin, skin sensors, and foldable smartphones have emerged. The performance of these flexible electronic devices depends greatly on their energy storage components, and the size and mechanical properties of the energy storage devices largely determine the applicability of wearable devices in various usage scenarios. Therefore, the development of flexible energy storage devices that are both safe and efficient is crucial to the future development of wearable electronic products. However, most commercial batteries on the market currently use components containing organic electrolytes and alkali metals. The flammability of these materials and the toxicity of organic electrolytes often cause safety hazards such as environmental pollution and fire. Considering these serious safety issues, aqueous zinc-ion batteries (AZIBs) using aqueous electrolytes with high safety factors have gradually become a new star in the field of flexible energy storage and are regarded as highly promising candidates for flexible energy storage devices.

[0003] Among the existing organic electrode materials, organic carbonyl and imine compounds have attracted more and more attention as high-performance cathode materials in AZIBs. Carbonyl and imine organic cathodes (such as quinones and pyrazines) have been widely studied because they are rich in highly active sites for redox reactions. Their zinc storage mechanism is mainly through the reversible ionization of C=O or C=N bonds, which serve as effective active sites for zinc ion insertion / deinsertion. In theory, quinone molecules with lower molecular weight and rich active groups can obtain higher theoretical capacity.

[0004] In recent years, inspired by the biological energy metabolism in organisms, people have studied the parts of organisms that perform redox behavior. These bio-inspired redox-active parts are able to undergo reversible redox reactions during charge and discharge. They can be overproduced by microorganisms or extracted from renewable biomass, for example, humification of plant and animal matter. These renewable biomolecule-based electrochemical energy storage materials are not only environmentally friendly, biocompatible and sustainable, minimizing chemical waste and safety hazards, but also have good electrochemical performance, structural flexibility and chemical diversity. For example, the isoalloxazine structure in flavin, the nitrogen heterocycle in phenazines and viologens have been shown to reversibly store zinc ions through a dual ion transfer process.

[0005] In order to balance the flexibility and high performance of aqueous zinc-ion battery cathodes, it is imperative to prepare high-performance flexible zinc-ion battery cathode materials and develop substrate materials that meet both requirements. By taking advantage of the substrate of MXene, a flexible binder-free hybrid nano cathode was constructed, using polyvinyl alcohol (PVA) hydrogel electrolyte and applied to AZIBs. The conductivity of the organic cathode and the stress-strain capacity during the cycle were improved. Summary of the invention

[0006] The purpose of the present invention is to overcome the deficiencies of the above-mentioned prior art and provide an isoalloxazine compound, a preparation method and an application thereof in the preparation of a flexible binder-free zinc ion battery positive electrode material.

[0007] To achieve the above object, the present invention adopts the following technical solutions:

[0008] 1. An isoalloxazine compound, selected from any one of pyrimido[5,4-g]pteridine-2,4,6,8(1H,3H,7H,9H)-tetraketone (PPT), naphtho[2,3-g]pteridine-2,4,6,11(1H,3H)-tetraketone (NPT), and benzo[1,2-g:5,4-g']dipteridine-2,4,6,8,10,13(1H,3H,9H,11H)-hexanone (BDH), and their chemical structural formulas are as follows:

[0009]

[0010] 2. A method for preparing the aforementioned isoalloxan compound: first add alloxan monohydrate and reactant 2 to a reaction vessel, then add glacial acetic acid and mix well, then slowly drip a boric acid acetic acid solution into the reaction vessel, heat and stir to react, and post-treat to obtain the isoalloxan compound; wherein reactant 2 is 5,6-amino-2,4(1H,3H)-pyrimidinedione, 2,3-diaminonaphthalene-1,4-dione or 2,3,5,6-tetrakis(amino)benzoquinone, and the corresponding isoalloxan compounds are the aforementioned PPT, NPT, and BDH, respectively.

[0011] The reaction formula is as follows:

[0012]

[0013] Preferably, when compound 2 is 5,6-amino-2,4(1H,3H)-pyrimidinedione or 2,3-diaminonaphthalene-1,4-dione, the molar ratio of alloxan monohydrate to compound 2 is 1:1 to 3, and more preferably 1:1 to 1.5; when compound 2 is 2,3,5,6-tetrakis(amino)benzoquinone, the molar ratio of alloxan monohydrate to compound 2 is 2 to 4:1, and more preferably 2 to 3:1.

[0014] Further preferably, the molar ratio of alloxan monohydrate to the boric acid contained in the boric acid acetic acid solution is 1:1, and the dosage ratio of alloxan monohydrate to glacial acetic acid is 1 mmol:15 mL, wherein the boric acid acetic acid solution is obtained by dissolving boric acid in glacial acetic acid with a molar ratio of 10 times that of boric acid.

[0015] More preferably, the process conditions for the heating and stirring reaction are: stirring rate 500 rpm, temperature 60° C., stirring time 4 to 7 h; the stirring time is more preferably 4 to 6 h.

[0016] Further preferably, the post-treatment includes: naturally cooling to room temperature, vacuum filtering to obtain a precipitate, washing with deionized water and ethanol for 2 to 3 times in sequence, and then drying in a vacuum drying oven for 12 hours.

[0017] 3. Application of the aforementioned isoalloxazine compounds in the preparation of flexible binder-free zinc ion battery positive electrode materials.

[0018] 4. A flexible binder-free zinc-ion battery positive electrode material (BM), prepared by using the aforementioned isoalloxazine compound as an active material and MXene as a flexible substrate.

[0019] Preferably, MXene is prepared by the following method: first, lithium fluoride is slowly added to concentrated hydrochloric acid, mixed at room temperature, Ti3AlC2 powder is carefully added, heated and stirred for reaction, and then post-treated to obtain the MXene.

[0020] Further preferably, the dosage ratio of concentrated hydrochloric acid, lithium fluoride and Ti3AlC2 powder is 60mL:2g:2g, the concentration of concentrated hydrochloric acid is 9mol / L; and the mixing time at room temperature is 20min.

[0021] Further preferably, the process conditions of the heating and stirring reaction are: stirring rate 500 rpm, temperature 40° C., and stirring time 24 h.

[0022] Further preferably, the post-treatment comprises: repeated centrifugation and deionized water washing until the pH value of the solution exceeds 6; in order to x ) flakes were separated, dissolved and dispersed in deionized water, and ultrasonically treated for 1 h under nitrogen protection to minimize oxidation, thereby obtaining Ti3C2T x solution; finally, Ti3C2T x The solution was centrifuged at 4000 rpm for 1 h to obtain a single-layer or few-layer MXene suspension; wherein the dosage ratio of MXene to deionized water was: 1 g: 50 mL.

[0023] More preferably, the positive electrode material is prepared by the following method: first, the isoalloxazine compound is added to anhydrous ethanol, subjected to ultrasonic treatment, and then the aforementioned MXene suspension is added, ultrasonic treatment is performed in an ice bath environment, the ethanol is removed by rotary evaporation, and vacuum drying is performed.

[0024] More preferably, the mass ratio of the isoalloxazine compound to the MXene suspension is 1:0.5-3, and more preferably 1:2-3, wherein the concentration of the ethanol solution of the isoalloxazine compound is 1 mg mL -1

[0025] More preferably, the ultrasonic time after adding the isoalloxazine compound to anhydrous ethanol is 0.5 h, and the ice bath ultrasonic time after adding the MXene suspension is 1 h.

[0026] More preferably, the process conditions for removing ethanol by rotary evaporation are: the speed of the rotary evaporator is set to 100 rpm and the temperature is 40°C.

[0027] More preferably, the vacuum drying temperature is 40° C. and the drying time is 6 h.

[0028] 5. Application of the aforementioned positive electrode materials in the preparation of flexible zinc-ion batteries.

[0029] Preferably, the zinc ion battery is obtained by assembling and packaging a carbon cloth positive electrode containing the aforementioned positive electrode material, a zinc-deposited carbon cloth, and a PVA hydrogel electrolyte in a sandwich structure.

[0030] Further preferably, the carbon cloth positive electrode is prepared by the following method: first, carbon black is evenly dispersed in N-methylpyrrolidone (NMP), then the aforementioned positive electrode material is added, and stirred and mixed under sealed conditions to obtain a slurry of suitable viscosity, and then the pretreated carbon cloth is fully immersed in the slurry, taken out and vacuum dried to obtain the obtained product.

[0031] More preferably, the usage ratio of carbon black, positive electrode material and NMP is 30 mg:120 mg:0.6 mL.

[0032] More preferably, the mixture is stirred at 800 rpm at room temperature for more than 24 hours under sealed conditions.

[0033] More preferably, a suitable criterion for judging the thick state is that when the container containing the slurry is turned upside down, the slurry slowly slides down along the wall.

[0034] More preferably, the pretreated carbon cloth is prepared by ultrasonically cleaning the carbon cloth with deionized water and anhydrous ethanol in sequence for 30 minutes, and then taking it out and vacuum drying it at 60° C. for 6 hours.

[0035] More preferably, the soaking time is 1 hour; after taking out, the mixture is vacuum dried at 80° C. for 12 hours.

[0036] Further preferably, the zinc-deposited carbon cloth is prepared by the following method: firstly dissolving zinc sulfate, sodium sulfate and boric acid in distilled water to prepare an electrolyte, and then using the chronopotentiometry to electro-deposit the pretreated carbon cloth using the electrolyte.

[0037] More preferably, the usage ratio of zinc sulfate, sodium sulfate, boric acid and distilled water is 20g:20g:4g:200mL.

[0038] More preferably, the pretreated carbon cloth is prepared by ultrasonically cleaning the carbon cloth with deionized water and anhydrous ethanol in sequence for 30 minutes, and then taking it out and vacuum drying it at 60° C. for 6 hours.

[0039] More preferably, at -15 mA cm -2 The electrodeposition was carried out at a constant current density of 30 min.

[0040] Further preferably, the PVA hydrogel electrolyte is prepared by the following method: firstly, polyvinyl alcohol (PVA) is mixed with anhydrous ethanol and deionized water, heated and stirred for the first time, then an aqueous zinc sulfate solution is slowly dripped into it, heated and stirred for the second time, and naturally cooled to room temperature to obtain the obtained product.

[0041] More preferably, the ratio of zinc sulfate contained in PVA, anhydrous ethanol, deionized water, and zinc sulfate aqueous solution is 1 g: 10 mL: 3 mL: 3.229 g; the zinc sulfate aqueous solution is obtained by dissolving 3.229 g zinc sulfate in 5 mL deionized water.

[0042] More preferably, the process conditions for the first heating and stirring are: stirring at 65°C and 500 rpm for 15 min; and the process conditions for the second heating and stirring are: stirring at 85°C and 500 rpm for 10 min.

[0043] Beneficial effects of the present invention:

[0044] The present invention uses MXene as a flexible two-dimensional substrate and composites it with a small molecule having an isoalloxazine skeleton structure to prepare a binder-free organic positive electrode material, thereby solving the problems of poor conductivity and high solubility of organic molecules, and making it have good flexibility, which can be applied to the preparation of flexible devices, while using the pseudocapacitive properties of MXene to provide additional capacity. In addition, the positive electrode material has simple preparation steps and low overall preparation cost, which can achieve large-scale preparation of materials. The application of a flexible organic positive electrode material of the present invention was tested in a button cell and showed excellent electrochemical properties, including high specific capacity, excellent cycle stability and rate performance. It can be used in 3Ag -1The research also revealed that the H + With Zn 2+ The double ion co-embedded, and H + This work not only optimizes organic electrode materials from the perspectives of molecular structure and surface engineering, but also provides new ideas for the development of low-cost, high-performance, and environmentally friendly rechargeable batteries. BRIEF DESCRIPTION OF THE DRAWINGS

[0045] Figure 1 A schematic flow chart of a method for preparing a battery positive electrode material of a MXene composite organic molecule prepared in the present invention.

[0046] Figure 2 This is a scanning electron microscope (SEM) image of the positive electrode material prepared in Example 7 of the present invention.

[0047] Figure 3 (a) SEM image of the positive electrode material prepared in Example 7 of the present invention, and the corresponding (b) Ti, (c) O, (d) C, (e) N and (f) F element distribution spectrum (EDS).

[0048] Figure 4 The flexible positive electrode material of the present invention is assembled into an assembly diagram of a flexible zinc ion battery.

[0049] Figure 5 The positive electrode material prepared in Example 8 of the present invention was assembled into a button-type zinc ion battery. -1 Cycling performance at different current densities.

[0050] Figure 6 The positive electrode material prepared in Example 12 of the present invention is assembled into a button-type zinc ion battery. -1 Cycling performance at different current densities.

[0051] Figure 7 The positive electrode material of the present invention is assembled into a button-type ion battery at 3Ag -1 Long cycle performance at different current densities.

[0052] Figure 8 A flexible zinc ion battery assembled from the positive electrode material of the present invention is shown in a diagram which stably supplies power to an LED device with a voltage of 3.0 V when bent. DETAILED DESCRIPTION

[0053] The present invention is further described below in conjunction with the accompanying drawings and embodiments. It should be noted that the following description is only for explaining the present invention and does not limit its contents.

[0054] Embodiment 1:

[0055] Synthesis of pyrimido[5,4-g]pteridine-2,4,6,8(1H,3H,7H,9H)-tetraone:

[0056]

[0057] Alloxan monohydrate (2.0mmol, 320.18mg) and 5,6-amino-2,4(1H,3H)-pyrimidinedione (2mmol, 284.30mg) were added to a 100mL reaction tube, glacial acetic acid (30mL) was added to dissolve the reactants, and then boric acid (2.0mmol, 123.60mg) was dissolved in an appropriate amount of glacial acetic acid and slowly dripped into the reaction tube, the reaction temperature was raised to 60°C, and stirred at 500rpm for 6h. After the temperature was cooled to room temperature, the precipitate was obtained by vacuum filtration, washed with deionized water and ethanol 2 to 3 times in sequence, and then placed in a vacuum drying oven for 12h to obtain a red product PPT (297.80mg, 60% yield). 1 H NMR(500MHz,DMSO-d6)δ12.19(s,1H),11.73(s,1H).MALDI-TOF(m / z):[M] + calculated for C8H4N6O4:248.0186; found,248.0183.

[0058] Embodiment 2:

[0059] Alloxan monohydrate (2.0mmol, 320.18mg) and 5,6-amino-2,4(1H,3H)-pyrimidinedione (3mmol, 426.45mg) were added to a 100mL reaction tube, glacial acetic acid (30mL) was added to dissolve the reactants, and then boric acid (2.0mmol, 123.60mg) was dissolved in an appropriate amount of glacial acetic acid and slowly dripped into the reaction tube, the reaction temperature was raised to 60°C, and stirred at 500rpm for 6h. After the temperature was cooled to room temperature, the precipitate was obtained by vacuum filtration, washed with deionized water and ethanol 2 to 3 times in sequence, and then placed in a vacuum drying oven for 12h to obtain a red product PPT (322.62mg, 65% yield).

[0060] Embodiment 3:

[0061] Synthesis of naphtho[2,3-g]pteridine-2,4,6,11(1H,3H)-tetraone:

[0062]

[0063] Alloxan monohydrate (2.0mmol, 320.18mg) and 2,3-diaminonaphthalene-1,4-dione (2.0mmol, 376.36mg) were added to a 100mL reaction tube, glacial acetic acid (30mL) was added to dissolve the reactants, and then boric acid (2.0mmol, 123.60mg) was dissolved in an appropriate amount of glacial acetic acid and slowly dripped into the reaction tube, the reaction temperature was raised to 60°C, and stirred at 500rpm for 6h. After the temperature was cooled to room temperature, the precipitate was obtained by vacuum filtration, washed with deionized water and ethanol 2 to 3 times in sequence, and then placed in a vacuum drying oven for 12h to obtain a green product NPT (494.31mg, 84% yield). 1 H NMR(500MHz,DMSO-d6)δ11.84(s,1H),11.16(s,1H),7.43(dd,J=17.9,6.6Hz,2H),7.24-7.01(m,2H).MALDI-TOF(m / z):[M] + calculated for C 14 H6N4O4:294.0281; found,294.0285.

[0064] Embodiment 4:

[0065] Alloxan monohydrate (2.0mmol, 320.18mg) and 2,3-diaminonaphthalene-1,4-dione (3.0mmol, 564.54mg) were added to a 100mL reaction tube, glacial acetic acid (30mL) was added to dissolve the reactants, and then boric acid (2.0mmol, 123.60mg) was dissolved in an appropriate amount of glacial acetic acid and slowly dripped into the reaction tube, the reaction temperature was raised to 60°C, and stirred at 500rpm for 6h. After the temperature was cooled to room temperature, the precipitate was obtained by vacuum filtration, washed with deionized water and ethanol 2 to 3 times in sequence, and then placed in a vacuum drying oven for 12h to obtain a green product NPT (506.08mg, 86% yield).

[0066] Embodiment 5:

[0067] Synthesis of benzo[1,2-g:5,4-g']dipterygium-2,4,6,8,10,13(1H,3H,9H,11H)-hexanone:

[0068]

[0069] Alloxan monohydrate (2.0mmol, 320.18mg) and 2,3,5,6-tetra(amino)-benzoquinone (1.0mmol, 168.15mg) were added to a 100mL reaction tube, glacial acetic acid (30mL) was added to dissolve the reactants, and then boric acid (2.0mmol, 123.60mg) was dissolved in an appropriate amount of glacial acetic acid and slowly dripped into the reaction tube, the reaction temperature was raised to 60°C, and stirred at 500rpm for 6h. After the temperature was cooled to room temperature, the precipitate was obtained by vacuum filtration, washed with deionized water and ethanol 2 to 3 times in sequence, and then placed in a vacuum drying oven for 12h to obtain a dark green product BDH (456.29mg, 80% yield).

[0070] 1 H NMR (500MHz, DMSO-d6): δ12.68 (s, 1H), 12.02 (s, 1H), MALDI-TOF (m / z): [M] + calculated for C 14 H4N8O6:380.0146; found,380.0152.

[0071] Embodiment 6:

[0072] Alloxan monohydrate (3.0mmol, 480.27mg) and 2,3,5,6-tetra(amino)-benzoquinone (1.0mmol, 168.15mg) were added to a 100mL reaction tube, glacial acetic acid (30mL) was added to dissolve the reactants, and then boric acid (2.0mmol, 123.60mg) was dissolved in an appropriate amount of glacial acetic acid and slowly dripped into the reaction tube, the reaction temperature was raised to 60°C, and stirred at 500rpm for 6h. After the temperature was cooled to room temperature, the precipitate was obtained by vacuum filtration, washed with deionized water and ethanol 2 to 3 times in sequence, and then placed in a vacuum drying oven for 12h to obtain a dark green product BDH (473.40mg, 83% yield).

[0073] Embodiment 7:

[0074] A method for preparing a BDH composite MXene positive electrode material according to an embodiment of the present invention and used for a flexible zinc ion battery positive electrode comprises the following steps:

[0075] First, 80 mg of BDH powder was added to a round-bottom flask, and then ethanol was added to the round-bottom flask to keep the concentration of BDH small molecules below 1 mg mL -1. The BDH dispersion was then ultrasonicated for more than 30 minutes to ensure that the BDH small molecules were evenly dispersed in the ethanol solution. Then 40 mg of MXene suspension was added. The mixture was then ultrasonicated for 1 hour in an ice bath. The ethanol solvent in the mixture was then slowly dried using a rotary evaporator with the speed set to 100 rpm and the temperature set to 40°C. Finally, the obtained sample BM-67 was vacuum dried at 40°C, where BDH:MXene=2:1 (w / w), for subsequent preparation of the positive electrode.

[0076] Add 0.03g of carbon black (CB) to a 5mL glass bottle, add 0.5mL of NMP and stir magnetically until it is evenly dispersed in NMP. Then add 0.12g of BM-67, and then continue to slowly drip 0.1mL of NMP solvent to make the slurry just in a suitable thick state (when the glass bottle is turned upside down, the slurry slowly slides down the wall). After sealing the glass bottle, stir at room temperature at 800rpm for more than 24h to ensure that the components in the slurry are evenly dispersed and mixed. After coating, the prepared slurry is vacuum dried at 80℃ for 12h to completely remove the NMP solvent. The BM-67 positive electrode without PVDF as a binder is named BMBF-67, which can be used in flexible zinc-ion batteries.

[0077] Please refer to Figure 1 , Figure 1 It is a schematic flow chart of the method for preparing the battery positive electrode material of MXene composite organic molecules in Example 7 of the present invention.

[0078] Please refer to Figure 2 , Figure 2 This is a scanning electron microscope (SEM) image of the positive electrode material prepared in Example 7 of the present invention.

[0079] Please refer to Figure 3 , Figure 3 This is the element distribution energy spectrum (EDS) of the positive electrode material prepared in Example 7 of the present invention.

[0080] Embodiment 8:

[0081] A method for preparing a BDH composite MXene positive electrode material according to an embodiment of the present invention and used for a flexible zinc ion battery positive electrode comprises the following steps:

[0082] First, 60 mg of BDH powder was added to a round-bottom flask, and then a certain amount of ethanol was added to the round-bottom flask to keep the concentration of BDH small molecules below 1 mg mL -1. The BDH dispersion was then ultrasonicated for more than 30 minutes to ensure that the BDH small molecules were evenly dispersed in the ethanol solution. Then 60 mg of MXene suspension was added, and the mixture was ultrasonicated for 1 hour in an ice bath. The ethanol solvent in the mixture was then slowly dried using a rotary evaporator with the speed set to 100 rpm and the temperature set to 40°C. Finally, the obtained sample BM-50 was vacuum dried at 40°C, where BDH:MXene=1:1 (w / w), for subsequent preparation of the positive electrode.

[0083] Add 0.03g CB to a 5mL glass bottle, add 0.5mL NMP and stir magnetically until it is evenly dispersed in NMP. Then add 0.12g BM-50, and then continue to slowly drop 0.1mL NMP solvent to make the slurry just in a suitable thick state (when the glass bottle is turned upside down, the slurry slowly slides down the wall). After sealing the glass bottle, stir at room temperature at 800rpm for more than 24h to ensure that the components in the slurry are evenly dispersed and mixed. After coating, the prepared slurry is vacuum dried at 80℃ for 12h to completely remove the NMP solvent. The BM-50 positive electrode without PVDF as a binder is named BMBF-50, which can be used in flexible zinc-ion batteries.

[0084] See also Figure 5 , Figure 5 This is a cycle performance diagram of the positive electrode material prepared in Example 8 of the present invention.

[0085] Embodiment 9:

[0086] A method for preparing a BDH composite MXene positive electrode material according to an embodiment of the present invention and used for a flexible zinc ion battery positive electrode comprises the following steps:

[0087] First, 40 mg of BDH powder was added to a round-bottom flask, and then a certain amount of ethanol was added to the round-bottom flask to keep the concentration of BDH small molecules below 1 mg mL -1 . The BDH dispersion was then ultrasonicated for more than 30 minutes to ensure that the BDH small molecules were evenly dispersed in the ethanol solution. Then 80 mg of MXene suspension was added. The mixture was then ultrasonicated for 1 hour in an ice bath. The ethanol solvent in the mixture was then slowly dried using a rotary evaporator with the speed set to 100 rpm and the temperature set to 40°C. Finally, the obtained sample BM-33 was vacuum dried at 40°C, where BDH:MXene=1:2 (w / w), for subsequent preparation of the positive electrode.

[0088] Add 0.03g CB to a 5mL glass bottle, add 0.5mL NMP and stir magnetically until it is evenly dispersed in NMP. Then add 0.12g BM-33, and then continue to slowly drop 0.1mL NMP solvent to make the slurry just in a suitable thick state (when the glass bottle is turned upside down, the slurry slowly slides down the wall). After sealing the glass bottle, stir at room temperature at 800rpm for more than 24h to ensure that the components in the slurry are evenly dispersed and mixed. After coating, the prepared slurry is vacuum dried at 80℃ for 12h to completely remove the NMP solvent. The BM-33 positive electrode without PVDF as a binder is named BMBF-33, which can be used in flexible zinc-ion batteries.

[0089] Embodiment 10:

[0090] A method for preparing a BDH composite MXene positive electrode material according to an embodiment of the present invention and used for a flexible zinc ion battery positive electrode comprises the following steps:

[0091] First, 30 mg of BDH powder was added to a round-bottom flask, and then a certain amount of ethanol was added to the round-bottom flask to keep the concentration of BDH small molecules below 1 mg mL -1 . The BDH dispersion was then ultrasonicated for more than 30 minutes to ensure that the BDH small molecules were evenly dispersed in the ethanol solution. Then 90 mg of MXene suspension was added. The mixture was then ultrasonicated for 1 hour in an ice bath. The ethanol solvent in the mixture was then slowly dried using a rotary evaporator with the speed set to 100 rpm and the temperature set to 40°C. Finally, the obtained sample BM-25 was vacuum dried at 40°C, where BDH:MXene=1:3 (w / w), for subsequent preparation of the positive electrode.

[0092] Add 0.03g CB to a 5mL glass bottle, add 0.5mL NMP and stir magnetically until it is evenly dispersed in NMP. Then add 0.12g BM-25, and then continue to slowly drop 0.1mL NMP solvent to make the slurry just in a suitable thick state (when the glass bottle is turned upside down, the slurry slowly slides down the wall). After sealing the glass bottle, stir at room temperature at 800rpm for more than 24h to ensure that the components in the slurry are evenly dispersed and mixed. After coating, the prepared slurry is vacuum dried at 80℃ for 12h to completely remove the NMP solvent. The BM-25 positive electrode without PVDF as a binder is named BMBF-25, which can be used in flexible zinc-ion batteries.

[0093] Embodiment 11:

[0094] A method for preparing a BDH composite MXene positive electrode material according to an embodiment of the present invention and used for a flexible zinc ion battery positive electrode comprises the following steps:

[0095] Add 0.03g CB to a 5mL glass bottle, add 0.4mL NMP and stir magnetically until it is evenly dispersed in NMP. Then add 0.07g BM, and then continue to slowly drop 0.1mL NMP solvent to make the slurry just in a suitable thick state (when the glass bottle is turned upside down, the slurry slowly slides down the wall). After sealing the glass bottle, stir at room temperature at 800rpm for more than 24h to ensure that the components in the slurry are evenly dispersed and mixed. After coating, the prepared slurry is vacuum dried at 80℃ for 12h to completely remove the NMP solvent. Among them, BM:CB=7:3(w / w), which can be used in flexible zinc-ion batteries.

[0096] Embodiment 12:

[0097] A method for preparing a BDH composite MXene positive electrode material according to an embodiment of the present invention and used for a flexible zinc ion battery positive electrode comprises the following steps:

[0098] Add 0.03g CB to a 5mL glass bottle, add 0.5mL NMP and stir magnetically until it is evenly dispersed in NMP. Then add 0.12g BM, and then continue to slowly drop 0.1mL NMP solvent to make the slurry just in a suitable thick state (when the glass bottle is turned upside down, the slurry slowly slides down the wall). After sealing the glass bottle, stir at room temperature at 800rpm for more than 24h to ensure that the components in the slurry are evenly dispersed and mixed. After coating, the prepared slurry is vacuum dried at 80℃ for 12h to completely remove the NMP solvent. Among them, BM:CB=8:2(w / w), which can be used in flexible zinc-ion batteries.

[0099] See also Figure 6 , Figure 6 This is a cycle performance diagram of the positive electrode material prepared in Example 12 of the present invention.

[0100] Embodiment 13:

[0101] A method for preparing a BDH composite MXene positive electrode material according to an embodiment of the present invention and used for a flexible zinc ion battery positive electrode comprises the following steps:

[0102] Add 0.02g CB to a 5mL glass bottle, add 0.6mL NMP and stir magnetically until it is evenly dispersed in NMP. Then add 0.18g BM, and then continue to slowly drop 0.1mL NMP solvent to make the slurry just in a suitable thick state (when the glass bottle is turned upside down, the slurry slowly slides down the wall). After sealing the glass bottle, stir at room temperature at 800rpm for more than 24h to ensure that the components in the slurry are evenly dispersed and mixed. After coating, the prepared slurry is vacuum dried at 80℃ for 12h to completely remove the NMP solvent. Among them, BM:CB=9:1(w / w), which can be used in flexible zinc-ion batteries.

[0103] Embodiment 14:

[0104] Button cell assembly: BMBF-25 / 1M ZnSO4+2M Na2SO4 / Zn

[0105] The prepared positive electrode was cut into a 12 mm diameter disc, the 0.1 mm thick zinc foil was cut into a 17 mm diameter disc, and the glass fiber separator was cut into a 19 mm diameter disc. A 304 stainless steel CR2025 battery case was used. The battery was assembled in the following order: positive electrode case-positive electrode-100 μL electrolyte-diaphragm-100 μL electrolyte-negative electrode-wavy spring-gasket-negative electrode case. Finally, the package was performed using a tablet press.

[0106] Embodiment 15:

[0107] Flexible battery assembly: BMBF-25 / PVA hydrogel electrolyte / Zn

[0108] The prepared carbon cloth positive electrode, zinc-deposited carbon cloth and PVA hydrogel electrolyte were cut into suitable shapes, and finally the three components were assembled together in a sandwich structure and packaged with ordinary transparent tape.

[0109] See also Figure 4 , Figure 4 is a schematic diagram of a flexible battery prepared in Example 15 of the present invention, Figure 8 This is a diagram showing the practical application of the flexible battery prepared in Example 15 of the present invention.

[0110] According to the above structure, the performance of the positive electrode as an aqueous zinc ion battery was prepared and characterized. -1 The current density was stable for more than 30,000 cycles, and the Coulomb efficiency was always about 100%. Figure 7 ).

[0111] In order to prove the good versatility of the prepared positive electrode material as a positive electrode of a flexible zinc ion battery, it is further assembled into a flexible zinc ion battery. Satisfactorily, after repeated shearing of the positive electrode, it can still stably supply power to an LED device with a voltage of 3.0V. Therefore, the flexible zinc ion battery positive electrode prepared by the present invention can adapt to various application scenarios of flexible batteries, and shows great application prospects in the field of flexible devices.

[0112] Although the above describes the specific implementation mode of the present invention in conjunction with the accompanying drawings, it is not intended to limit the scope of protection of the present invention. Based on the technical solution of the present invention, various modifications or variations that can be made by those skilled in the art without creative work are still within the scope of protection of the present invention.

Claims

1. An isoalloxazine compound, characterized in that Any one selected from pyrimido[5,4-g]pteridine-2,4,6,8(1H,3H,7H,9H)-tetraone, naphtho[2,3-g]pteridine-2,4,6,11(1H,3H)-tetraone, benzo[1,2-g:5,4-g']dipteridine-2,4,6,8,10,13(1H,3H,9H,11H)-hexanone, and their chemical structural formulas are as follows:

2. The method for preparing the isoalloxazine compound according to claim 1, characterized in that: First, alloxan monohydrate and reactant 2 are added to a reaction container, and then glacial acetic acid is added and mixed evenly, and then the boric acid acetic acid solution is slowly dripped into the reaction container, heated and stirred for reaction, and post-treatment is performed to obtain an isoalloxazine compound; wherein, reactant 2 is 5,6-amino-2,4(1H,3H)-pyrimidinedione, 2,3-diaminonaphthalene-1,4-dione or 2,3,5,6-tetra(amino)benzoquinone, and the corresponding isoalloxazine compounds are PPT, NPT, and BDH, respectively.

3. The preparation method according to claim 2, characterized in that: When compound 2 is 5,6-amino-2,4(1H,3H)-pyrimidinedione or 2,3-diaminonaphthalene-1,4-dione, the molar ratio of alloxan monohydrate to the compound is 1:1 to 3; when compound 2 is 2,3,5,6-tetrakis(amino)benzoquinone, the molar ratio of alloxan monohydrate to the compound is 2 to 4:

1.

4. The preparation method according to claim 2, characterized in that: The molar ratio of alloxan monohydrate to boric acid is 1:1, and the dosage ratio of alloxan monohydrate to glacial acetic acid is 1mmol:15mL, wherein the boric acid acetic acid solution is obtained by dissolving boric acid in glacial acetic acid with a molar ratio of 10 times.

5. The preparation method according to claim 2, characterized in that: The process conditions of the heating and stirring reaction are: stirring rate 500 rpm, temperature 60° C., and stirring time 4 to 7 h.

6. Use of the isoalloxazine compound according to claim 1 in preparing a flexible binder-free zinc ion battery positive electrode material.

7. A flexible binder-free zinc ion battery positive electrode material, characterized in that: The isoalloxazine compound described in claim 1 is used as an active material, and MXene is used as a flexible substrate.

8. A flexible binder-free zinc ion battery positive electrode material according to claim 7, characterized in that: MXene is prepared by the following method: first slowly add lithium fluoride to concentrated hydrochloric acid, mix at room temperature, carefully add Ti3AlC2 powder, heat and stir to react, and then post-treat to obtain it.

9. Use of the positive electrode material according to claim 7 in preparing a flexible zinc ion battery.

10. The use according to claim 9, characterized in that: The zinc ion battery is obtained by assembling and packaging a carbon cloth positive electrode containing the above-mentioned positive electrode material, a zinc-deposited carbon cloth, and a PVA hydrogel electrolyte in a sandwich structure.

Citation Information

Patent Citations

  • Organic composite positive electrode material, preparation method thereof and all-solid-state battery

    CN114242979A

  • Conjugated quinone azine organic electrode material and preparation method and application thereof

    CN114497547A

  • MXene / mesoporous polypyrrole composite material, preparation method thereof, electrode and energy storage device

    CN114497705A

  • Pyrazine skeleton pyrimidine ring substituted derivative, preparation method thereof and flow battery

    CN116425753A

  • Covalent organic framework containing anthraquinone structure and application of covalent organic framework in aqueous zinc ion battery

    CN116925308A

Cited By

  • Aqueous zinc-based electrolyte and preparation method and application thereof

    CN120149582A