Polypropylene as well as preparation method and application thereof

By using a double-ring reactor and asymmetric hydrogenation method in the polymerization reaction, combining the cocatalyst and external electron donor, the problems of low puncture strength and breakdown resistance of polypropylene products in the lithium battery separator are solved, and excellent preparation is made Polypropylene with performance is suitable for lithium battery separators below 10 microns.

CN118994449AActive Publication Date: 2024-11-22XINJIANG DUSHANZI PETROCHEMICAL CO LTD +1
View PDF 14 Cites 0 Cited by

Patent Information

Application Number
CN202411489356.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-24
Publication Date
2024-11-22
Estimated Expiration
2044-10-24

AI Technical Summary

Technical Problem

Existing polypropylene products have problems such as low puncture strength or low breakdown voltage in lithium battery separators, which affects their application effect.

Method used

A double-ring tube reactor was used to carry out multi-step polymerization reaction, combined with asymmetric hydrogenation method, cocatalyst and external electron donor treatment, polypropylene with a wide molecular weight distribution was prepared to improve its puncture strength and breakdown voltage resistance.

Benefits of technology

The prepared polypropylene products show strong puncture strength and high breakdown resistance voltage in lithium battery separators below 10 microns, improving the comprehensive performance of lithium battery separators.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention provides polypropylene and a preparation method and application thereof, and the preparation method comprises the following steps: taking propylene, hydrogen, a catalyst, a cocatalyst and an external electron donor, and carrying out a first polymerization reaction in a first loop reactor, adding propylene and hydrogen into the obtained first polymerization reaction post-material in a second loop reactor for second polymerization reaction, and sequentially steaming, drying and granulating the obtained second polymerization reaction post-material to obtain polypropylene; the melt flow rate of the polypropylene obtained by the invention is 0.2 g / 10min to 0.4 g / 10min, the isotacticity is 98.5% to 99.0%, the ash content is 0.0015% to 0.003%, the molecular weight distribution index is 6 to 9, and the weight-average molecular weight is 500,000 to 7,000,000, and when the polypropylene is used for preparing a 10-micron lithium battery diaphragm, the polypropylene shows relatively high puncture strength and relatively high breakdown voltage resistance, and has excellent performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of polyolefin resins, and in particular to polypropylene and a preparation method and application thereof. Background Art

[0002] With the development of the new energy industry, the comprehensive indicators of the downstream lithium battery industry such as capacity, energy density, performance, and safety are constantly improving, and the demand for thinner and more functional diaphragm products will further increase. Thin diaphragm products have always been one of the key development focuses of the lithium battery diaphragm industry.

[0003] At present, polyolefin separators are used as common lithium battery separators, and their materials mainly include polyethylene and polypropylene. Among them, the production process of polypropylene lithium battery separators is a dry process, which can be further divided into unidirectional stretching and bidirectional stretching according to different stretching directions. The dry unidirectional stretching process (dry single-stretching process) first stretches at low temperature to form defects such as silver streaks, and then pulls the defects apart at high temperature to form a flat microporous structure. The principle of the dry bidirectional stretching process (dry double-stretching process) is to add a β-crystal modifier with a nucleating effect to polypropylene. It is mainly based on the difference in density between different phases of polypropylene, and the crystal form of polypropylene changes under the action of thermal stress during the stretching process to form a microporous structure. However, more than 90% of the dry processes for the production of lithium battery separators in China today are dry single-stretching processes.

[0004] The Chinese patent document with publication number CN115322271A discloses a special material for polypropylene lithium battery separator and its preparation method. The method uses liquid bulk gas phase polymerization process to prepare a special material for polypropylene lithium battery separator with high isotactic index and low ash content. Among them, the isotactic index can reach 99.3%, and the ash content can be reduced to 0.006%. The production process of the precursor film prepared by it is stable, safe, and controllable, so that the catalyst cost can be reduced, and the precursor film has good tensile properties. The performance indicators of the product prepared by the invention can simultaneously meet the melt flow rate (2.16kg) 2.00±0.10g / 10min, isotactic index ≥98.0%, ash ≥0.0100%, and crystallinity ≥48.5%. The Chinese patent document with the authorization announcement number CN115160463B discloses a method for producing high-purity, low-precipitate polypropylene, which comprises: mixing propylene monomer with a main catalyst, an external electron donor, and an activator, and adding the mixture to a prepolymerization reactor, and then sequentially entering the first loop reactor and the second loop reactor for polymerization reaction; the product is subjected to flash evaporation to remove liquid propylene, an antistatic agent is added during flash evaporation, and then further degassing, steaming, and drying treatment are performed to obtain homopolymerized polypropylene powder. Finally, a compounding auxiliary agent is added and mixed, and the mixture is melt-cut and pelletized by an extruder to obtain a homopolymerized polypropylene resin. The invention adopts a Ziegler-Natta catalyst and is directly generated by a one-step method. It is a high-purity polypropylene material (ash content is less than 30 mg / kg, ultra-pure polypropylene) with a high isotactic index, a wide molecular weight distribution, and a relatively small content of small molecules. It has the characteristics of high withstand voltage at high temperature, excellent dielectric breakdown characteristics, good film-forming processing performance, and less smoke and precipitation of oligomers. It is mainly used in capacitor films and lithium battery separators.

[0005] The Chinese patent document with publication number CN112876591A discloses an industrial production method for polypropylene resin for battery separators. In a double loop reactor, a synergistic hydrogen transfer catalyst (HCAT) is used to produce polypropylene powder, and the polypropylene powder and resin additives are melt-extruded and granulated. The obtained polypropylene resin product has the characteristics of high isotacticity and low ash content. The product is mainly used as a raw material for battery separators and applied to the lithium-ion battery industry. The Chinese patent document with the Chinese invention publication number CN111019026A discloses a method for preparing a polypropylene resin for lithium battery separators with high isotacticity, comprising the following steps: adding propylene to a polymerization kettle, stirring and heating to 35-40°C, then adding a co-catalyst, an external electron donor and a supported main catalyst thereto, and introducing hydrogen, controlling the polymerization reaction temperature to 75-80°C, the polymerization reaction pressure to 0.6-0.8MPa, and the polymerization reaction time to 120-240min, to obtain a polypropylene resin for lithium battery separators with high isotacticity. The polymerization process of the invention adopts an intermittent bulk method. By controlling parameters such as the melt index of the product in the polymerization reaction process at 0.3~2.1g / 10min, the polymerization reaction temperature at 75~80°C, the polymerization reaction pressure at 0.6~0.8MPa, the polymerization reaction time at 120~240min, and the amount of the external electron donor at 10~18% of the total mass of the catalyst, polypropylene resin particles with an isotacticity of more than 98.8% and an elastic recovery rate of more than 90% are obtained, which are used to produce high-performance, high-value-added lithium battery separators, greatly improving the quality and film-forming rate of the lithium battery separators.

[0006] The Chinese patent document with the publication number CN106397643A discloses a method for producing a special material for polypropylene resin particles for lithium battery membranes. The specific steps include: in four series reactors, by controlling different residence times and different product melt flow rates, the lithium battery membrane material is finally prepared. By adjusting the process parameters of each reactor and strictly controlling the melt flow rate of each reactor, the problem that the special material for polypropylene lithium battery separator needs to have a wide molecular weight distribution and good film-forming performance is solved; by adjusting the polymerization temperature of each reactor and strictly controlling it within the specified range, the problem that the lithium battery membrane material needs to have good mechanical properties, including puncture strength and tensile strength, is solved. The Chinese patent document with the authorization announcement number CN103540020B discloses a method for producing a special material for homopolymer polypropylene for lithium ion battery barrier membrane. The invention uses a propylene polymerization catalyst with high activity and moderate hydrogen sensitivity. The propylene polymerization activator is triethyl aluminum, and its addition amount is controlled to be less than 7.0L / hour. The external electron donor uses dicyclopentyldimethoxysilane and tetraethoxysilane. In the granulation section of the invention, a stabilizer system consisting of a primary antioxidant, a secondary antioxidant and an acid scavenger is added. The final product is a BOPP film material for lithium ion barrier film production with an isotacticity greater than 98%, a melt flow rate (MFR) controlled at 2.8±0.2g / 10min, an ash content controlled at 50~100ppm, a volatile content less than 100ppm, an oxidation induction period greater than 15min, and a molecular weight distribution controlled at 7.0~10.0.

[0007] Therefore, the above patents are all about preparing polypropylene materials for lithium-ion separators, but all of the above polypropylene products are used for lithium battery separators with a thickness of more than 10 microns. When used for lithium battery separators with a thickness of less than 10 microns, they all have low puncture strength and low breakdown voltage, which affects their application in lithium batteries.

[0008] Based on this, in the face of the problem that polypropylene products in the prior art have low puncture strength or low breakdown voltage when used in lithium battery separators, there is an urgent need to provide a polypropylene and a preparation method thereof to improve the above problems. Summary of the invention

[0009] The main purpose of the present invention is to provide a polypropylene and a preparation method and application thereof, so as to solve the problem that the polypropylene products in the prior art have low puncture strength or low breakdown voltage when used in lithium battery separators.

[0010] In order to achieve the above object, according to one aspect of the present invention, a method for preparing polypropylene is provided, the method comprising: step S1, taking propylene, hydrogen, a catalyst, a co-catalyst and an external electron donor in a first loop reactor of a double loop reactor to carry out a first polymerization reaction to obtain a first polymerization reaction material; Step S2, taking the first polymerization reaction material, adding propylene and hydrogen, and carrying out a second polymerization reaction in the second loop reactor of the double loop reactor to obtain a second polymerization reaction material; Step S3, taking the material after the second polymerization reaction and sequentially performing steaming, drying and granulation treatments to obtain polypropylene; The double loop reactor comprises a first loop reactor and a second loop reactor, the molar amount of hydrogen added to the first loop reactor accounts for 0.007% to 0.015% of propylene, and the molar amount of additional hydrogen added to the second loop reactor accounts for 0.4% to 0.6% of the additional propylene; the co-catalyst is triethylaluminum, and the amount of the co-catalyst added accounts for 0.0018% to 0.0025% of the weight of propylene; the external electron donor is cyclohexylmethyldimethoxysilane and / or dicyclopentyldimethoxysilane, and the weight ratio of the external electron donor added to the co-catalyst is 1:1 to 3; in step S3, the temperature of the steaming treatment is 100°C to 130°C, the time is 0.2h to 0.5h, and the temperature of the drying treatment is 70°C to 100°C, and the time is 0.1h to 0.3h.

[0011] Furthermore, the molar amount of hydrogen added to the first loop reactor accounts for 0.007% to 0.012% of the propylene, and the molar amount of additional hydrogen added to the second loop reactor accounts for 0.5% to 0.6% of the additional propylene.

[0012] Furthermore, in step S2, the weight ratio of the amount of the additional propylene to the material after the first polymerization reaction is (0.5~1):1.

[0013] Furthermore, the catalyst is a titanium-based catalyst, the model of the titanium-based catalyst is HA catalyst and / or HA-R catalyst, and the activity of the titanium-based catalyst is 100,000 gPP / g catalyst to 200,000 gPP / g catalyst.

[0014] Furthermore, the reaction temperature of the double loop reactor is 67° C. to 73° C., the reaction time is 1.5 h to 3.0 h, and the reaction pressure is 3.6 MPa to 4.0 MPa.

[0015] In order to achieve the above object, according to one aspect of the present invention, a polypropylene is provided, which is a polypropylene product obtained by the above preparation method.

[0016] Furthermore, the melt flow rate of the polypropylene is 0.2 g / 10 min to 0.4 g / 10 min, the isotacticity is 98.5% to 99.0%, the ash content is 0.0015% to 0.0030%, the molecular weight distribution index is 6 to 9, and the weight average molecular weight is 500,000 to 700,000.

[0017] According to another aspect of the present invention, there is provided an application of polypropylene in the field of lithium battery separators.

[0018] The polypropylene product obtained by applying the technical solution of the present invention, when used for preparing a 10-micron lithium battery separator, exhibits strong puncture strength and high breakdown voltage resistance, and has excellent performance. DETAILED DESCRIPTION

[0019] In order to make the purpose, technical solutions and advantages of the embodiments of the present application clearer, the technical solutions in the embodiments of the present application are clearly and completely described. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.

[0020] According to what is described in the background technology part of the present invention, the polypropylene products in the prior art have the problem of low puncture strength or low breakdown voltage when used in lithium battery separators. Based on this, the present invention provides a method for preparing polypropylene, which comprises: step S1, taking propylene, hydrogen, a catalyst, a co-catalyst and an external electron donor in a first loop reactor of a double loop reactor to carry out a first polymerization reaction to obtain a first polymerization reaction material; step S2, taking the first polymerization reaction material, adding propylene and hydrogen to the second loop reactor of the double loop reactor to carry out a second polymerization reaction to obtain a second polymerization reaction material; step S3, taking the second polymerization reaction material and then steaming, drying and granulating it in sequence to obtain polypropylene; wherein the double loop reactor comprises a first loop reactor and a second loop reactor, and the first loop reactor The molar amount of hydrogen added in the reactor accounts for 0.007% to 0.015% of propylene, and the molar amount of additional hydrogen added in the second loop reactor accounts for 0.4% to 0.6% of the additional propylene; the co-catalyst is triethylaluminum, and the amount of the co-catalyst added accounts for 0.0018% to 0.0025% of the weight of propylene; the external electron donor is cyclohexylmethyldimethoxysilane and / or dicyclopentyldimethoxysilane, and the weight ratio of the external electron donor added to the co-catalyst is 1:1 to 3; in step S3, the temperature of the steaming treatment is 100°C to 130°C, the time is 0.2h to 0.5h, and the temperature of the drying treatment is 70°C to 100°C, and the time is 0.1h to 0.3h.

[0021] Based on the polypropylene material for lithium ion separators prepared in the prior art, the polypropylene product is used for lithium battery separators with a thickness of more than 10 microns. When used for lithium battery separators with a thickness of less than 10 microns, it has low puncture strength and low breakdown voltage, which affects its application in lithium batteries. The invention adopts a novel preparation method to prepare polypropylene, and the preparation method comprises: step S1, taking propylene, hydrogen, a catalyst, a co-catalyst and an external electron donor in a first loop reactor of a double loop reactor to carry out a first polymerization reaction to obtain a first polymerization reaction material; step S2, taking the first polymerization reaction material, adding propylene and hydrogen to carry out a second polymerization reaction in a second loop reactor of the double loop reactor to obtain a second polymerization reaction material; step S3, taking the second polymerization reaction material and then sequentially performing steaming, drying and granulation treatment to obtain polypropylene; wherein the double loop reactor comprises a first loop reactor and a second loop reactor, and in particular, the molar amount of hydrogen added in the first loop reactor accounts for 0.007% to 0.015% of propylene, and the molar amount of the additional hydrogen added in the second loop reactor accounts for 0.4% to 0.6% of the additional propylene. The hydrogenation method of the asymmetric hydrogenation can maximize the molecular weight distribution of the product, so that the product has both a small molecule part, which can ensure that it has good processing performance, and a large molecule part, which can ensure the mechanical properties of the product, so that the polypropylene product has both excellent processing performance and excellent mechanical properties, thereby improving the puncture strength and breakdown voltage of the polypropylene product. On the other hand, a co-catalyst and an external electron donor are also added during the preparation process of the present invention, wherein the co-catalyst is triethyl aluminum, and the amount of the co-catalyst added accounts for 0.0018% to 0.0025% of the weight of the propylene; the external electron donor is cyclohexylmethyldimethoxysilane and / or dicyclopentyldimethoxysilane, and the weight ratio of the amount of the external electron donor to the co-catalyst is 1:1 to 3. By adding the above-mentioned co-catalyst, it can be more conducive to the activation of the catalyst, thereby meeting the technical effect of low ash content of the product. At the same time, the addition of an external electron donor can play a role in increasing the isotactic index of the product, so that the product can achieve the purpose of good pore-forming performance when processing lithium battery separators.

[0022] Finally, the material after the second polymerization reaction is sequentially steamed, dried and granulated to obtain a polypropylene product; wherein the temperature of the steaming treatment is 100° C. to 130° C., the time is 0.2 h to 0.5 h, the temperature of the drying treatment is 70° C. to 100° C., the time is 0.1 h to 0.3 h, and the steaming and drying treatment parameters are preferably within the above ranges, which can make the product have a lower volatile matter, so that it can better reduce the smoke emission during the polyolefin processing, thereby improving the processing environment during the preparation process.

[0023] In a preferred embodiment, the molar amount of hydrogen added to the first loop reactor is 0.007% to 0.012% of the propylene, and the molar amount of additional hydrogen added to the second loop reactor is 0.5% to 0.6% of the additional propylene, so as to further improve the puncture strength and breakdown voltage of the polypropylene.

[0024] In order to further improve the activity of the polymerization reaction and catalyze the polymerization reaction to proceed fully, the catalyst is preferably a titanium-based catalyst, the titanium-based catalyst is a Ziegler-Natta catalyst, the active component is titanium (Ti), and its model is HA catalyst and / or HA-R catalyst; the activity of the catalyst is 100,000 gPP / g catalyst to 200,000 gPP / g catalyst, thereby further improving the activity and stability of the catalyst.

[0025] In a preferred embodiment, in step S2, the weight ratio of the amount of additional propylene to the material after the first polymerization reaction is (0.5~1):1, so as to further improve the activity of the catalyst, improve the performance of polypropylene, and optimize the polymerization process.

[0026] In order to further improve the performance of the polypropylene product, the reaction temperature of the double loop reactor is preferably 67°C to 73°C, the reaction time is 1.5h to 3.0h, and the reaction pressure is 3.6MPa to 4.0MPa, so that the polypropylene product has a wider molecular weight distribution and has better processing performance at a low melt flow rate.

[0027] On the other hand, the present invention also provides a polypropylene, which is a polypropylene product prepared by the above-mentioned polypropylene preparation method. The polypropylene product has a melt flow rate of 0.2 g / 10 min to 0.4 g / 10 min, an isotacticity of 98.5% to 99.0%, an ash content of 0.0015% to 0.0030%, a molecular weight distribution index of 6 to 9, and a weight average molecular weight of 500,000 to 700,000.

[0028] On the other hand, the present invention also provides an application of polypropylene in the field of lithium battery separators, which is used to improve lithium battery separators and has the characteristics of high puncture strength and high breakdown voltage resistance, and can ultimately be applied to the batch preparation of lithium battery separators of 10 microns and below.

[0029] The present application is further described in detail below in conjunction with specific embodiments. These embodiments should not be construed as limiting the scope of protection claimed in the present application.

[0030] Example 1 Propylene, hydrogen, catalyst, co-catalyst and external electron donor are taken in the first loop reactor of the double loop reactor to carry out a first polymerization reaction to obtain a first polymerization reaction material, wherein the catalyst is a titanium catalyst, its model is HA catalyst, and its activity is 180000gPP / g catalyst, the co-catalyst is triethylaluminum, and its addition amount accounts for 0.0018% of the weight of propylene, and the external electron donor is cyclohexylmethyldimethoxysilane, and its weight ratio with the co-catalyst is 1:1. The first polymerization reaction material is taken, propylene and hydrogen are added, and a second polymerization reaction is carried out in the second loop reactor of the double loop reactor to obtain a second polymerization reaction material. Among them, the molar amount of hydrogen added in the first loop reactor accounts for 0.007% of propylene, and the amount of hydrogen added in the second loop reactor accounts for 0.6% of the added propylene. The weight ratio of the amount of added propylene to the material after the first polymerization reaction is 0.6:1, the reaction temperature of the double loop reactor is 70°C, the reaction time is 2h, the reaction pressure is 4MPa, and the material after the second polymerization reaction is steamed, dried and granulated in sequence, wherein the steaming temperature is 120°C, the time is 0.5h, the drying temperature is 90°C, and the time is 0.2h. The polypropylene product is obtained. The melt flow rate of the polypropylene is 0.3g / 10min, the isotacticity is 98.8%, the ash content is 0.002%, the molecular weight distribution index is 7.5, and the weight average molecular weight is 580,000.

[0031] Example 2 The only difference from Example 1 is that the catalyst activity is 120000 gPP / g catalyst, the cocatalyst is triethylaluminum, the amount of which is 0.0025% of the weight of propylene, the external electron donor is cyclohexylmethyldimethoxysilane, the weight ratio of which to the cocatalyst is 1:2, the amount of hydrogen added to the second loop reactor is 0.4% of the added propylene, the reaction pressure is 3.8 MPa, and a polypropylene product is obtained. The polypropylene has a melt flow rate of 0.2 g / 10 min, an isotacticity of 98.6%, an ash content of 0.0025%, a molecular weight distribution index of 6.5, and a weight average molecular weight of 650,000.

[0032] Example 3 The only difference from Example 1 is that the catalyst activity is 150000 gPP / g catalyst, the cocatalyst is triethylaluminum, the amount of which is 0.0025% of the weight of propylene, the external electron donor is cyclohexylmethyldimethoxysilane, the weight ratio of which to the cocatalyst is 1:3, the molar amount of hydrogen added in the first loop reactor is 0.015% of the weight of propylene, the molar amount of additional hydrogen added in the second loop reactor is 0.5% of the weight of additional propylene, the reaction temperature is 73°C, the reaction pressure is 4MPa, and a polypropylene product is obtained. The polypropylene has a melt flow rate of 0.3 g / 10min, an isotacticity of 98.5%, an ash content of 0.0025%, a molecular weight distribution index of 6.5, and a weight average molecular weight of 580,000.

[0033] Example 4 The only difference from Example 1 is that the catalyst activity is 100000 gPP / g catalyst, the cocatalyst is triethylaluminum, the amount of which is 0.0025% of the weight of propylene, the external electron donor is cyclohexylmethyldimethoxysilane, the weight ratio of which to the cocatalyst is 1:3, the molar amount of hydrogen added in the first loop reactor is 0.015% of the propylene, the molar amount of hydrogen added in the second loop reactor is 0.6% of the added propylene, the reaction temperature is 67°C, the reaction pressure is 4MPa, and a polypropylene product is obtained. The polypropylene has a melt flow rate of 0.4 g / 10min, an isotacticity of 98.5%, an ash content of 0.003%, a molecular weight distribution index of 7, and a weight average molecular weight of 500,000.

[0034] Example 5 The difference from Example 1 is that the cocatalyst used is triethylaluminum, the amount of which is 0.002% of the weight of propylene, and the external electron donor is dicyclopentyldimethoxysilane, the weight ratio of which to the cocatalyst is 1:2. The melt flow rate of the polypropylene is 0.3 g / 10 min, the isotacticity is 98.6%, the ash content is 0.0024%, the molecular weight distribution index is 7.5, and the weight average molecular weight is 580,000.

[0035] Comparative Example 1 The polypropylene product prepared by the conventional method is different from that of Example 1 only in that: a symmetrical hydrogenation method is adopted, the molar amount of hydrogen added in the first loop reactor is 0.032% of propylene, the molar amount of hydrogen added in the second loop reactor is 0.032% of propylene, the reaction temperature is 70°C, the reaction pressure is 3.4MPa, the catalyst activity is 100000gPP / gcatalyst, and the polypropylene product is obtained. The melt flow rate of the polypropylene is 1.0g / 10min, the isotacticity is 98.6%, the ash content is 0.003%, the molecular weight distribution index is 4, and the weight average molecular weight is 380,000.

[0036] Comparative Example 2 The only difference from Example 1 is that no external electron donor is added. The polypropylene has a melt flow rate of 0.3 g / 10 min, an isotacticity of 97.8%, an ash content of 0.002%, a molecular weight distribution index of 7.5, and a weight average molecular weight of 580,000.

[0037] Comparative Example 3 The only difference from Example 1 is that the weight ratio of the added amount of the external electron donor to the co-catalyst is 1:5. The polypropylene has a melt flow rate of 0.3 g / 10 min, an isotacticity of 98.1%, an ash content of 0.002%, a molecular weight distribution index of 7.5, and a weight average molecular weight of 580,000.

[0038] Comparative Example 4 The only difference from Example 1 is that the weight ratio of the added amount of the external electron donor to the co-catalyst is 1:0.5. The polypropylene has a melt flow rate of 0.3 g / 10 min, an isotacticity of 99.0%, an ash content of 0.003%, a molecular weight distribution index of 7.5, and a weight average molecular weight of 580,000.

[0039] Comparative Example 5 The only difference from Example 1 is that no co-catalyst is added. The polypropylene has a melt flow rate of 3.0 g / 10 min, an isotacticity of 98.8%, an ash content of 0.005%, a molecular weight distribution index of 7.5, and a weight average molecular weight of 300,000.

[0040] Comparative Example 6 The only difference from Example 1 is that the amount of the co-catalyst added is 0.005% of the weight of propylene. The melt flow rate of the polypropylene is 0.3 g / 10 min, the isotacticity is 98.8%, the ash content is 0.005%, the molecular weight distribution index is 7.5, and the weight average molecular weight is 580,000.

[0041] Comparative Example 7 The only difference from Example 1 is that during the post-polymerization treatment, the steaming temperature is 80°C and the time is 0.5 h. The polypropylene has a melt flow rate of 0.3 g / 10 min, an isotacticity of 98.8%, an ash content of 0.002%, a molecular weight distribution index of 7.5, and a weight average molecular weight of 580,000.

[0042] Comparative Example 8 The only difference from Example 1 is that during the post-polymerization treatment, the steaming temperature is 150°C and the time is 0.2h. The polypropylene has a melt flow rate of 0.3g / 10min, an isotacticity of 98.8%, an ash content of 0.002%, a molecular weight distribution index of 7.5, and a weight average molecular weight of 580,000.

[0043] Performance Testing (1) Puncture strength The test was conducted using a tensile testing machine, specifically including: using the polypropylene product prepared in the above-mentioned Examples 1 to 4 and Comparative Example 1, and preparing a lithium battery separator using a dry uniaxial stretching process (i.e., first stretching at low temperature to form defects such as silver streaks, and then pulling the defects apart at high temperature). Then, a scalpel was used to cut the lithium battery separator into strips with a width of about 10 cm in the transverse direction. The first test point was 5 cm from the edge. Three points were tested in the transverse direction of the separator. The test point positions were determined according to the film width to ensure that the distance between each test point was consistent. The puncture speed of the flat-head needle was 120 mm / min, the round-head needle speed was 50 mm / min, and the return needle speed was 200 mm / min.

[0044] (2) Breakdown voltage The test is performed using a withstand voltage tester, specifically including: selecting a flat film sample with a width of about 20 cm, placing it on the lower sheet, gently placing the upper sheet in the middle of the test sample, using the positive probe to contact the upper sheet, and pressing the start button to perform the test.

[0045] The polypropylene obtained in the above-mentioned embodiment and comparative example was used to prepare a lithium battery separator with a thickness of 10 μm using a dry single-drawing process, and the performance test was carried out. The test results are shown in Table 1.

[0046] Table 1 From the above description, it can be seen that the above embodiments of the present invention achieve the following technical effects: From the test results in Table 1 above, it can be found that when the melt flow rate of the product is lower, the isotacticity is higher, and the weight-average molecular weight is larger, the puncture strength of the prepared lithium battery separator is higher; when the melt flow rate of the product is lower, the isotacticity is higher, the ash content is lower, and the weight-average molecular weight is larger, the prepared lithium battery separator has a better breakdown voltage resistance.

[0047] Compared with the polypropylene obtained by the traditional method, when the polypropylene product obtained by the preparation method of the present invention is used to prepare a 10-micron lithium battery separator, the polypropylene obtained by the preparation method of the present invention has higher puncture strength and higher breakdown voltage, and its comprehensive performance is better.

[0048] Although this specification includes many specific implementation details, these should not be interpreted as limiting the scope of any invention or the scope of protection claimed, but are mainly used to describe the features of the specific embodiments of specific inventions. Certain features described in multiple embodiments in this specification may also be implemented in combination in a single embodiment. On the other hand, the various features described in a single embodiment may also be implemented separately in multiple embodiments or in any suitable sub-combination. In addition, although features may work in certain combinations as described above and even initially claim protection, one or more features from the claimed combination may be removed from the combination in some cases, and the claimed combination may point to a sub-combination or a variation of a sub-combination.

[0049] Thus, particular embodiments of the subject matter have been described. Other embodiments are within the scope of the following claims. In some cases, the actions recited in the claims can be performed in a different order and still achieve desirable results.

[0050] It should be noted that, in this article, relational terms such as "first" and "second" are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, the elements defined by the sentence "comprise a ..." do not exclude the existence of other identical elements in the process, method, article or device including the elements.

[0051] The above description is only a specific implementation of the present application, so that those skilled in the art can understand or implement the present application. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present application. Therefore, the present application will not be limited to the embodiments shown herein, but will conform to the widest range consistent with the principles and novel features applied for herein.

Claims

1. A method for preparing polypropylene, characterized in that: The preparation method comprises: Step S1, taking propylene, hydrogen, a catalyst, a co-catalyst and an external electron donor into a first loop reactor in a double loop reactor to carry out a first polymerization reaction to obtain a first polymerization reaction material; Step S2, taking the first polymerization reaction material, adding propylene and hydrogen, and carrying out a second polymerization reaction in the second loop reactor of the double loop reactor to obtain a second polymerization reaction material; Step S3, taking the material after the second polymerization reaction and then sequentially steaming, drying and granulating to obtain polypropylene; wherein, The double loop reactor comprises a first loop reactor and a second loop reactor, the molar amount of hydrogen added to the first loop reactor accounts for 0.007% to 0.015% of the propylene, and the molar amount of the additional hydrogen added to the second loop reactor accounts for 0.4% to 0.6% of the additional propylene; The co-catalyst is triethylaluminum, and the amount of the co-catalyst added is 0.0018% to 0.0025% of the weight of the propylene; the external electron donor is cyclohexylmethyldimethoxysilane and / or dicyclopentyldimethoxysilane, and the weight ratio of the amount of the external electron donor added to the co-catalyst is 1:1 to 3; In step S3, the temperature of the steaming treatment is 100-130° C., the time is 0.2-0.5 h, and the temperature of the drying treatment is 70-100° C., the time is 0.1-0.3 h.

2. The method for preparing polypropylene according to claim 1, characterized in that: The molar amount of hydrogen added to the first loop reactor is 0.007% to 0.012% of the propylene, and the molar amount of additional hydrogen added to the second loop reactor is 0.5% to 0.6% of the additional propylene.

3. The method for preparing polypropylene according to claim 1, characterized in that: In the step S2, the weight ratio of the additional propylene to the first polymerization reaction material is 0.5 to 1:

1.

4. The method for preparing polypropylene according to claim 1, characterized in that: The catalyst is a titanium-based catalyst, the model of the titanium-based catalyst is HA catalyst and / or HA-R catalyst, and the activity of the titanium-based catalyst is 100,000 gPP / g catalyst to 200,000 gPP / g catalyst.

5. The method for preparing polypropylene according to claim 1, characterized in that: The reaction temperature of the double loop reactor is 67° C. to 73° C., the reaction time is 1.5 h to 3.0 h, and the reaction pressure is 3.6 MPa to 4.0 MPa.

6. A polypropylene, characterized in that The polypropylene is a polypropylene obtained by the method for preparing polypropylene according to any one of claims 1 to 4.

7. The polypropylene according to claim 6, characterized in that The polypropylene has a melt flow rate of 0.2 g / 10 min to 0.4 g / 10 min, an isotacticity of 98.5% to 99.0%, an ash content of 0.0015% to 0.0030%, a molecular weight distribution index of 6 to 9, and a weight average molecular weight of 500,000 to 700,000.

8. Use of the polypropylene according to claim 6 or 7 in the field of lithium battery separators.

Citation Information

Patent Citations

  • Method for preparing polypropylene with high melt strength

    CN102134291A

  • Preparation method for propylene polymer and propylene polymer prepared by using same

    CN102453163A

  • Preparation method of polypropylene with high melt strength

    CN103788265A

  • Preparation method of high-melt-strength polypropylene

    CN106432569A

  • Material special for lithium battery diaphragm and preparation method thereof

    CN109306030A