Preparation method of low-bulk-density hydroxypropyl methylcellulose

Through the mixed alkali treatment of solid alkali and liquid alkali and multiple centrifugal washing processes, low-loose density hydroxypropyl methylcellulose was successfully prepared, solving the problem of high loose density in the prior art and improving the compressibility and ease of the preparation Controlled release performance, suitable for industrial mass production.

CN118994422APending Publication Date: 2024-11-22ANHUI SUNHERE PHARMA EXCIPIENTS
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411256878.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-09
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

In the prior art, there are fewer preparation methods for low-volume density hydroxypropyl methylcellulose, resulting in higher loose density of domestically produced hydroxypropyl methylcellulose, affecting the compressibility and slow-release performance of the preparation.

Method used

The mixed alkali of solid alkali and liquid alkali is treated with a mixture of solid alkali and liquid alkali. After low-temperature alkali, the alkali is added to alkaline for alkalinization. The etherification reaction is then carried out, and the loose density of the product is controlled by multiple centrifugation. Finally, the loose density is obtained by sieving. Low-volume density hydroxypropyl methylcellulose with a density of 0.26-0.31 g/mL.

Benefits of technology

It improves the compressibility and sustained release performance of hydroxypropyl methylcellulose, is suitable for direct powder pressing agents, has high production efficiency, environmental protection, and is suitable for large-scale industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005034353370000091
    Figure BDA0005034353370000091
Patent Text Reader

Abstract

The invention discloses a preparation method of low-bulk-density hydroxypropyl methylcellulose, and belongs to the technical field of pharmaceutical excipients, the preparation method comprises the following steps: adding solid alkali and liquid alkali into a mixed solution of toluene, isopropanol and water, performing alkalization at 80-90 DEG C for 25-35 minutes, and then cooling the system to 15-25 DEG C; adding refined cotton into the system, and carrying out alkalization reaction for 115-125 minutes; adding epoxypropane and chloromethane into the system, uniformly stirring and mixing, heating to 80-90 DEG C, and carrying out etherification reaction for 2.5-3.5 hours; adjusting the pH value of the system to 6.5-7.5, and completely recovering the solvent; adding hot water into the material, repeatedly washing twice, and centrifuging until the water content is less than or equal to 35% after washing each time; drying and sieving; the bulk density of the hydroxypropyl methylcellulose prepared by the method is 0.26-0.31 g / mL, and the compressibility of the hydroxypropyl methylcellulose can be improved when powder is directly compressed.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of pharmaceutical excipients, and particularly relates to a method for preparing low bulk density hypromellose. Background Art

[0002] In the preparation production process, compared with the wet granulation tableting method, the use of powder direct tableting method can ensure product quality, and the process is simple, which can save a large part of the raw materials and improve production efficiency.

[0003] Hydroxypropyl methylcellulose is a partial methyl and partial polyhydroxypropyl ether of cellulose; it has many properties that other excipients do not have. It has excellent cold water solubility and can be dissolved into a transparent solution with a little stirring in cold water. On the contrary, it is basically insoluble in more than 60% hot water and can only swell. It is a non-ionic cellulose ether, and its solution does not carry ionic charge, does not react with metal salts or ionic organic compounds, and does not react with other raw materials and excipients during the preparation production process; it has strong anti-allergic properties, and with the increase of the degree of substitution in the molecular structure, its anti-allergic properties are stronger and more stable; as a pharmaceutical excipient, it is widely used in sustained-release preparations because of its good biocompatibility, strong drug loading capacity and excellent biochemical inertness.

[0004] The surface of low bulk density HPMC is rough and porous, which gives it a larger specific surface area. When the preparation powder is tableted, it is more conducive to contact and embedding with the raw material particles, which can rearrange and combine the particles during the tablet forming process, making the tablet stronger. Therefore, low bulk density HPMC will show better compressibility when the powder is directly tableted.

[0005] Chinese patent CN 108129575 A discloses a method for preparing low-viscosity pharmaceutical excipient hydroxypropyl methylcellulose for plant capsules. The method comprises the following steps: crushing the refined cotton and putting it into a mixed solvent of toluene, isopropanol and water, adding solid sodium hydroxide to alkalize the cellulose, and the whole process takes 6-8 hours; then putting in propylene oxide and methyl chloride to start a staged temperature rise etherification reaction; putting the material after the etherification reaction into a desolventizing kettle for neutralization, and then starting to heat up and desolventize for a total of 2.5-3.5 hours, keeping the temperature above 100°C for centrifugal separation, and separating it into a viscosity reduction kettle for viscosity reduction; the viscosity reduction time is 3-4 hours, the temperature is maintained above 95°C, and the pH is adjusted to between 5-6 after the viscosity reduction is completed; after the viscosity reduction, the material is centrifuged into a washing kettle with 8-10 tons of softened water above 95°C, and the temperature in the kettle is maintained after the centrifugation is completed for discharging and drying; then crushing, sieving, and packaging. This patent does not focus on the bulk density of HPMC, and if HPMC is prepared according to the method disclosed in this patent, the bulk density of the prepared HPMC will be relatively high.

[0006] There are few reports on low bulk density hydroxypropyl methylcellulose in the prior art. Therefore, designing a process for low bulk density hydroxypropyl methylcellulose is of great significance for domestically produced hydroxypropyl methylcellulose. Summary of the invention

[0007] In order to solve the above technical problems, the present invention provides a method for preparing low bulk density hypromellose, which can prepare low bulk density hypromellose with a bulk density of 0.26-0.31 g / mL, and can improve the compressibility of hypromellose when direct powder compression is performed.

[0008] The technical solution adopted by the present invention is as follows:

[0009] The present invention provides a method for preparing low bulk density hypromellose, comprising the following steps:

[0010] (1) adding solid alkali and liquid alkali to a mixed solution of toluene, isopropanol and water, alkaliizing at 80-90° C. for 25-35 minutes, and then cooling the system to 15-25° C.;

[0011] (2) Add refined cotton to the system and carry out alkalization reaction for 115 to 125 minutes;

[0012] (3) Add propylene oxide and methyl chloride to the system, stir and mix evenly, and then heat to 80-90° C. for etherification reaction for 2.5-3.5 hours;

[0013] (4) adjusting the pH of the system to 6.5-7.5 and recovering all the solvent;

[0014] (5) adding hot water to the material, stirring evenly and centrifuging until the weight percentage of water in the material is ≤35%;

[0015] (6) adding hot water to the material again, stirring evenly and centrifuging until the weight percentage of water in the material is ≤35%;

[0016] (7) drying and sieving;

[0017] The low bulk density hypromellose has a bulk density of 0.26-0.31 g / mL.

[0018] In step (1), the solid alkali is solid sodium hydroxide; and the liquid alkali is a sodium hydroxide solution with a mass concentration of 35 to 45%.

[0019] In step (1), the mass ratio of the solid alkali to the liquid alkali is 1:2.5-3.5. If only the solid alkali is used, the alkalization speed is slow and the alkalization efficiency is low. If only the liquid alkali is used, the water content of the reaction solution is high, which will lead to an increase in by-products in the reaction system. The weight ratio of the sum of the solid alkali and the liquid alkali to the mixed solution is 1:8-13.

[0020] In step (1), the volume ratio of toluene, isopropanol and water is 15-20:2.5-3.5:1.

[0021] In step (2), the solid-liquid ratio of the purified cotton to the reaction solution is 1 g: 10-12 mL.

[0022] In step (3), the mass ratio of refined cotton to propylene oxide and methyl chloride is 1:0.2-0.4:0.6-1.0.

[0023] The step (4) specifically comprises the following steps: pumping the reaction liquid after the etherification reaction into a desolventizing kettle, adding a hydrochloric acid solution with a mass concentration of 30% to adjust the pH of the reaction liquid to 6.5-7.5, and then introducing steam into the desolventizing kettle to recover the solvent.

[0024] In step (5) and step (6), the temperature of the hot water is above 95° C.; the weight of the hot water is 100 to 130 times the weight of the refined cotton.

[0025] In step (7), the drying temperature is 70-120°C.

[0026] In step (7), the sieving is through a 100-mesh sieve.

[0027] The preparation method of low bulk density hydroxypropyl methylcellulose provided by the present invention comprises the following steps: firstly, solid alkali and liquid alkali are added to a mixed solution of toluene, isopropanol and water for alkalization, which greatly improves the efficiency of alkalization, avoids alkali crystal deposition, and makes the alkalization reaction more complete, compared with directly using solid alkali, or adding refined cotton and then adding solid alkali, or then adding a mixture of solid alkali and liquid alkali. After alkalization of refined cotton, propylene oxide and methyl chloride are added for etherification reaction, and after the etherification reaction, the pH of the reaction system is adjusted to 6.5-7.5, and then the solvent is recovered; and then the material after the solvent is recovered is washed twice with hot water, and the weight percentage of water in the material is controlled to be ≤35% after each washing, and then the hydroxypropyl methylcellulose with a bulk density of 0.26-0.31 g / mL is obtained after drying and sieving.

[0028] Compared with the prior art, the present invention has the following beneficial effects:

[0029] The present invention prepares low bulk density hydroxypropyl methylcellulose by low-temperature alkali treatment of a mixed region of solid alkali and liquid alkali in a mixed solution, then low-temperature alkalization and one-step etherification of refined cotton, and controlling the moisture content of the wet material after centrifugation during product washing. The hydroxypropyl methylcellulose prepared by the present invention has low bulk density and good compressibility, and can significantly improve the sustained release performance of the powder during direct compression.

[0030] The preparation process of low bulk density hypromellose provided by the invention has high production efficiency, is environmentally friendly, and is suitable for industrial mass production. DETAILED DESCRIPTION

[0031] The present invention is described in detail below with reference to the embodiments.

[0032] Example 1

[0033] A method for preparing low bulk density hypromellose, comprising the following steps:

[0034] (1) adding 450 g of solid sodium hydroxide and a 40% sodium hydroxide aqueous solution in a mass ratio of 1:3 to a mixed solution of 4000 g toluene, 750 g isopropanol and 250 g water, alkali treatment was carried out at 85° C. for 30 min, and then the system was cooled to 20° C.;

[0035] (2) Add 450 g of refined cotton to the system and alkalize for 120 min;

[0036] (3) Add 135 g of propylene oxide and 400 g of methyl chloride to the system, stir and mix for 20 min, then heat to 86 °C for etherification reaction for 3.0 h;

[0037] (4) the reaction liquid after the etherification reaction is pumped into a desolventizing kettle, a hydrochloric acid solution with a mass concentration of 30% is added to adjust the pH of the reaction liquid to 7.0, and then water vapor is introduced into the desolventizing kettle to recover the solvent;

[0038] (5) Add 50 kg of hot water above 95° C. to the material, stir evenly, and then centrifuge until the weight percentage of water in the material is 30%;

[0039] (6) Add 50 kg of hot water above 95° C. to the material again, stir evenly, and then centrifuge until the weight percentage of water in the material is 25%;

[0040] (7) Dry at 100°C and pass through a 100-mesh sieve to obtain hydroxypropyl methylcellulose powder.

[0041] Example 2

[0042] A method for preparing low bulk density hypromellose, comprising the following steps:

[0043] (1) adding 500 g of solid-liquid alkali composed of solid sodium hydroxide and a sodium hydroxide aqueous solution with a mass concentration of 45% in a mass ratio of 1:2.5 to a mixed solution composed of 4000 g of toluene, 700 g of isopropanol and 200 g of water, alkaliizing at 80° C. for 35 min, and then cooling the system to 15° C.;

[0044] (2) Add 410 g of refined cotton to the system and alkalize for 115 min;

[0045] (3) Add 130 g of propylene oxide and 380 g of methyl chloride to the system, stir and mix for 20 min, and then heat to 90 ° C for etherification reaction for 2.5 h;

[0046] (4) the reaction liquid after the etherification reaction is pumped into a desolventizing kettle, a hydrochloric acid solution with a mass concentration of 30% is added to adjust the pH of the reaction liquid to 7.0, and then water vapor is introduced into the desolventizing kettle to recover the solvent;

[0047] (5) Add 45 kg of hot water above 95° C. to the material, stir evenly, and then centrifuge until the weight percentage of water in the material is 35%;

[0048] (6) Add 45 kg of hot water above 95° C. to the material again, stir evenly, and then centrifuge until the weight percentage of water in the material is 30%;

[0049] (7) Dry at 90°C and pass through a 100-mesh sieve to obtain hydroxypropyl methylcellulose powder.

[0050] Comparative Example 1

[0051] A method for preparing hypromellose comprises the following steps:

[0052] (1) Add 250 g of solid sodium hydroxide to a mixed solution consisting of 4000 g of toluene, 750 g of isopropanol, and 250 g of water, alkalize at 85° C. for 30 min, and then cool the system to 20° C.;

[0053] (2) Add 450 g of refined cotton to the system and alkalize for 120 min;

[0054] (3) Add 135 g of propylene oxide and 400 g of methyl chloride to the system, stir and mix for 20 min, then heat to 86 °C for etherification reaction for 3.0 h;

[0055] (4) the reaction liquid after the etherification reaction is pumped into a desolventizing kettle, a hydrochloric acid solution with a mass concentration of 30% is added to adjust the pH of the reaction liquid to 7.0, and then water vapor is introduced into the desolventizing kettle to recover the solvent;

[0056] (5) Add 50 kg of hot water above 95° C. to the material, stir evenly, and then centrifuge until the weight percentage of water in the material is 30%;

[0057] (6) Add 50 kg of hot water above 95° C. to the material again, stir evenly, and then centrifuge until the weight percentage of water in the material is 25%;

[0058] (7) Dry at 100°C and pass through a 100-mesh sieve to obtain hydroxypropyl methylcellulose powder.

[0059] Comparative Example 2

[0060] A method for preparing hypromellose comprises the following steps:

[0061] (1) adding 450 g of solid-liquid alkali composed of solid sodium hydroxide and a sodium hydroxide aqueous solution with a mass concentration of 40% in a mass ratio of 1:3 to a mixed solution composed of 4000 g of toluene, 750 g of isopropanol and 250 g of water, and alkali treatment was carried out at 85° C. for 30 min;

[0062] (2) Add 450 g of refined cotton to the system and react at 85°C for 120 min;

[0063] (3) Add 135 g of propylene oxide and 400 g of methyl chloride to the system, stir and mix for 20 min, and then carry out etherification reaction at 86° C. for 3.0 h;

[0064] (4) the reaction liquid after the etherification reaction is pumped into a desolventizing kettle, a hydrochloric acid solution with a mass concentration of 30% is added to adjust the pH of the reaction liquid to 7.0, and then water vapor is introduced into the desolventizing kettle to recover the solvent;

[0065] (5) Add 50 kg of hot water above 95° C. to the material, stir evenly, and then centrifuge until the weight percentage of water in the material is 30%;

[0066] (6) Add 50 kg of hot water above 95° C. to the material again, stir evenly, and then centrifuge until the weight percentage of water in the material is 25%;

[0067] (7) Dry at 100°C and pass through a 100-mesh sieve to obtain hydroxypropyl methylcellulose powder.

[0068] Comparative Example 3

[0069] A method for preparing hypromellose comprises the following steps:

[0070] (1) adding 450 g of solid sodium hydroxide and a 40% sodium hydroxide aqueous solution in a mass ratio of 1:3 to a mixed solution of 4000 g toluene, 750 g isopropanol and 250 g water, alkali treatment was carried out at 85° C. for 30 min, and then the system was cooled to 20° C.;

[0071] (2) Add 450 g of refined cotton to the system and alkalize for 120 min;

[0072] (3) Add 135 g of propylene oxide and 400 g of methyl chloride to the system, stir and mix for 20 min, then heat to 86 °C for etherification reaction for 3.0 h;

[0073] (4) the reaction liquid after the etherification reaction is pumped into a desolventizing kettle, a hydrochloric acid solution with a mass concentration of 30% is added to adjust the pH of the reaction liquid to 7.0, and then steam is introduced into the desolventizing kettle to recover the solvent;

[0074] (5) Add 50 kg of hot water above 95° C. to the material, stir evenly, and then centrifuge until the weight percentage of water in the material is 50%;

[0075] (6) adding 50 kg of hot water above 95° C. to the material again, stirring evenly and centrifuging until the weight percentage of water in the material is 52%;

[0076] (7) Dry at 100°C and pass through a 100-mesh sieve to obtain hydroxypropyl methylcellulose powder.

[0077] Comparative Example 4

[0078] A method for preparing hypromellose comprises the following steps:

[0079] The refined cotton is crushed into cotton powder with a size of more than 100 meshes for production use; 4900g of a mixed solvent consisting of toluene, isopropanol and water in a volume ratio of 16:3:1 is added, and then 450g of cotton powder is added into the mixed solvent, and 250g of solid sodium hydroxide is added to carry out alkalization treatment of cellulose, and the whole process takes 7 hours; 135g of propylene oxide and 400g of methyl chloride are added to start etherification reaction; the temperature is raised to 50°C and kept for 3 hours in the first stage, and the temperature is raised to 80°C and kept for 3 hours in the second stage; the material after the etherification reaction is put into a desolventizing kettle, glacial acetic acid is added to adjust the pH of the reaction solution to 7.0, and then the temperature is raised to desolventize, the temperature is 85-100°C, the time is 3.5 hours, and the temperature is kept above 100°C for centrifugal separation, and after separation, it is dried, crushed and sieved to obtain the finished product.

[0080] Comparative Example 5

[0081] A method for preparing hypromellose comprises the following steps:

[0082] The refined cotton is crushed into cotton powder with a size of more than 100 meshes for production use; 4900g of a mixed solvent consisting of toluene, isopropanol and water in a volume ratio of 16:3:1 is added, then 450g of the refined cotton powder is added into the mixed solvent, and 450g of a solid-liquid alkali consisting of solid sodium hydroxide and a sodium hydroxide aqueous solution with a mass concentration of 40% in a mass ratio of 1:3 is added to carry out alkalization treatment of the cellulose, and the whole process takes 7 hours; 135g of propylene oxide and 400g of methyl chloride are added to start an etherification reaction; the first stage is heated to 50°C and kept warm for 3 hours, and the second stage is heated to 80°C and kept warm for 3 hours; the material after the etherification reaction is put into a desolventizing kettle, glacial acetic acid is added to adjust the pH of the reaction liquid to 7.0, and then the temperature is increased for desolventizing at 85-100°C for 3.5 hours, and the temperature is kept above 100°C for centrifugal separation, and after separation, it is dried, crushed and sieved to obtain a finished product.

[0083] The bulk density, methoxy content and hydroxypropoxy content of the hypromellose prepared in the above-mentioned embodiments and comparative examples were tested, and the results are shown in Table 1.

[0084] Table 1

[0085]

[0086] The methoxy content and hydroxypropoxy content were tested according to the method in Part IV of the 2020 edition of the Chinese Pharmacopoeia.

[0087] Bulk density test method: Take a 100ml clean and dry measuring cylinder, tilt it slightly, and gently pour the weighed Mg sample into the measuring cylinder. Use a long-handled spoon to gently smooth the surface (be careful not to press the sample tightly), read the volume (V0), and calculate the bulk density according to the formula M / V0. Repeat the measurement three times and take the average value.

[0088] It can be seen from the above that the preparation method of the present invention can be used to prepare hydroxypropyl methylcellulose with a bulk density of 0.26-0.31 g / mL.

[0089] Comparative Example 1 is relative to Example 1, in which solid sodium hydroxide is directly added for alkalization. At the same time and temperature, solid sodium hydroxide will produce alkali crystals and precipitate at the bottom of the equipment during alkalization, affecting the subsequent alkalization reaction and efficiency and the degree of alkalization, and further affecting the bulk density of hydroxypropyl methylcellulose, resulting in a higher bulk density.

[0090] Comparative Example 2 Compared with Example 1, the temperature during the alkalization of refined cotton is higher, which is not conducive to the formation of alkali cellulose, resulting in the inability to fully carry out the alkalization reaction, and further affecting the bulk density of hydroxypropyl methylcellulose, resulting in a higher bulk density.

[0091] Comparative Example 3 Compared with Example 1, the moisture content of the material after hot water washing and centrifugation is relatively high, which will cause the material to absorb water and become gel-like. After drying, it will become hard particles, and further affect the bulk density of HPMC, resulting in a higher bulk density.

[0092] Comparative Examples 4 and 5 adopt the currently commonly used method for preparing hypromellose, and the bulk density of the hypromellose prepared by this method is also relatively high.

[0093] The detailed description of the preparation method of low bulk density hydroxypropyl methylcellulose with reference to the above-mentioned examples is illustrative rather than restrictive, and several examples can be listed according to the limited scope. Therefore, changes and modifications without departing from the overall concept of the present invention should fall within the scope of protection of the present invention.

Claims

1. A method for preparing low bulk density hypromellose, characterized in that: The preparation method comprises the following steps: (1) adding solid alkali and liquid alkali to a mixed solution of toluene, isopropanol and water, alkaliizing at 80-90° C. for 25-35 minutes, and then cooling the system to 15-25° C.; (2) Add refined cotton to the system and carry out alkalization reaction for 115 to 125 minutes; (3) Add propylene oxide and methyl chloride to the system, stir and mix evenly, and then heat to 80-90° C. for etherification reaction for 2.5-3.5 hours; (4) adjusting the pH of the system to 6.5-7.5 and recovering all the solvent; (5) adding hot water to the material, stirring evenly and centrifuging until the weight percentage of water in the material is ≤35%; (6) adding hot water to the material again, stirring evenly and centrifuging until the weight percentage of water in the material is ≤35%; (7) drying and sieving; The low bulk density hypromellose has a bulk density of 0.26-0.31 g / mL.

2. The preparation method according to claim 1, characterized in that: In step (1), the solid alkali is solid sodium hydroxide; and the liquid alkali is a sodium hydroxide solution with a mass concentration of 35 to 45%.

3. The preparation method according to claim 1, characterized in that: In step (1), the mass ratio of the solid alkali to the liquid alkali is 1:2.5-3.5; the weight ratio of the sum of the solid alkali and the liquid alkali to the mixed solution is 1:8-13.

4. The preparation method according to claim 1, characterized in that: In step (1), the volume ratio of toluene, isopropanol and water is 15-20:2.5-3.5:

1.

5. The preparation method according to claim 1, characterized in that: In step (2), the solid-liquid ratio of the purified cotton to the reaction solution is 1 g: 10-12 mL.

6. The preparation method according to claim 1, characterized in that: In step (3), the mass ratio of refined cotton to propylene oxide and methyl chloride is 1:0.2-0.4:0.6-1.

0.

7. The preparation method according to claim 1, characterized in that: In step (5) and step (6), the temperature of the hot water is above 95° C.; the weight of the hot water is 100 to 130 times the weight of the refined cotton.

8. The preparation method according to claim 1, characterized in that: In step (7), the drying temperature is 70-120°C.

9. The preparation method according to claim 1, characterized in that: In step (7), the sieving is through a 100-mesh sieve.