Method for preparing solvent-free cation exchange resin through acid sleeving pretreatment
Through the acid-studded pretreatment method with step-by-step increase in the multi-gradient sulfuric acid concentration, the problems of organic solvent residue and local exothermic in the preparation of cation exchange resin were solved, and solvent-free cation exchange resin with high mechanical strength and excellent performance were prepared, which is suitable for water quality. deal with.
Patent Information
- Application Number
- CN202411278094.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-12
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-09-12
AI Technical Summary
The use of organic solvents during the preparation of existing cation exchange resins results in solvent residues, affecting the water quality treatment effect and polluting the environment. The direct use of high concentration of sulfuric acid will lead to excessive local exothermic heat and reduce the strength of the resin.
The acid pretreatment process with the multi-gradient sulfuric acid concentration gradually increased, avoiding the use of organic solvents, reducing local exothermic through gradient changes, improving the efficiency of the sulfonation reaction, and preparing a strong acid cation exchange resin with high mechanical strength.
The solvent-free cation exchange resin with high full exchange capacity, suitable moisture content and high sphere rate after grinding was successfully prepared, which solved the problems of solvent residue and local exothermic, and improved the mechanical strength and performance indicators of the resin.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of ion exchange resin preparation, and in particular relates to a method for preparing a solvent-free cation exchange resin by acid pretreatment. Background Art
[0002] Cation exchange resin is a granular polymer material with cation exchange function. Since cation exchange resin can remove cations through ion exchange, it is widely used in the separation of cations in fluids, such as the removal of calcium, magnesium ions, heavy metal cations, and ammonia nitrogen in water. Hydrogen cation exchange resin, as a solid acid, can also be used as a catalyst for many chemical reactions or a carrier for nanomaterials.
[0003] The preparation process of existing cation exchange resins generally uses organic solvents to swell and then carry out sulfonation reaction. For example, in the method disclosed in the patent with publication number CN 112062888 A, the resin white balls are swelled with dichloroethane and then sulfonated with concentrated sulfuric acid under heating conditions. In fact, the method of using organic solvents to swell and prepare strong acid cation exchange resins is very mature, but the cation exchange resins prepared by this method will eventually have residual organic solvents. The article "Study on organic dissolution of ion exchange resins for condensate treatment" (Ion Exchange and Adsorption, 1999, (03): 272-278) points out that the organic matter dissolved by the cation resin may not only affect the water treatment effect, but also pollute the anion exchange resin in the mixed bed. Moreover, some dissolved organic matter is also toxic or carcinogenic, which will harm the environment and human health when used in water treatment. Therefore, a method for preparing a solvent-free cation exchange resin is urgently needed.
[0004] Chinese patent CN108102032 A discloses a method for preparing a solvent-free green styrene-based cation exchange resin. The method does not use ethylene dichloride as a swelling agent to carry out the sulfonation reaction. Instead, a cross-linking agent is used to increase the elasticity of the skeleton, a secondary polymerization is used to increase the strength, a high-concentration concentrated sulfuric acid is used for sulfonation, and a multi-gradient concentration is used for stepwise acidification to obtain a resin with the same performance and index as an ion exchange resin prepared without using ethylene dichloride as a swelling agent. In addition, multiple applications of the water phase can reduce the pollution of the water phase to the environment. However, not using a swelling agent will increase the risk of reduced resin strength. Summary of the invention
[0005] The purpose of the present invention is to provide a method for preparing a solvent-free cation exchange resin by acid pretreatment on the basis of the prior art. Before the sulfonation reaction, an acid pretreatment process with a multi-gradient sulfuric acid concentration increasing step by step is adopted to avoid the use of an organic solvent and strengthen the swelling process, thereby overcoming the defect of excessive local heat release caused by directly using high-concentration sulfuric acid, thereby preparing a strong acid cation exchange resin with high mechanical strength, wherein the total exchange capacity of the resin is greater than 4.5 mmol / g, the water content is 45-58%, the ball rate after grinding is greater than 99%, and the ball rate after infiltration grinding is greater than 98%.
[0006] The technical solution of the present invention is as follows:
[0007] A method for preparing an acid pretreated solvent-free cation exchange resin comprises the following steps:
[0008] (1) Acid pretreatment: The polystyrene-divinylbenzene white balls are acid pretreated with sulfuric acid. During the acid pretreatment, the concentration of sulfuric acid is increased in a gradient distribution, and each stage lasts 10 to 120 minutes to obtain a pretreated resin;
[0009] (2) Sulfonation reaction: the resin obtained in step (1) is mixed with concentrated sulfuric acid, and the temperature is raised to 95 to 155° C. for sulfonation reaction, and the reaction time is 1 to 10 hours;
[0010] (3) acidification: the resin obtained in step (2) is acidified with sulfuric acid, and the concentration of sulfuric acid is gradually reduced according to a gradient distribution during the acidification process, and each stage lasts for 0.5 to 2 hours;
[0011] (4) Washing: The resin obtained in step (3) is transformed with a sodium hydroxide solution and then washed until neutral to obtain an acid-pretreated solvent-free cation exchange resin.
[0012] In the present invention, in step (1), sulfuric acid is divided into 1 to 8 successively increasing concentration gradients for acid pretreatment, and the concentration of sulfuric acid is 3 to 89%. Preferably, it can be divided into 3 to 6 successively increasing concentration gradients, and more preferably, it can be divided into 6 successively increasing concentration gradients.
[0013] For example, sulfuric acid is divided into three successively increasing concentration gradients for acid pretreatment, and the concentration gradient of sulfuric acid is 20-30%, 40-60%, and 75-85%; preferably, the concentration gradient of sulfuric acid is 25%, 50%, and 80%.
[0014] For example, sulfuric acid is divided into four successively increasing concentration gradients for acid pretreatment, and the concentration gradients of sulfuric acid are 5-25%, 35-50%, 65-75%, and 83-88%; preferably, the concentration gradients of sulfuric acid are 10-20%, 40-45%, 70%, and 85-87%.
[0015] For example, sulfuric acid is divided into 6 successively increasing concentration gradients for acid pretreatment, and the concentration gradients of sulfuric acid are 3-18%, 19-32%, 33-47%, 48-57%, 58-77%, and 78-87%; preferably, the concentration gradient of sulfuric acid is 5-15%, 20-30%, 35-45%, 50-55%, 60-75%, and 80-85%.
[0016] In the present invention, in step (1), the moisture content of the polystyrene-divinylbenzene white balls is 1-10%, specifically 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9% or 10%.
[0017] In the present invention, in step (2), the concentration of concentrated sulfuric acid is 90 to 98%, preferably 90 to 95%.
[0018] In step (3) of the present invention, during the acid treatment, the concentration of sulfuric acid is gradually reduced, and the concentration of sulfuric acid is 87-3%. The sulfuric acid can be divided into 5-12 successively reduced concentration gradients for acid treatment. Preferably, it can be divided into 5-10 successively reduced concentration gradients, and more preferably, it can be divided into 8 successively reduced concentration gradients.
[0019] Specifically, when sulfuric acid is divided into 8 successively decreasing concentration gradients, the concentration gradient of sulfuric acid is 87-79%, 77-69%, 67-59%, 57-49%, 47-39%, 37-29%, 27-19%, and 17-3%; more preferably, the concentration gradient of sulfuric acid is 85-80%, 75-70%, 65-60%, 55-50%, 45-40%, 35-30%, 25-20%, and 10-5%.
[0020] Adopt the technical scheme of the present invention, the advantages are as follows:
[0021] The invention provides a method for preparing a solvent-free cation exchange resin by acid pretreatment. Before a sulfonation reaction, an acid pretreatment process with a multi-gradient sulfuric acid concentration increasing step by step is adopted, aiming to avoid using an organic solvent and strengthen the swelling process, thereby overcoming the defect of excessive local heat release caused by directly using high-concentration sulfuric acid, thereby preparing a strong acid cation exchange resin with high mechanical strength, wherein the total exchange capacity of the resin is greater than 4.5 mmol / g, the water content is 45-58%, the ball rate after grinding is greater than 99%, and the ball rate after infiltration grinding is greater than 98%. DETAILED DESCRIPTION
[0022] The present invention can be better understood according to the following examples. However, it is easy for those skilled in the art to understand that the contents described in the examples are only used to illustrate the present invention, and should not and will not limit the present invention described in detail in the claims.
[0023] Example 1
[0024] A method for preparing an acid pretreated solvent-free cation exchange resin comprises the following steps:
[0025] (1) Acid pretreatment: The polystyrene-divinylbenzene white balls with a moisture content of 1% were acid pretreated with sulfuric acid. The sulfuric acid was divided into 6 increasing concentration gradients, namely 5%, 20%, 35%, 50%, 60%, and 80%.
[0026] The specific acid pretreatment process is as follows: after mixing polystyrene-divinylbenzene white balls with a moisture content of 1% with 5% sulfuric acid for 90 minutes, solid material I is separated by centrifugation; after mixing solid material I with 20% sulfuric acid for 80 minutes, solid material II is separated by centrifugation; after mixing solid material II with 35% sulfuric acid for 80 minutes, solid material III is separated by centrifugation; after mixing solid material III with 50% sulfuric acid for 80 minutes, solid material IV is separated by centrifugation; after mixing solid material IV with 60% sulfuric acid for 80 minutes, solid material V is separated by centrifugation; after mixing solid material V with 80% sulfuric acid for 80 minutes, solid material VI is separated by centrifugation.
[0027] (2) Sulfonation reaction: The resin obtained in step (1) (i.e., solid material VI) was mixed with 90% concentrated sulfuric acid, and the temperature was raised to 120° C. for sulfonation reaction. The reaction time was 9 hours, and a solid material VII was separated.
[0028] (3) Acidification: The resin obtained in step (2) (i.e., solid material VII) is acidified with sulfuric acid. During the acidification process, the concentration of sulfuric acid is gradually reduced according to a gradient distribution. The concentrations of sulfuric acid are 85%, 70%, 60%, 54%, 43%, 30%, 21%, and 6%, respectively. Each stage is performed for 1 hour.
[0029] (4) Washing: The resin obtained in step (3) is washed with deionized water, then transformed with a 5% sodium hydroxide solution, and then washed to neutrality to obtain an acid-pretreated solvent-free cation exchange resin.
[0030] Example 2
[0031] A method for preparing an acid pretreated solvent-free cation exchange resin comprises the following steps:
[0032] (1) Acid pretreatment: The polystyrene-divinylbenzene white balls with a moisture content of 5% were acid pretreated with sulfuric acid. The sulfuric acid was divided into four increasing concentration gradients, namely 10%, 40%, 70%, and 85%.
[0033] The specific acid pretreatment process is as follows: after mixing polystyrene-divinylbenzene white balls with a moisture content of 5% with 10% sulfuric acid for 60 minutes, solid material I is separated by centrifugation; after mixing solid material I with 40% sulfuric acid for 60 minutes, solid material II is separated by centrifugation; after mixing solid material II with 70% sulfuric acid for 60 minutes, solid material III is separated by centrifugation; after mixing solid material III with 85% sulfuric acid for 60 minutes, solid material IV is separated by centrifugation.
[0034] (2) Sulfonation reaction: The resin obtained in step (1) (i.e., solid material IV) was mixed with 95% concentrated sulfuric acid, and the temperature was raised to 95° C. for sulfonation reaction. The reaction time was 1 hour, and then the temperature was raised to 100° C. for further sulfonation reaction. The reaction time was 2 hours, and the solid material V was separated.
[0035] (3) Acidification: The resin obtained in step (2) (i.e., solid material V) is acidified with sulfuric acid. During the acidification process, the concentration of sulfuric acid is gradually reduced according to a gradient distribution. The concentrations of sulfuric acid are 85%, 70%, 60%, 54%, 43%, 30%, 21%, and 6%, respectively. Each stage lasts for 1 hour.
[0036] (4) Washing: The resin obtained in step (3) is washed with deionized water, then transformed with a 5% sodium hydroxide solution, and then washed to neutrality to obtain an acid-pretreated solvent-free cation exchange resin.
[0037] Example 3
[0038] A method for preparing an acid pretreated solvent-free cation exchange resin comprises the following steps:
[0039] (1) Acid pretreatment: The polystyrene-divinylbenzene white balls with a moisture content of 10% were acid pretreated with sulfuric acid. The sulfuric acid was divided into four increasing concentration gradients, namely 20%, 45%, 70%, and 87%.
[0040] The specific acid pretreatment process is as follows: after mixing polystyrene-divinylbenzene white balls with a moisture content of 10% with 20% sulfuric acid for 30 minutes, centrifuge to separate solid material I; after mixing solid material I with 45% sulfuric acid for 45 minutes, centrifuge to separate solid material II; after mixing solid material II with 70% sulfuric acid for 30 minutes, centrifuge to separate solid material III; after mixing solid material III with 87% sulfuric acid for 30 minutes, centrifuge to separate solid material IV.
[0041] (2) Sulfonation reaction: The resin obtained in step (1) (i.e., solid material IV) was mixed with 93% concentrated sulfuric acid, and the temperature was raised to 100° C. for sulfonation reaction for 2 hours, and then the temperature was raised to 120° C. for further sulfonation reaction for 6 hours, and solid material V was separated.
[0042] (3) Acidification: The resin obtained in step (2) (i.e., solid material V) is acidified with sulfuric acid. During the acidification process, the concentration of sulfuric acid is gradually reduced according to a gradient distribution. The concentrations of sulfuric acid are 85%, 70%, 60%, 54%, 43%, 30%, 21%, and 6%, respectively. Each stage lasts for 1 hour.
[0043] (4) Washing: The resin obtained in step (3) is washed with deionized water, then transformed with a 5% sodium hydroxide solution, and then washed to neutrality to obtain an acid-pretreated solvent-free cation exchange resin.
[0044] Example 4
[0045] A method for preparing an acid pretreated solvent-free cation exchange resin comprises the following steps:
[0046] (1) Acid pretreatment: The polystyrene-divinylbenzene white balls with a moisture content of 10% were acid pretreated with sulfuric acid. The sulfuric acid was divided into 6 increasing concentration gradients, namely 15%, 30%, 45%, 55%, 75%, and 85%.
[0047] The specific acid pretreatment process is as follows: after mixing polystyrene-divinylbenzene white balls with a moisture content of 10% with 15% sulfuric acid for 20 minutes, centrifuge to separate solid material I; after mixing solid material I with 30% sulfuric acid for 30 minutes, centrifuge to separate solid material II; after mixing solid material II with 45% sulfuric acid for 30 minutes, centrifuge to separate solid material III; after mixing solid material III with 55% sulfuric acid for 30 minutes, centrifuge to separate solid material IV; after mixing solid material IV with 75% sulfuric acid for 30 minutes, centrifuge to separate solid material V; after mixing solid material V with 85% sulfuric acid for 20 minutes, centrifuge to separate solid material VI.
[0048] (2) Sulfonation reaction: The resin obtained in step (1) (i.e., solid material VI) was mixed with 93% concentrated sulfuric acid, and the temperature was raised to 110° C. for sulfonation reaction. The reaction time was 2 hours, and then the temperature was raised to 130° C. for further sulfonation reaction. The reaction time was 6 hours, and the solid material VII was separated.
[0049] (3) Acidification: The resin obtained in step (2) (i.e., solid material VII) is acidified with sulfuric acid. During the acidification process, the concentration of sulfuric acid is gradually reduced according to a gradient distribution. The concentrations of sulfuric acid are 85%, 70%, 60%, 54%, 43%, 30%, 21%, and 6%, respectively. Each stage is performed for 1 hour.
[0050] (4) Washing: The resin obtained in step (3) is washed with deionized water, then transformed with a 5% sodium hydroxide solution, and then washed to neutrality to obtain an acid-pretreated solvent-free cation exchange resin.
[0051] Example 5
[0052] A method for preparing an acid pretreated solvent-free cation exchange resin comprises the following steps:
[0053] (1) Acid pretreatment: The polystyrene-divinylbenzene white balls with a moisture content of 8% were acid pretreated with sulfuric acid. The sulfuric acid concentration gradient was 3 increasing levels, namely 25%, 50%, and 80%.
[0054] The specific acid pretreatment process is as follows: after mixing polystyrene-divinylbenzene white balls with a moisture content of 8% with 25% sulfuric acid for 45 minutes, centrifuge to separate solid material I; after mixing solid material I with 50% sulfuric acid for 45 minutes, centrifuge to separate solid material II; after mixing solid material II with 80% sulfuric acid for 45 minutes, centrifuge to separate solid material III.
[0055] (2) Sulfonation reaction: The resin obtained in step (1) (i.e., solid material III) was mixed with 94% concentrated sulfuric acid, and the temperature was raised to 100° C. for sulfonation reaction. The reaction time was 1 hour, and then the temperature was raised to 155° C. for further sulfonation reaction. The reaction time was 3 hours, and the solid material IV was separated.
[0056] (3) Acidification: The resin obtained in step (2) (i.e., solid material IV) is acidified with sulfuric acid. During the acidification process, the concentration of sulfuric acid is gradually reduced according to a gradient distribution. The concentrations of sulfuric acid are 85%, 70%, 60%, 54%, 43%, 30%, 21%, and 6%, respectively. Each stage lasts for 1 hour.
[0057] (4) Washing: The resin obtained in step (3) is washed with deionized water, then transformed with a 5% sodium hydroxide solution, and then washed to neutrality to obtain an acid-pretreated solvent-free cation exchange resin.
[0058] Comparative Example 1
[0059] (1) Sulfonation reaction: polystyrene-divinylbenzene white balls with a moisture content of 1% were mixed with 93% concentrated sulfuric acid, and the temperature was raised to 120° C. for sulfonation reaction. The reaction time was 9 hours, and a solid material I was separated.
[0060] (2) Acidification: The resin obtained in step (1) (i.e., solid material I) is acidified with sulfuric acid. During the acidification process, the concentration of sulfuric acid is gradually reduced according to a gradient distribution. The concentrations of sulfuric acid are 85%, 70%, 60%, 54%, 43%, 30%, 21%, and 6%, respectively. Each stage lasts for 1 hour.
[0061] (3) Washing: The resin obtained in step (2) is washed with deionized water, then transformed with a 5% sodium hydroxide solution, and then washed to neutrality to obtain an acid-pretreated solvent-free cation exchange resin.
[0062] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, a person skilled in the art should understand that it is still possible to modify the technical solutions described in the aforementioned embodiments, or to perform equivalent replacements on some of the technical features therein. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for preparing an acid pretreated solvent-free cation exchange resin, characterized in that: The steps include: (1) Acid pretreatment: The polystyrene-divinylbenzene white balls are acid pretreated with sulfuric acid. During the acid pretreatment, the concentration of sulfuric acid is increased in a gradient distribution, and each stage lasts 10 to 120 minutes to obtain a pretreated resin; (2) Sulfonation reaction: the resin obtained in step (1) is mixed with concentrated sulfuric acid, and the temperature is raised to 95 to 155° C. for sulfonation reaction, and the reaction time is 1 to 10 hours; (3) acidification: the resin obtained in step (2) is acidified with sulfuric acid, and the concentration of sulfuric acid is gradually reduced according to a gradient distribution during the acidification process, and each stage lasts for 0.5 to 2 hours; (4) Washing: The resin obtained in step (3) is transformed with a sodium hydroxide solution and then washed until neutral to obtain an acid-pretreated solvent-free cation exchange resin.
2. The preparation method according to claim 1, characterized in that: In step (1), sulfuric acid is divided into 1 to 8 successively increasing concentration gradients for acid pretreatment, and the concentration of sulfuric acid is 3 to 89%.
3. The preparation method according to claim 2, characterized in that: In step (1), sulfuric acid is divided into three successively increasing concentration gradients for acid pretreatment, and the concentration gradients of sulfuric acid are 20-30%, 40-60%, and 75-85%; preferably, the concentration gradients of sulfuric acid are 25%, 50%, and 80%.
4. The preparation method according to claim 2, characterized in that: In step (1), sulfuric acid is divided into 4 successively increasing concentration gradients for acid pretreatment, and the concentration gradients of sulfuric acid are 5-25%, 35-50%, 65-75%, and 83-88%; preferably, the concentration gradients of sulfuric acid are 10-20%, 40-45%, 70%, and 85-87%.
5. The preparation method according to claim 2, characterized in that: In step (1), sulfuric acid is divided into 6 successively increasing concentration gradients for acid pretreatment, and the concentration gradients of sulfuric acid are 3-18%, 19-32%, 33-47%, 48-57%, 58-77%, and 78-87%; preferably, the concentration gradient of sulfuric acid is 5-15%, 20-30%, 35-45%, 50-55%, 60-75%, and 80-85%.
6. The preparation method according to claim 1, characterized in that: In step (1), the water content of the polystyrene-divinylbenzene white balls is 1-10%.
7. The preparation method according to claim 1, characterized in that: In step (2), the concentration of concentrated sulfuric acid is 90 to 98%, preferably 90 to 95%.
8. The preparation method according to claim 1, characterized in that: In step (3), the concentration of sulfuric acid is 87-3%, and the sulfuric acid is divided into 5-12 successively decreasing concentration gradients for acid treatment.
9. The preparation method according to claim 9, characterized in that: In step (3), sulfuric acid is divided into 8 successively decreasing concentration gradients for acid treatment, and the concentration gradients of sulfuric acid are 87-79%, 77-69%, 67-59%, 57-49%, 47-39%, 37-29%, 27-19%, and 17-3%.
10. The preparation method according to claim 9, characterized in that: In step (3), the concentration gradient of sulfuric acid is 85-80%, 75-70%, 65-60%, 55-50%, 45-40%, 35-30%, 25-20%, and 10-5%.
Citation Information
Patent Citations
Method for preparing no-solvent green styrene-series cation exchange resin
CN108102032A
Preparation method of super-strong acid cation exchange resin
CN112062888A
Method for reducing waste acid amount in cation resin production process by adopting gradient dilution method
CN107903350A
Nuclear-grade cation exchange resin and preparation method thereof
CN117264104A
Production method of highly purified ion cation-exchange resin
JP2024079022A
Cited By
Swelling-agent-free production method of macroporous ion exchange resin
CN119306876A
Sulfonic acid type cation exchange resin as well as preparation method and application thereof
CN121591940A