Production method for converting bimodal metallocene polyethylene product into unimodal metallocene polyethylene product
By using CO2 inactivation and bed pretreatment agent without emptying the bed, the rapid conversion of bimodal metallocene polyethylene to unimodal metallocene polyethylene is achieved, and the long production time in the prior art is solved The problem of unqualified fisheye indicators has reduced production costs and equipment maintenance needs.
Patent Information
- Application Number
- CN202411489361.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-24
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-10-24
AI Technical Summary
In the prior art, the production of bimodal metallocene polyethylene and unimodal metallocene polyethylene requires discontinuous production conversion, resulting in long downtime of reactors, affecting benefits, and the single active center catalyst is sensitive to impurities, resulting in product fisheye index. Failed.
By stopping the injection of the dual-active center catalyst without emptying the bed, naturally deactivated, and deactivate the catalyst with CO2, and then injecting the bed pretreatment agent and the monoactive center catalyst, the gas phase component concentration is reestablished. Achieve rapid production of bimodal metallocene polyethylene to unimodal metallocene polyethylene, reduce reactor load, maintain reaction temperature and fluidization state, and ensure product quality.
The rapid switching between bimodal metallocene polyethylene to unimodal metallocene polyethylene is achieved, reducing production time and cost, ensuring that the fisheye index of unimodal metallocene polyethylene film materials is qualified, and there is no need to replace the seed bed, reducing the Equipment maintenance and modification costs.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of petrochemical industry, and specifically relates to a production method for converting a bimodal metallocene polyethylene product into a unimodal metallocene polyethylene product. Background Art
[0002] Metallocene polyethylene is a polyethylene resin polymerized by a catalyst consisting of a metallocene organic compound and a co-catalyst. It includes bimodal metallocene polyethylene and unimodal metallocene polyethylene. Bimodal metallocene polyethylene is prepared by a dual-active center catalyst and is mainly used to prepare pipes; unimodal metallocene polyethylene is prepared by a single-active center catalyst and is mainly used to prepare film materials. At present, foreign companies mainly use gas phase and loop slurry production processes. The comonomer is mostly 1-hexene, and some use 1-octene. The metallocene catalysts used are all independently developed, and the products have become serialized. Domestic mPE production companies mainly use gas phase production processes, and the comonomer is 1-hexene. The catalyst mainly uses Univation's metallocene catalyst, and a few companies use GRACE and New Plastic Chemical Metallocene TH-5 series catalysts.
[0003] For example, the BMC-200 bimodal catalyst used in Univation's Unipol gas-phase fluidized bed process is a PRODIGY bimodal catalyst series that can produce high-density polyethylene film and pipe resins with dual molecular weight distributions in a single reactor. The corresponding PE product is PE-100 grade pipe resin with a density of 0.947 to 0.951 g / cm 3 , which is widely used in water pipes, natural gas pipelines, large diameter pressure pipelines, etc. BMC-200 catalyst is a suspension with spherical particles in a mixture of mineral oil and isooctane, containing high MW-PE catalyst, low MW-PE catalyst and a common activator (methylaluminoxane or "MAO"). It must be transported and stored at low temperature (-10℃) to maintain stable performance.
[0004] As the market demand for metallocene products increases year by year, domestic enterprises have put forward new requirements for optimizing product production configuration. In order to use the same production equipment to prepare bimodal metallocene polyethylene and unimodal metallocene polyethylene, thereby avoiding the need to purchase production equipment again and saving production costs, the production equipment is generally treated after the production of bimodal metallocene polyethylene series products is completed, and unimodal metallocene polyethylene is produced instead. However, the single-active center metallocene catalyst is a homogeneous catalyst system composed of methylaluminoxane (MAO) and metallocene catalyst Cp2MCl2 (M=Ti, Zr, Hf), which has a single active center and extremely high catalytic activity. It is sensitive to impurity components in the raw materials, and also has large differences in response to hydrogen and comonomers. At present, the conversion between bimodal metallocene polyethylene series products (used to prepare pipes) and unimodal metallocene polyethylene products (used to prepare film materials) adopts a discontinuous conversion method. The reactor is emptied and overhauled before being reconnected to the bed and started again. The shutdown time is about 5 days, which is a long time and no product is produced during the period, affecting the benefits. Summary of the invention
[0005] In view of this, the present invention provides a production method for converting a bimodal metallocene polyethylene product into a unimodal metallocene polyethylene product, so as to directly convert a bimodal metallocene polyethylene series product into a unimodal metallocene polyethylene product without emptying the bed layer, and at the same time reduce the crystal point of the unimodal metallocene polyethylene, so as to ensure that the fisheye index of the unimodal metallocene polyethylene film material product is qualified.
[0006] In a first aspect, the present invention provides a method for converting a bimodal metallocene polyethylene product into a unimodal metallocene polyethylene product, comprising the following steps: 1) Before stopping the injection of the dual-active-site catalyst, stop feeding the induced condensing agent and the recovered liquid; heat the reaction system to raise the temperature, inject a bed pretreatment agent, make the content of the bed pretreatment agent reach 50ppm to 80ppm of the reactor production load, and reduce the reaction heat load to 0 t / h, wherein the bed pretreatment agent includes an antistatic agent, and the antistatic agent includes at least one of CA-200 and CA-300; 2) Stop injecting the dual-active-center catalyst to allow the dual-active-center catalyst to deactivate naturally; inject CO2 when exiting the condensed state; 3) Stop injecting gas phase components, reduce the discharge frequency of the reactor discharge system, and maintain the reactor bed weight to the quality required for the start-up of unimodal metallocene polyethylene; 4) Heating the reaction system to a reaction temperature of a unimodal metallocene polyethylene product; maintaining the reaction temperature, pressure and fluidization state of the reaction system, and replacing the reaction system with nitrogen; then maintaining the reaction temperature of the reaction system, and replacing the reaction system with ethylene; 5) Pretreating the bed powder in the reaction system with a bed pretreatment agent, wherein the bed pretreatment agent includes an antistatic agent, and the antistatic agent includes at least one of CA-300 and CA-200, and the injection amount of the bed pretreatment agent is 15 ppm to 25 ppm of the bed weight, and the bed pretreatment agent is injected and circulated in the fluidized state of the reaction system for 1 h to 2 h; 6) Re-establish the gas phase component concentration according to the initiation conditions of the single-active-center metallocene catalyst; inject the single-active-center metallocene catalyst to initiate the reaction and convert to the production of a single-peak metallocene polyethylene product.
[0007] In the above production method, in step 1), the dual-active center catalyst includes a BMC-200 catalyst.
[0008] In the present invention, the type of the dual-active-center catalyst is not specifically limited, and those skilled in the art may use a conventional dual-active-center catalyst in the art, for example, a BMC-200 catalyst.
[0009] BMC-200 catalyst is a suspension with spherical particles in a mixture of mineral oil and isooctane, containing high MW-PE catalyst, low MW-PE catalyst and a common activator (methylaluminoxane or "MAO"), which must be transported and stored at low temperature (-10°C) to maintain stable performance. In order to make the polyethylene product have a wide / bimodal molecular weight distribution, it is usually necessary to add a molecular weight regulator Trim, which is a newly added LWM-PE catalyst solution. During production operation, it is mixed online with the BMC-200 catalyst to control the polymer flow index (FI).
[0010] In the above production method, in step 1), before stopping the injection of the dual-active site catalyst, the feeding of the induced condensing agent (ICA) and the recovery liquid is stopped to reduce the concentration of the induced condensing agent in the system to 50% to 80% of the original concentration.
[0011] In the above production method, in step 1), the induced condensing agent includes at least one of isopentane, hexane and isobutane.
[0012] In the above production method, in step 1), the recovery liquid is a liquid formed by condensing some residual components or unreacted components in the reactor outside the reactor through condensation technology. The recovery liquid is transported into the reactor for recycling and used to remove the reaction heat generated by the reaction system. The recovery liquid generally includes C6 organic matter, C8 organic matter and isopentane.
[0013] In the present invention, after the injection of the dual-active-center catalyst is stopped, the catalyst will be slowly consumed during the reaction process, thereby reducing the load of the reaction system. In the process of reducing the reaction load, the heat of reaction will gradually decrease, and thus, there is no need for too much condensing agent to remove the heat of reaction generated by the reaction system. Therefore, before stopping the injection of the dual-active-center catalyst, the present invention reduces the condensing agent content in the reactor to make the reaction system exit the condensed state, avoiding too much condensing agent causing the temperature of the reaction system to be too low, causing the condensing agent to be in a liquid state in the reaction system and mixed in the powder in the reactor, causing the powder to become sticky, and easily form flakes and lumps to block the reactor.
[0014] In the above production method, in step 1), the reaction system is heated to 100°C to 110°C.
[0015] In the above production method, in step 1), the heating to raise the temperature of the reaction system comprises the following steps: The start-up heater was put into use, and the steam control valve was adjusted according to the polymerization reaction temperature of the bimodal metallocene polyethylene product. Preheating was performed in advance to prevent a sharp drop in the temperature of the reaction system after the deactivation of the dual-active center catalyst.
[0016] In the present invention, the bed pretreatment agent is injected and the injection amount of the bed pretreatment agent is increased to 50 ppm to 80 ppm to ensure that the electrostatic stability and wall temperature of the reactor are stable, and the injection is maintained until the reaction heat load drops to 0 t / h.
[0017] In the above production method, in the step 2), exiting the condensed state means injecting CO2 after the condensation rate of the reaction system reaches 3% to 5%, and exiting the condensed state.
[0018] In the above production method, in the step 2), when the condensation rate is 3% to 5%, CO2 is injected to a concentration less than 2 ppm, and then CO2 is injected again to a concentration of 3 ppm to 8 ppm.
[0019] In the present invention, the dual-active-center catalyst can be a conventional catalyst in the art, such as a BMC-200 bimodal catalyst. The reaction of the bimodal metallocene polyethylene catalyzed by the catalyst is very rapid (i.e., the BMC-200 bimodal catalyst has the characteristic of rapid catalyst activity), and it is necessary to avoid the problem of agglomeration and flake formation in the reactor caused by too intense reaction. Therefore, in the present invention, when exiting the condensed state, CO2 is used to immediately deactivate the dual-active-center catalyst.
[0020] In the above production method, in step 2), when the condensation rate is 3% to 5%, open the angle valve of the CO2 cylinder and inject CO2 for 5 to 15 seconds to make the CO2 concentration less than 2 ppm; inject CO2 again for 5 to 10 seconds to ensure that the CO2 concentration is between 3 ppm and 8 ppm.
[0021] In the present invention, the injection of the dual-active center catalyst is stopped to allow the dual-active center catalyst to deactivate naturally, and then the condensation rate of the reactor is paid attention to. When the condensation rate is 3% to 5%, the angle valve of the CO2 cylinder is opened to inject CO2 for 5 to 15 seconds to make the CO2 concentration less than 2 ppm, so that the dual-active center catalyst can be quickly deactivated at a low condensation rate; CO2 is injected again for 5 to 10 seconds to ensure that the CO2 concentration is between 3 ppm and 8 ppm, so that the residual dual-active center catalyst is completely deactivated and quickly exits the condensed state, thereby achieving the condition that the original dual-active center catalyst in the reaction system is deactivated, and the CO2 concentration in the system is guaranteed to be the lowest, so that the CO2 can be replaced cleanly later.
[0022] In the above production method, in the step 3), the injection of the gas phase component is stopped, the discharge frequency of the reactor discharge system is reduced, the reactor bed weight is maintained to the required quality for the start-up of unimodal metallocene polyethylene, and the circulating gas flow rate is maintained at 0.6 m / s to 0.8 m / s, and the material level in the expansion section is maintained at 35% to 60%.
[0023] In the present invention, the circulating gas flow rate is maintained at 0.6 m / s to 0.8 m / s, and the material level in the expanded section is maintained at 35% to 60%, so that the powder in the reaction system is in a fluidized state to avoid the occurrence of skinning and agglomeration that may be caused by the powder falling on the bed.
[0024] In the above production method, in the step 3), the gas phase components include ethylene, hydrogen and comonomers.
[0025] In the above production method, in the step 3), the required start-up mass of the unimodal metallocene polyethylene is 110 t to 150 t.
[0026] In the present invention, the injection of the dual-active center catalyst is stopped, and when the condensation rate of the reactor is 3% to 5%, CO2 is injected to deactivate the dual-active center catalyst in the reaction system; during this process, when the polymerization reaction in the reactor no longer occurs (determined by the bottom temperature of the reactor), the injection of gas phase components such as ethylene, hydrogen, and comonomers is stopped, the discharge frequency of the reactor discharge system is reduced, and the reactor bed weight is maintained to the required mass of 110 t to 150 t for the start-up of single-peak metallocene polyethylene to meet the conditions for single-peak metallocene initiation; at the same time, the circulating gas velocity is maintained at 0.6 m / s to 0.8 m / s, and the material level of the expansion section is maintained at 35% to 60%.
[0027] In the above production method, in the step 4), the reaction temperature of the unimodal metallocene polyethylene product is 80°C to 90°C.
[0028] In the above production method, in step 4), the steam control valve of the start-up heater is adjusted to maintain the reaction temperature of the reaction system at 80° C. to 90° C., in preparation for the single active site catalyst to initiate the reaction.
[0029] In the above production method, in step 4), the reaction system is replaced with nitrogen to terminate the polymerization reaction of the bimodal metallocene series products and reduce the reaction pressure, with the lowest pressure being the one in which no surging of the compressor occurs.
[0030] In step 4) of the present invention, under the conditions of maintaining the reaction temperature, pressure and fluidized state of the reaction system, each purge main pipe in the reaction system is switched from ethylene to HPPN (high pressure purified nitrogen) to completely deactivate the original dual active center catalyst components in the bed, thereby preparing for the replacement, pretreatment and subsequent initiation conditions of the single peak metallocene catalyst.
[0031] In the above production method, in step 4), the reaction system is replaced by ethylene using a pressure increase / decrease method.
[0032] In the above production method, in step 4), the displacement pressure of the pressure rise and fall method is 900 kPa to 1100 kPa to 1400 kPa, that is, the displacement pressure is increased from 900 kPa to 1100 kPa, then increased to 1400 kPa, and then decreased back to 900 kPa, and the above process is repeated.
[0033] In the above production method, in step 4), ethylene is used to replace the reaction system to replace the materials (for example, CO2 and N2) in the reactor used to deactivate the dual-active center catalyst. The replacement completion standard is: CO2 in the reactor is less than 5ppm.
[0034] In the present invention, in the step 4), the reaction temperature is maintained in the reactor, the purge main pipe is switched back to ethylene from HPPN, the amount of ethylene entering the purge main pipe is increased, and the material used for the dual-active center catalytic polymerization reaction in the reactor is replaced by the pressure increase and decrease method, and the replacement pressure is 900kPa to 1100kPa to 1400kPa (the replacement pressure is increased from 900kPa to 1100kPa, then increased to 1400kPa, and then reduced back to 900kPa, and the above process is repeated), and the replacement standard is CO2 in the reactor <5 ppm (at this time, the dual-active center catalyst has been deactivated). Under this condition, the material used for the dual-active center catalytic polymerization reaction has been completely replaced in the reaction system, and the residual CO2 in the reactor <5 ppm will not deactivate the newly injected catalyst subsequently.
[0035] In the present invention, a bed pretreatment agent is used to pretreat the bed powder in the reactor. Specifically, CA-300 and / or CA-200 are selected as the bed pretreatment agent to completely eliminate the influence of the metallocene catalyst residual poison on the metallocene catalyst to prevent flakes from occurring in the reactor.
[0036] In the above production method, in step 6), re-establishing the gas phase component concentration includes: establishing ethylene concentration and nitrogen concentration.
[0037] In the above production method, in step 6), after the gas phase components are established, a single active site metallocene catalyst is injected to initiate the reaction, and heat load can be seen in 20 minutes (ie, the reaction has been initiated).
[0038] In the above production method, in step 6), the single-active-site metallocene catalyst includes an easily processable metallocene catalyst (eg, EZ series metallocene catalyst).
[0039] In the above production method, the total switching time for converting the bimodal metallocene polyethylene product to the unimodal metallocene polyethylene product is 22 h to 24 h.
[0040] In the above production method, the melt index of the bimodal metallocene polyethylene product is 5 g·10 min -1 Up to 7g·10 min -1 , density is 0.947 g / cm 3 Up to 0.951 g / cm 3 .
[0041] In the present invention, the bimodal metallocene polyethylene product belongs to high-density polyethylene (HDPE), which is prepared by using a conventional dual-active center catalyst in the art.
[0042] In the above production method, the melt index of the unimodal metallocene polyethylene product is 0.2 g / 10 min to 20 g / 10 min, and the density is 0.910 g / cm 3 Up to 0.940 g / cm 3 .
[0043] In the present invention, since the dual-active-center catalyst has the characteristic of rapid manifestation of catalytic activity, in the process of converting the bimodal metallocene polyethylene product to the unimodal metallocene polyethylene product, the conversion process cannot directly make the reaction system exit the condensed state like the titanium or chromium catalysts, and the dual-active-center catalyst must be immediately deactivated and then exit the condensed state. In addition, during the conversion process, the reaction system cannot be converted from the condensed state to the dry state. If the production of the bimodal metallocene polyethylene is converted to the dry state for a period of time, the reactor is prone to agglomeration, which causes the powder in the reactor to be unable to continue to be used as a seed bed for the start of the unimodal metallocene production.
[0044] Therefore, the present invention adopts the method of first stopping the feeding of induced condensing agent (ICA) and recycling liquid to reduce the concentration of induced condensing agent in the system to 50% to 80% of the original concentration, and heating the reaction system to make the temperature of the reaction system reach 100°C to 110°C without directly exiting the condensed state, so that the remaining dual-active center catalyst reacts quickly and is completely consumed, and at the same time injecting a bed pretreatment agent to avoid agglomeration of the polymerization product. Then, the injection of the dual-active center catalyst is stopped, and the dual-active center catalyst is immediately deactivated by using CO2 to ensure that the reactor in the bimodal metallocene production process can continue to serve as a seed bed for the start-up of the single-modal metallocene.
[0045] In the prior art, the conversion between bimodal metallocene polyethylene series products (used to prepare pipes) and unimodal metallocene polyethylene products (used to prepare film materials) is carried out in a discontinuous conversion mode, and the reactor is emptied and repaired before being reconnected and put into operation. In the production process of metallocene polyethylene products, metallocene polyethylene is used as a seed bed to start production. Considering the compatibility between the metallocene polyethylene powder (mLLDPE) in the seed bed and the metallocene polyethylene product prepared by initiating a single-active center metallocene catalyst, the conventional method generally uses a high-strength metallocene catalyst HP series as a single-active center metallocene catalyst to initiate polymerization to achieve the conversion of unimodal metallocene polyethylene, so that the fisheye index of the polyethylene film material product produced by using the unimodal metallocene polyethylene product obtained as a raw material is qualified.
[0046] In the present invention, the bimodal metallocene polyethylene series products (belonging to HDPE) are directly converted to unimodal metallocene polyethylene products without emptying the bed layer, wherein the seed bed for converting the unimodal metallocene polyethylene is the powder remaining in the reactor after the bimodal metallocene polyethylene product is completed (that is, the powder is HDPE), which is incompatible with conventional unimodal metallocene polyethylene (LLDPE). Therefore, under the premise of not having an empty bed layer of powder, directly using the technical solution in the prior art to convert the bimodal metallocene polyethylene series products into unimodal metallocene polyethylene products is likely to result in the fisheye index of the polyethylene film material product finally obtained from the conversion being unqualified. In order to make the fish-eye index of the polyethylene film material product qualified, the present invention adopts an easy-to-process metallocene catalyst (for example, EZ series) instead of the conventional high-strength metallocene catalyst HP series when converting to a unimodal metallocene polyethylene product. The unimodal metallocene polyethylene product obtained by initiating polymerization thereof can be well mixed with the powder in the seed bed used for the conversion of the unimodal metallocene polyethylene in the present invention, thereby reducing the crystal point of the unimodal metallocene polyethylene and ensuring that the fish-eye index of the unimodal metallocene polyethylene film material product is qualified.
[0047] In the above production method, the unimodal metallocene polyethylene produced has the following properties: tensile strength ≥11 MPa, dart impact damage mass ≥300 g, 0.8 mm fisheye number <6 / 1520cm 2 , 0.4 mm fisheye number <15 / 1520cm 2 .
[0048] In the present invention, when the fisheye level of the unimodal metallocene polyethylene product reaches 0.8 mm, the number of fisheyes is less than 6 / 1520cm 2 , 0.4 mm fisheye number <15 / 1520cm 2 After meeting this standard, the quality of this unimodal metallocene polyethylene product is comparable to that of similar foreign products.
[0049] Compared with the prior art, the technical solution of the present invention has the following beneficial technical effects: (1) The switching method for converting a bimodal metallocene polyethylene product to a unimodal metallocene polyethylene product provided by the present invention takes a short time, which is shortened from 120 hours in the traditional method to within 24 hours, effectively reducing the time cost and realizing the rapid switching from a bimodal metallocene polyethylene product to a unimodal metallocene polyethylene product; (2) The switching method for converting a bimodal metallocene polyethylene product to a unimodal metallocene polyethylene product provided by the present invention does not require a complete shutdown of the reaction, opening of the reactor, or purchase of metallocene polyethylene powder as a seed bed. Instead, the switching is achieved in a dual-active-center catalyst bed, which greatly reduces the difficulty of metallocene polyethylene development and production. (3) The switching method for converting a bimodal metallocene polyethylene product to a unimodal metallocene polyethylene product provided by the present invention does not require large-scale transformation of existing raw material storage tanks, seed bins, refining systems, catalyst filling systems, raw material feed control systems, and electrostatic control systems, thereby greatly reducing the cost of transformation investment; (4) Using the switching method of the bimodal series products provided by the present invention to produce unimodal metallocene products, the produced metallocene polyethylene has the following properties: melt index range 0.2 g / 10 min to 20 g / 10 min, density range 0.910 g / cm 3 Up to 0.940 g / cm 3 , tensile strength ≥11 MPa, dart impact damage mass ≥300 g, fisheye (0.8 mm) <6 / 1520cm 2 ,Fisheye (0.4 mm) < 15 / 1520 cm 2 . DETAILED DESCRIPTION
[0050] In order to make the purpose, technical scheme and advantages of the embodiments of the present application clearer, the technical scheme in the embodiments of the present application is clearly and completely described below. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.
[0051] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in this application can be purchased from the market or prepared by existing methods.
[0052] In the prior art, the conversion between bimodal metallocene polyethylene series products (used to prepare pipes) and unimodal metallocene polyethylene products (used to prepare film materials) is carried out in a discontinuous conversion mode. The reactor is emptied and repaired before being reconnected to the bed and restarted. The shutdown time is about 5 days, which is a long time and no product is produced during the period, affecting the efficiency. The present invention provides a production method for converting bimodal metallocene polyethylene products to unimodal metallocene polyethylene products, so that the bimodal metallocene polyethylene series products can be directly converted to unimodal metallocene polyethylene products without emptying the bed layer, and the crystal point of the unimodal metallocene polyethylene is reduced at the same time, ensuring that the fisheye index of the unimodal metallocene polyethylene film material product is qualified.
[0053] However, since the dual-active-site catalyst and the single-active-site metallocene catalyst are incompatible, before injecting the single-active-site metallocene catalyst, the dual-active-site catalyst needs to be completely consumed or deactivated before the conversion to the single-peak metallocene polyethylene product can be carried out.
[0054] Some embodiments of the present invention provide a method for converting a bimodal metallocene polyethylene product into a unimodal metallocene polyethylene product, comprising the following steps: S1: Before stopping the injection of the dual-active-center catalyst, stop feeding the induced condensing agent and the recovered liquid; heat the reaction system to raise its temperature, and inject a bed pretreatment agent to reduce the reaction heat load; S2: stop injecting the dual-active-center catalyst to allow the dual-active-center catalyst to deactivate naturally; inject CO2 when exiting the condensed state; S3: Stop injecting gas phase components, reduce the discharge frequency of the reactor discharge system, and maintain the reactor bed weight to the required quality for the start-up of unimodal metallocene polyethylene; S4: heating the reaction system to a reaction temperature of a unimodal metallocene polyethylene product; maintaining the reaction temperature, pressure and fluidization state of the reaction system, and replacing the reaction system with nitrogen; then maintaining the reaction temperature of the reaction system, and replacing the reaction system with ethylene; S5: pretreating the bed powder in the reaction system with a bed pretreatment agent; S6: Re-establish the gas phase component concentration according to the initiation conditions of the single-active-site metallocene catalyst; inject the single-active-site metallocene catalyst to initiate the reaction to convert the production of a single-peak metallocene polyethylene product.
[0055] In some embodiments, in step S1, the dual-active site catalyst includes a BMC-200 catalyst.
[0056] In some embodiments, in step S1, before stopping the injection of the dual-active site catalyst, the feeding of the induced condensing agent and the recovery liquid is stopped to (rapidly) reduce the concentration of the induced condensing agent in the system to 50% to 80% (e.g., 55%, 60%, 65%, 70% or 75%) of the original concentration.
[0057] In some embodiments, in step S1, the induced condensing agent includes at least one of isopentane, hexane and isobutane.
[0058] In some embodiments, in step S1, the recovery liquid is a liquid formed by condensing some residual components or unreacted components in the reactor outside the reactor through condensation technology. The recovery liquid is transported into the reactor for recycling and is used to remove the heat of reaction generated by the reaction system. The recovery liquid generally includes C6 organic matter, C8 organic matter and isopentane, etc.
[0059] In the present invention, after the injection of the dual-active-center catalyst is stopped, the catalyst will be slowly consumed during the reaction process, thereby reducing the load of the reaction system. In the process of reducing the reaction load, the heat of reaction will gradually decrease, and thus, there is no need for too much condensing agent to remove the heat of reaction generated by the reaction system. Therefore, before stopping the injection of the dual-active-center catalyst, the present invention reduces the condensing agent content in the reactor to make the reaction system exit the condensed state, avoiding too much condensing agent causing the temperature of the reaction system to be too low, causing the condensing agent to be in a liquid state in the reaction system and mixed in the powder in the reactor, causing the powder to become sticky, and easily form flakes and lumps to block the reactor.
[0060] In some embodiments, in step S1, heating the reaction system to 100° C. to 110° C. specifically comprises the following steps: Put the start-up heater into use, adjust the steam control valve according to the polymerization temperature of the bimodal metallocene polyethylene product, and control the reaction temperature at 100°C to 110°C (for example, 102°C, 105°C or 108°C) by controlling the steam flow rate to preheat the reaction system in advance and prevent the temperature of the reaction system from dropping sharply after the dual-active center catalyst is deactivated.
[0061] In some embodiments, in step S1, the bed pretreatment agent is injected so that the content of the bed pretreatment agent reaches 50 ppm to 80 ppm (eg, 55 ppm, 60 ppm, 65 ppm, 70 ppm or 75 ppm) of the production load of the reactor (or reaction system).
[0062] In the present invention, the bed pretreatment agent is injected and the injection amount of the bed pretreatment agent is increased to 50 ppm to 80 ppm to ensure that the electrostatic stability and wall temperature of the reactor are stable, and the injection is maintained until the reaction heat load drops to 0 t / h.
[0063] In some embodiments, in step S1, the bed pretreatment agent includes an antistatic agent, and the antistatic agent includes at least one of CA-200 and CA-300.
[0064] Bed pretreatment agents CA-200 and CA-300 are common antistatic agents in the field. The main components of CA-200 are aluminum stearate, oil-soluble alkyl alcohol amine and mineral oil solvent, with a ratio of 10% to 30%: 15% to 25%: 65% to 90%; the main components of CA-300 are aluminum stearate, oil-soluble alkanolamide, mineral oil solvent, stearate, with a ratio of 10% to 30%: 15% to 25%: 65% to 90%: 1% to 3%.
[0065] In some embodiments, in step S2, exiting the condensed state means injecting CO2 to exit the condensed state after the condensation rate of the reaction system is 3% to 5%; when the condensation rate is 3% to 5% (for example, 3.5%, 4%, 4.5% or 4.8%), injecting CO2 to make its concentration less than 2 ppm, and then injecting CO2 again to make its concentration 3 ppm to 8 ppm (for example, 3.5 ppm, 4 ppm, 5 ppm, 6 ppm, 6.5 ppm or 7.5 ppm).
[0066] In the present invention, the dual-active-center catalyst can be a conventional catalyst in the art, such as a BMC-200 bimodal catalyst. The reaction of the bimodal metallocene polyethylene catalyzed by the catalyst is very rapid (i.e., the BMC-200 bimodal catalyst has the characteristic of rapid manifestation of catalyst activity), and it is necessary to avoid the problem of agglomeration and flake formation in the reactor due to excessively violent reaction. Therefore, in the present invention, when exiting the condensed state (i.e., when the condensation rate is 3% to 5%), CO2 is used to immediately deactivate the dual-active-center catalyst.
[0067] In some embodiments, in step S2, when the condensation rate is 3% to 5%, the angle valve of the CO2 cylinder is opened to inject CO2 for 5 seconds to 15 seconds (for example, 6 seconds, 8 seconds, 10 seconds or 12 seconds) to make the CO2 concentration less than 2 ppm, and CO2 is injected again for 5 seconds to 10 seconds (for example, 6 seconds, 7 seconds, 8 seconds or 9 seconds) to ensure that the CO2 concentration is 3 ppm to 8 ppm.
[0068] In the present invention, the injection of the dual-active center catalyst is stopped to allow the dual-active center catalyst to deactivate naturally, and then the condensation rate of the reactor is paid attention to. When the condensation rate is 3% to 5%, the angle valve of the CO2 cylinder is opened to inject CO2 for 5 to 15 seconds, and the CO2 concentration is less than 2ppm, so that the dual-active center catalyst is quickly deactivated at a low condensation rate (or when exiting the condensation state); CO2 is injected again for 5 to 10 seconds to ensure that the CO2 concentration is 3 ppm to 8 ppm, so that the residual dual-active center catalyst is completely deactivated, thereby achieving the condition that the original dual-active center catalyst in the reaction system is deactivated, and the CO2 concentration in the system is guaranteed to be the lowest, so as to facilitate the subsequent replacement of CO2.
[0069] In some embodiments, in step S3, the injection of gas phase components is stopped, the discharge frequency of the reactor discharge system is reduced, the reactor bed weight is maintained to the required mass for the start-up of unimodal metallocene polyethylene, and the circulating gas flow rate is maintained at 0.6 m / s to 0.8 m / s (for example, 0.65 m / s, 0.7 m / s or 0.75 m / s), and the material level in the expansion section is maintained at 35% to 60% (for example, 42%, 45% or 48%).
[0070] In some embodiments, in step S3, the gas phase components include ethylene, hydrogen and comonomers.
[0071] In some embodiments, in step S3, the required start-up mass of the unimodal metallocene polyethylene is 110 t to 150 t (e.g., 115 t, 120 t, 125 t, 130 t, 135 t, 140 t or 145 t).
[0072] In the present invention, the injection of the dual-active center catalyst is stopped, and when the condensation rate of the reactor is 3% to 5%, CO2 is injected to deactivate the dual-active center catalyst in the reaction system; during this process, when the polymerization reaction in the reactor no longer occurs (judged according to the bottom temperature of the reactor), the injection of gas phase components such as ethylene, hydrogen, and comonomers is stopped, the discharge frequency of the reactor discharge system is reduced, and the reactor bed weight is maintained to the required mass of 110 t to 150 t for the start-up of single-peak metallocene polyethylene to meet the conditions for single-peak metallocene initiation; at the same time, the circulating gas velocity is maintained at 0.6 m / s to 0.8 m / s, and the material level of the expanded section is maintained at 35% to 60%, so that the powder in the bed is in a fluidized state and does not fall on the bed to form sheets and lumps.
[0073] In some embodiments, the reaction temperature of the unimodal metallocene polyethylene product in step S4 is 80°C to 90°C (for example, 82°C, 85°C or 88°C); specifically, in step 4), the steam control valve of the start-up heater is adjusted to maintain the reaction temperature of the reaction system at 80°C to 90°C, in preparation for the single active site catalyst to initiate the reaction.
[0074] In some embodiments, in step S4, the reaction system is replaced with nitrogen to terminate the polymerization reaction of the bimodal metallocene series products, and the reaction pressure is reduced to the lowest pressure when no surge occurs in the compressor.
[0075] In step 4) of the present invention, under the conditions of maintaining the reaction temperature, pressure and fluidized state of the reaction system, each purge main pipe in the reaction system is switched from ethylene to HPPN (high pressure purified nitrogen) to completely deactivate the original dual active center catalyst components in the bed, thereby preparing for the replacement, pretreatment and subsequent initiation conditions of the single peak metallocene catalyst.
[0076] In some embodiments, in step S4, the reaction system is replaced by ethylene using a pressure increase / decrease method; the replacement pressure of the pressure increase / decrease method is 900 kPa to 1100 kPa to 1400 kPa (the replacement pressure is increased from 900 kPa to 1100 kPa, then increased to 1400 kPa, and then decreased back to 900 kPa, and the above process is repeated).
[0077] In some embodiments, in step S4, ethylene is used to replace the reaction system to replace the materials (eg, CO2 and N2) in the reactor used to deactivate the dual-active site catalyst, and the replacement completion standard is: CO2 in the reactor <5ppm.
[0078] In the present invention, in step S4, the reaction temperature is maintained in the reactor, the purge main pipe is switched back to ethylene from HPPN, the amount of ethylene entering the purge main pipe is increased, and the material used for the dual-active center catalytic polymerization reaction in the reactor is replaced by the pressure increase and decrease method, and the replacement pressure is 900kPa to 1100kPa to 1400kPa (the replacement pressure is increased from 900kPa to 1100kPa, then increased to 1400kPa, and then reduced back to 900kPa, and the above process is repeated), and the replacement standard is CO2 in the reactor <5 ppm (at this time, the dual-active center catalyst has been deactivated). Under this condition, the material used for the dual-active center catalytic polymerization reaction has been completely replaced in the reaction system, and the residual CO2 in the reactor <5 ppm will not deactivate the newly injected catalyst subsequently.
[0079] In some embodiments, in step S5, the bed pretreatment agent includes an antistatic agent, and the antistatic agent includes at least one of CA-300 and CA-200; the injection amount of the bed pretreatment agent is 15 ppm to 25 ppm (for example, 18 ppm, 20 ppm, 22 ppm or 24 ppm) of the bed weight; the bed pretreatment agent is injected and circulated in the fluidized state of the reaction system for 1 h to 2 h (for example, 1.5 h).
[0080] In some embodiments, in step S6, re-establishing the gas phase component concentration includes: establishing ethylene concentration and nitrogen concentration; after the gas phase components are established, injecting a single active site metallocene catalyst to initiate the reaction, and heat load can be seen in 20 minutes (ie, the reaction has been initiated).
[0081] In some embodiments, in step S6, the single-active site metallocene catalyst includes an easily processable metallocene catalyst (eg, an EZ series metallocene catalyst).
[0082] In some embodiments, the total switching time for converting the bimodal metallocene polyethylene product to the unimodal metallocene polyethylene product is 22 h to 24 h (eg, 22.5 h, 23 h, or 23.5 h).
[0083] In some embodiments, the produced unimodal metallocene polyethylene has the following properties: melt index range 0.2 g / 10 min to 20 g / 10 min, density range 0.910 g / cm 3Up to 0.940 g / cm 3 , tensile strength ≥11 MPa, dart impact damage mass ≥300 g, number of 0.8 mm fisheyes <6 / 1520 cm 2 , 0.4 mm fisheye number <15 / 1520cm 2 .
[0084] In the present invention, when the fisheye level of the unimodal metallocene polyethylene product reaches 0.8 mm, the number of fisheyes is less than 6 / 1520cm 2 , 0.4 mm fisheye number <15 / 1520cm 2 After meeting this standard, the quality of this unimodal metallocene polyethylene product is comparable to that of similar foreign products.
[0085] The present application will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are intended only to illustrate the present application and are not intended to limit the scope of the present application. The experimental methods for which specific conditions are not specified in the following examples are usually measured according to national standards. If there is no corresponding national standard, then the conditions recommended by the manufacturer are followed.
[0086] Example 1 A method for converting a bimodal metallocene polyethylene product into a unimodal metallocene polyethylene product comprises the following steps: S1: Before stopping the injection of the dual-active center catalyst, stop feeding fresh isopentane (i.e., ICA) and recycled liquid, and quickly reduce the ICA concentration in the system to 60% of the original concentration; put the start-up heater into use, adjust the steam control valve according to the reaction temperature, and control the reaction temperature to 100°C to 110°C by controlling the steam flow rate to preheat the reaction system in advance to prevent a sharp drop in temperature after the dual-active center catalyst is deactivated; increase the injection amount of the bed pretreatment agent to 60 ppm to ensure the stability of the reactor's electrostatic and wall temperature, and maintain injection until the reaction heat load drops to 0 t / h.
[0087] S2: Stop injecting the dual-active center catalyst to allow it to deactivate naturally. Pay attention to the condensation rate of the reactor. When the condensation rate is close to 5%, open the angle valve of the CO2 cylinder and inject CO2 for 10 seconds. If the CO2 concentration is less than 2 ppm, inject CO2 again for 5 seconds to ensure that the CO2 concentration is between 3 ppm and 8 ppm.
[0088] S3: When the polymerization reaction no longer occurs, stop injecting gas phase components such as ethylene, hydrogen, and comonomers, reduce the discharge frequency of the reactor discharge system, maintain the reactor bed weight to the metallocene start-up requirement of 110 t, while maintaining the circulating gas velocity at 0.7 m / s and the material level in the expansion section at 40% to 50%.
[0089] S4: Adjust the steam control valve of the start-up heater to make the reactor temperature 80℃ to 90℃; maintain the reaction temperature, pressure and fluidization state in the reactor, and cut the purge mains in the reactor from ethylene to HPPN (high-pressure purified nitrogen) to completely deactivate the original dual-active center catalyst components in the bed; after the reaction is completely terminated, reduce the reactor pressure, and take the lowest pressure when the compressor does not surge; continue to maintain the reaction temperature in the reactor, cut the purge main from HPPN back to ethylene, increase the amount of ethylene entering the purge main, and replace the materials used for deactivating the dual-active center catalytic polymerization reaction in the reactor by the pressure increase and decrease method. The replacement pressure is 900kPa to 1100kPa to 1400kPa (the replacement pressure is increased from 900kPa to 1100kPa, then increased to 1400kPa, and then reduced back to 900kPa, and the above process is repeated), and the replacement standard is CO2 in the reactor <5ppm.
[0090] S5: For the pretreatment operation of the bed powder in the reactor, CA-300 or CA-200 is selected as the bed pretreatment agent to completely eliminate the influence of the double active center catalyst residues and bed impurities on the metallocene catalyst; wherein, the injection amount of the bed pretreatment agent is 20 ppm of the bed weight, and after injection, it circulates in the reactor fluidized state for 1.5 h.
[0091] S6: According to the initiation conditions of the metallocene catalyst, the concentration of the gas phase components is re-established. Usually, only the concentrations of ethylene and nitrogen need to be established. After the gas phase components are established, a single-active-site metallocene catalyst is injected to initiate the reaction and produce a single-peak metallocene polyethylene product. Usually, the heat load can be seen in 20 minutes. Among them, the single-active-site metallocene catalyst adopts the easy-to-process metallocene catalyst EZ series.
[0092] Example 2 A method for converting a bimodal metallocene polyethylene product into a unimodal metallocene polyethylene product comprises the following steps: S1: Before stopping the injection of the dual-active center catalyst (using the same catalyst as in Example 1), stop feeding fresh isopentane (i.e., ICA) and recycled liquid, and quickly reduce the ICA concentration in the system to 60% of the original concentration; put the start-up heater into use, adjust the steam control valve according to the reaction temperature, and maintain the reaction temperature at 100°C to 110°C to preheat the reaction system in advance to prevent a sharp drop in temperature after the dual-active center catalyst is deactivated; increase the injection amount of the bed pretreatment agent (using the same bed pretreatment agent as in Example 1) to 70 ppm to ensure that the electrostatic stability and wall temperature of the reactor are stable, and maintain the injection until the reaction heat load drops to 0 t / h.
[0093] S2: Stop the injection of the dual-active center catalyst to allow it to deactivate naturally. Pay attention to the condensation rate of the reactor. When the condensation rate is close to 5%, open the angle valve of the CO2 cylinder and inject CO2 for 12 seconds. If the CO2 concentration is less than 2 ppm, inject CO2 for another 5 seconds to ensure that the CO2 concentration is between 3 ppm and 8 ppm.
[0094] S3: When the polymerization reaction no longer occurs, stop injecting gas phase components such as ethylene, hydrogen, and comonomers, reduce the discharge frequency of the reactor discharge system, maintain the reactor bed weight to the metallocene start-up requirement of 110 t, while maintaining the circulating gas velocity at 0.75 m / s and the expansion section material level at 45% to 55%.
[0095] S4: Adjust the steam control valve of the start-up heater to make the reactor temperature 80℃ to 90℃; maintain the reaction temperature, pressure and fluidization state in the reactor, and cut the purge mains of the reactor from ethylene to HPPN (high-pressure purified nitrogen) to completely deactivate the original dual-active center catalyst components in the bed; after the reaction is completely terminated, reduce the reactor pressure, and take the lowest pressure when the compressor does not surge; continue to maintain the reaction temperature in the reactor, cut the purge main from HPPN back to ethylene, increase the amount of ethylene entering the purge main, and replace the materials used for dual-active center catalytic polymerization reaction in the reactor by the pressure increase and decrease method. The replacement pressure is 900kPa to 1100kPa to 1400kPa (the replacement pressure is increased from 900kPa to 1100kPa, then increased to 1400kPa, and then reduced back to 900kPa, and the above process is repeated), and the replacement standard is CO2 in the reactor <5 ppm.
[0096] S5: For the pretreatment operation of the bed powder in the reactor, CA-300 or CA-200 is selected as the bed pretreatment agent to completely eliminate the influence of the double active center catalyst residues and bed impurities on the metallocene catalyst; wherein, the injection amount of the bed pretreatment agent is 25 ppm of the bed weight, and after injection, it circulates in the reactor fluidized state for 1 hour.
[0097] S6: According to the initiation conditions of the metallocene catalyst, the concentration of the gas phase components is re-established. Usually, only the concentrations of ethylene and nitrogen need to be established. After the gas phase components are established, a single-active-site metallocene catalyst (easy-to-process metallocene catalyst EZ series, using the same catalyst as in Example 1) is injected to initiate the reaction. Usually, the heat load can be seen in 20 minutes.
[0098] Comparative Example 1 A method for converting a bimodal metallocene polyethylene product into a unimodal metallocene polyethylene product comprises the following steps: S1: Before stopping the injection of the dual-active center catalyst (using the same dual-active center catalyst as in Example 1), stop feeding fresh isopentane (i.e., ICA) and recycled liquid, and quickly reduce the ICA concentration in the system to 60% of the original concentration; put the start-up heater into use, and adjust the steam control valve according to the reaction temperature to make the reaction temperature 100°C to 110°C, so as to preheat the reaction system in advance and prevent the temperature from dropping sharply after the dual-active center catalyst is deactivated; increase the injection amount of the bed pretreatment agent (the same as the bed pretreatment agent in Example 1) to 70 ppm, ensure that the electrostatic stability and wall temperature of the reactor are stable, and maintain the injection until the reaction heat load drops to 0 t / h.
[0099] S2: Stop the injection of the dual-active center catalyst to allow it to deactivate naturally. Pay attention to the reactor condensation rate. When the condensation rate is close to 5%, open the angle valve of the CO2 cylinder and inject CO2 for 12 seconds. If the CO2 concentration is less than 2 ppm, inject CO2 for another 5 seconds to ensure that the CO2 concentration is between 3 ppm and 8 ppm. S3: When the polymerization reaction is no longer occurring, stop injecting gas phase components such as ethylene, hydrogen, and comonomers, reduce the discharge frequency of the reactor discharge system, maintain the reactor bed weight to the metallocene start-up requirement of 110 t, while maintaining the circulating gas velocity at 0.75 m / s and the expansion section material level at 45% to 55%.
[0100] S4: Close the guide vane opening, set the PDS system parameters, and increase the material discharge speed until the bed powder is emptied.
[0101] S5: Adjust the steam control valve of the startup heater to maintain the reactor temperature at 80°C to 90°C.
[0102] S6: The reactor pressure is released to 300 kPa, the on-site steam manual valve is fully opened, and steam is added for 30 minutes, about 400 ppm, corresponding to the dew point: -30℃, and circulated for 1 hour.
[0103] S7: Open up the crude nitrogen process, purge the main pipe to the reactor with the maximum amount, and flow the displacement reactor at about 500 kPa (to ensure that the pressure difference between nitrogen and the reactor is above 100 kPa) until the hydrocarbon content is ≤ 0.2% v / v.
[0104] S8: The system replacement is qualified, the reaction system blind plate isolation is completed, the pipeline is disconnected, and the reactor manhole is opened for maintenance.
[0105] S9: After the overhaul is completed, replace with nitrogen until the oxygen content is ≤2% v / v, and carry out operations such as filling, replacing, heating, and establishing the gas phase of the metallocene polyethylene seed bed.
[0106] S10: According to the initiation conditions of the metallocene catalyst, the concentration of the gas phase components is re-established. Usually, only the concentrations of ethylene and nitrogen need to be established. After the gas phase components are established, the high-strength metallocene catalyst HP series is injected to initiate the reaction. Usually, the heat load can be seen in 20 minutes.
[0107] Comparative Example 2 A method for converting a bimodal metallocene polyethylene product into a unimodal metallocene polyethylene product comprises the following steps: S1: Before stopping the injection of the dual-active center catalyst (the same as the dual-active center catalyst in Example 1), stop feeding fresh isopentane (i.e., ICA) and recycled liquid to quickly reduce the ICA concentration in the system to 60% of the original concentration; put the start-up heater into use, adjust the steam control valve according to the reaction temperature, and make the reaction temperature 100°C to 110°C to preheat the reaction system in advance to prevent the temperature from dropping sharply after the dual-active center catalyst is deactivated; increase the injection amount of the bed pretreatment agent (the same as the bed pretreatment agent in Example 1) to 70 ppm to ensure that the electrostatic stability and wall temperature of the reactor are stable, and maintain the injection until the reaction heat load drops to 0 t / h.
[0108] S2: Stop injecting the dual-active-center catalyst to allow the dual-active-center-200 catalyst to deactivate naturally. Pay attention to the condensation rate of the reactor. When the condensation rate is close to 5%, open the angle valve of the CO2 cylinder and inject CO2 for 12 seconds. If the CO2 concentration is less than 2 ppm, inject CO2 again for 5 seconds to ensure that the CO2 concentration is between 3 ppm and 8 ppm.
[0109] S3: When the polymerization reaction is no longer occurring, stop injecting gas phase components such as ethylene, hydrogen, and comonomers, reduce the discharge frequency of the reactor discharge system, maintain the reactor bed weight to the metallocene start-up requirement of 110 t, while maintaining the circulating gas velocity at 0.75 m / s and the expansion section material level at 45% to 55%.
[0110] S4: Adjust the steam control valve of the start-up heater to maintain the reactor temperature at 80°C to 90°C; maintain the reaction temperature, pressure and fluidization state in the reactor, and cut the purge mains of the reactor from ethylene to HPPN (high-pressure purified nitrogen) to completely deactivate the original dual-active center catalyst components in the bed; after the reaction is completely terminated, reduce the reactor pressure, and take the lowest pressure when the compressor does not surge; continue to maintain the reaction temperature in the reactor, cut the purge main from HPPN back to ethylene, increase the amount of ethylene entering the purge main, and replace the materials used for dual-active center catalytic polymerization reaction in the reactor by the pressure increase and decrease method. The replacement pressure is 900kPa to 1100kPa to 1400kPa (the replacement pressure is increased from 900kPa to 1100kPa, then increased to 1400kPa, and then reduced back to 900kPa, and the above process is repeated), and the replacement standard is CO2 in the reactor <5 ppm.
[0111] S5: For the pretreatment operation of the bed powder in the reactor, CA-300 or CA-200 is selected as the bed pretreatment agent to completely eliminate the influence of the double active center catalyst residues and bed impurities on the metallocene catalyst; the injection amount of the bed pretreatment agent is 25 ppm of the bed weight, and after injection, it circulates in the reactor fluidized state for 1 hour.
[0112] S6: According to the initiation conditions of the metallocene catalyst, the concentration of the gas phase components is re-established. Usually, only the concentrations of ethylene and nitrogen need to be established. After the gas phase components are established, a single-active-site metallocene catalyst is injected. Here, the high-strength metallocene catalyst HP series is used to initiate the reaction. Usually, the heat load can be seen in 20 minutes.
[0113] Table 1 shows the conversion time of the production method of converting the bimodal metallocene polyethylene product to the unimodal metallocene polyethylene product provided in Examples 1 to 2 and Comparative Examples 1 to 2 and the fisheye level of the unimodal metallocene polyethylene products prepared therefrom.
[0114] As shown in Table 1, the fisheye index of the metallocene polyethylene film prepared by the methods provided in Examples 1 and 2 of the present invention and Comparative Example 1 can meet the requirements, and the time taken is less than 24 h; and Examples 1, 2 and Comparative Example 1 respectively meet the requirements of fisheye (0.8 mm) ≤ 6 / 1520 cm 2 , fisheye (0.4 mm) ≤ 15 / 1520 cm 2 The quality of the conversion method provided in Comparative Example 1 is comparable to that of similar foreign products. Although the product fisheye index can meet the requirements, the entire conversion adopts a discontinuous conversion method, which requires the reactor to be emptied and repaired before restarting the bed, which takes 120 hours. The conversion method provided in Comparative Example 2 takes less than 24 hours, but because the high-strength metallocene catalyst HP series is used when converting to single-peak metallocene polyethylene products, the metallocene polyethylene product obtained by catalytic polymerization is not soluble in the granular powder in the seed bed when the bed is not emptied. The polyethylene film material prepared from the metallocene polyethylene product has more fisheyes. Specifically, the fisheyes (0.4 mm) are greater than 15 / 1520cm 2 , fisheye (0.8 mm) greater than 6 / 1520 cm 2 , which is obviously disadvantageous compared to the conversion method provided in Example 1-2.
[0115] In summary, the production method of converting a bimodal metallocene polyethylene product to a unimodal metallocene polyethylene product provided by the present invention adopts the natural deactivation of a dual-active center catalyst, assists in the injection of a trace amount of CO2, does not empty the bed powder, does not clean the reactor, and adopts a bed pretreatment agent to avoid the electrostatic fluctuation of the reactor causing the bed to agglomerate. After the replacement is qualified, the gas phase is established, and a single-active center metallocene catalyst is injected to initiate the reaction to produce a unimodal metallocene polyethylene product. At the same time, the present invention sets a reasonable conversion sequence and adopts a reasonable single-active center metallocene catalyst to ensure that the fisheye index of the metallocene film product is qualified. The method has the following advantages: ① The conversion of the dual-active center product to the metallocene product can be completed without pouring out the dual-active center product seed bed and refilling the metallocene polyethylene seed bed, which minimizes the cost of extracting and filling the seed bed, greatly reduces the workload and working time, and reduces the inspection and maintenance cost of the device. ② The influence of the dual-active center series products on the fisheye level of the metallocene film product is greatly reduced, and the fisheye index of the produced metallocene film product is qualified.
[0116] In this article, "and / or" describes the association relationship of associated objects, indicating that three relationships may exist. For example, A and / or B can mean: A exists alone, A and B exist at the same time, and B exists alone. A and B can be singular or plural. In this article, "at least one" means one or more, and "plurality" means two or more. "At least one", "at least one of the following" or similar expressions refer to any combination of these items, including any combination of single or plural items.
[0117] The above description is only a specific implementation of the present application, so that those skilled in the art can understand or implement the present application. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present application. Therefore, the present application will not be limited to the embodiments shown herein, but will conform to the widest range consistent with the principles and novel features applied for herein.
[0118] Table 1 .
Claims
1. A method for converting a bimodal metallocene polyethylene product into a unimodal metallocene polyethylene product, characterized in that: The production method comprises the following steps: 1) Before stopping the injection of the dual-active-site catalyst, stop feeding the induced condensing agent and the recovered liquid; heat the reaction system to raise the temperature, inject a bed pretreatment agent, make the content of the bed pretreatment agent reach 50 ppm to 80 ppm of the reactor production load, and reduce the reaction heat load to 0 t / h, wherein the bed pretreatment agent includes an antistatic agent, and the antistatic agent includes at least one of CA-200 and CA-300; 2) Stop injecting the dual-active-center catalyst to allow the dual-active-center catalyst to deactivate naturally; inject CO2 when exiting the condensed state; 3) Stop injecting gas phase components, reduce the discharge frequency of the reactor discharge system, and maintain the reactor bed weight to the quality required for the start-up of unimodal metallocene polyethylene; 4) Heating the reaction system to a reaction temperature of a unimodal metallocene polyethylene product; maintaining the reaction temperature, pressure and fluidization state of the reaction system, and replacing the reaction system with nitrogen; then maintaining the reaction temperature of the reaction system, and replacing the reaction system with ethylene; 5) Pretreating the bed powder in the reaction system with a bed pretreatment agent, wherein the bed pretreatment agent includes an antistatic agent, and the antistatic agent includes at least one of CA-300 and CA-200, and the injection amount of the bed pretreatment agent is 15 ppm to 25 ppm of the bed weight, and the bed pretreatment agent is injected and circulated in the fluidized state of the reaction system for 1 h to 2 h; 6) Re-establish the gas phase component concentration according to the initiation conditions of the single-active-center metallocene catalyst; inject the single-active-center metallocene catalyst to initiate the reaction and convert to the production of a single-peak metallocene polyethylene product.
2. The method for converting a bimodal metallocene polyethylene product into a unimodal metallocene polyethylene product according to claim 1, characterized in that: In the step 1), the dual active site catalyst includes a BMC-200 catalyst; or / and In the step 1), the induced condensing agent comprises at least one of isopentane, hexane and isobutane; or / and In the step 1), the reaction system is heated to 100° C. to 110° C.
3. The method for converting a bimodal metallocene polyethylene product into a unimodal metallocene polyethylene product according to claim 1 or 2, characterized in that: In the step 1), the heating to raise the temperature of the reaction system comprises the following steps: The start-up heater was put into use, and the steam control valve was adjusted according to the polymerization reaction temperature of the bimodal metallocene polyethylene product. Preheating was performed in advance to prevent a sharp drop in the reaction temperature of the system after the deactivation of the dual-active center catalyst.
4. The method for converting a bimodal metallocene polyethylene product into a unimodal metallocene polyethylene product according to claim 3, characterized in that: In the step 2), exiting the condensed state means injecting CO2 after the condensation rate of the reaction system reaches 3% to 5%, thereby exiting the condensed state.
5. The method for converting a bimodal metallocene polyethylene product into a unimodal metallocene polyethylene product according to claim 4, characterized in that: In the step 2), when the condensation rate of the reaction system is 3% to 5%, CO2 is injected to a concentration less than 2 ppm, and then CO2 is injected again to a concentration of 3 ppm to 8 ppm.
6. The method for converting a bimodal metallocene polyethylene product into a unimodal metallocene polyethylene product according to claim 1, 2, 4 or 5, characterized in that: In step 3), the injection of gas phase components is stopped, the discharge frequency of the reactor discharge system is reduced, the reactor bed weight is maintained to the required quality for the start-up of unimodal metallocene polyethylene, and the circulating gas flow rate is maintained at 0.6 m / s to 0.8 m / s, and the material level of the expansion section is maintained at 35% to 60%; or / and In the step 3), the gas phase components include ethylene, hydrogen and comonomers; or / and In the step 3), the required start-up mass of the unimodal metallocene polyethylene is 110 t to 150 t.
7. The method for converting a bimodal metallocene polyethylene product into a unimodal metallocene polyethylene product according to claim 6, characterized in that: In the step 4), the reaction temperature of the unimodal metallocene polyethylene product is 80°C to 90°C; or / and In the step 4), the reaction system is replaced with nitrogen to terminate the polymerization reaction of the bimodal metallocene series product, and the reaction pressure is reduced to the lowest pressure when the compressor does not surge; or / and In the step 4), the reaction system is replaced by ethylene using a pressure increase / decrease method.
8. The method for converting a bimodal metallocene polyethylene product into a unimodal metallocene polyethylene product according to claim 7, characterized in that: In the step 4), the replacement pressure of the pressure rise and fall method is 900 kPa to 1100 kPa to 1400 kPa.
9. The method for converting a bimodal metallocene polyethylene product into a unimodal metallocene polyethylene product according to claim 8, characterized in that: In the step 4), ethylene is used to replace the reaction system to replace the material used to deactivate the dual-active center catalyst in the reactor. The replacement completion standard is: CO2 in the reactor is less than 5 ppm.
10. The method for converting a bimodal metallocene polyethylene product into a unimodal metallocene polyethylene product according to claim 1 or 2 or 4 or 5 or 7 or 8 or 9, characterized in that: In step 6), re-establishing the gas phase component concentrations includes: establishing ethylene concentration and nitrogen concentration; or / and In the step 6), the single-active-site metallocene catalyst comprises an easily processable metallocene catalyst.
11. The method for converting a bimodal metallocene polyethylene product into a unimodal metallocene polyethylene product according to claim 10, characterized in that: In step 6), a single active site metallocene catalyst is injected to initiate the reaction, and heat load can be seen in 20 minutes.
12. The method for converting a bimodal metallocene polyethylene product into a unimodal metallocene polyethylene product according to claim 11, characterized in that: The total switching time from bimodal metallocene polyethylene product to unimodal metallocene polyethylene product is 22 h to 24 h.
13. The method for converting a bimodal metallocene polyethylene product into a unimodal metallocene polyethylene product according to claim 12, characterized in that: The melt index of the produced unimodal metallocene polyethylene is 0.2 g / 10 min to 20 g / 10 min and the density is 0.910 g / cm 3 Up to 0.940 g / cm 3 .
Citation Information
Patent Citations
Method for quickly starting polymerization reaction in alpha-olefin gas-phase fluidized bed reactor
CN102558402A
Closed reactor transitions between metallocene catalysts
CN107531836A
Methods for scale-up from pilot plant to larger production facility
CN112055720A
Online switching method of metallocene catalyst and Ziegler-Natta catalyst
CN114426590A
Production method for converting chromium polyethylene into metallocene polyethylene
CN117567675A
Cited By
Equipment and method for preparing metallocene product antistatic agent storage tank
CN119911561A