Preparation process of slow-rebound foam with magnetic effect
By embedding magnetic particles in slow rebound foam, the problem of insufficient recovery speed and breathability of traditional foam is solved. Combined with the magnetic therapy effect, the preparation of magnetic foam is realized, and the functionality and applicability of the product is improved.
Patent Information
- Application Number
- CN202411141347.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-20
- Publication Date
- 2024-11-22
AI Technical Summary
Traditional slow rebound foams have limitations in recovery speed and breathability, limiting their application in a wider field and lacking magnetic functions to exploit magnetic therapeutic effects.
A process is used to embed magnetic particles (such as Fe3O4) into a slow rebound foam, and the preparation of basic copper carbonate, benzoyl chloride and diphenylmethane diisocyanate trimer (MDI) and other materials to form a slow magnetic effect. Rebound bubble. The process includes the preparation of alkaline copper carbonate under vacuum, the preparation of magnetic particles, the preparation of benzoyl chloride and MDI, and finally the material is fully foamed while standing.
It improves the magnetic properties and breathability of the foam, while maintaining the original comfort and support, enhancing the functionality of the product, and is suitable for improving sleep quality and promoting physical health.
Smart Images

Figure CN118994535A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the preparation of a new material, in particular to a preparation process of a slow-rebound foam with magnetic effect. Background Art
[0002] As people's pursuit of healthy life continues to increase and science and technology continue to advance, people pay more and more attention to improving sleep quality and promoting physical health. Good sleep is essential to maintaining the balance of human physiological functions, improving quality of life and work efficiency.
[0003] In recent years, a series of products designed to improve sleep quality have appeared on the market. Among them, bedding with special functions has attracted attention. Among many beddings, slow-rebound foam is favored by consumers because of its unique physical properties. It can be shaped according to the pressure of the human body, provide personalized support effects, effectively relieve the pressure of the neck and spine, and help improve sleep quality. However, traditional slow-rebound foam has some limitations, such as slow recovery speed and poor air permeability. These problems limit its application in a wider range of fields. In order to overcome the above limitations and further improve the functionality of the product, people began to explore the introduction of magnetic materials into slow-rebound foam. Magnetic therapy, as a traditional natural therapy, is widely believed to have certain help and benefits to the human body, such as promoting blood circulation and relieving muscle pain. Embedding magnetic particles into slow-rebound foam can not only utilize the beneficial effects of magnetism, but also maintain the original comfort and support of slow-rebound foam. Therefore, it is urgent to invent slow-rebound foam containing magnetic particles. Summary of the invention
[0004] In view of the above problems, the present invention provides a process for preparing slow-rebound foam with magnetic effect.
[0005] The invention relates to a preparation process of slow-rebound foam with magnetic effect, comprising the following steps: preparation of basic copper carbonate, preparation of magnetic particles, preparation of benzoyl chloride, preparation of diphenylmethane diisocyanate trimer (MDI), and preparation of slow-rebound foam.
[0006] Preferably, step (1) preparation of basic copper carbonate
[0007] A certain proportion of copper-based precursor and water are placed in a round-bottom flask, filtered by a vacuum pump, the vacuum degree is controlled, the electric heating jacket is heated at high temperature, ammonia tail gas is absorbed by a three-stage absorption bottle, water is used as the tail gas absorption liquid, and after the ammonia is evaporated, the solid is filtered and washed to obtain basic copper carbonate;
[0008] Step (2) Preparation of magnetic particles
[0009] First, weigh a small amount of hydrated ammonium ferrous sulfate and a small amount of hydrated ferric chloride (FeCl3·6H2O), and a certain amount of basic copper carbonate in step (1), dissolve them in distilled water, control the reaction temperature, stir, and obtain a mixed solution. Under argon protection, weigh hydrazine hydrate, slowly add it dropwise to the mixed solution, stir to react, centrifuge, and obtain a brown-black solid. Wash with distilled water until the pH value of the mixed solution is within a certain range, then wash with anhydrous ethanol and dry to obtain a precursor FeO(OH). Then add the precursor FeO(OH) to a hydrothermal autoclave, add a small amount of ammonia water, react at high temperature for a period of time, cool naturally to room temperature, take out the reactant, centrifuge, and obtain a black solid precipitate. Wash with distilled water repeatedly until the pH value of the solution is within a certain range, wash with anhydrous ethanol again and dry to obtain Fe3O4 particles.
[0010] Step (3) Preparation of benzoyl chloride
[0011] In a three-necked flask equipped with a spherical condenser and a stirring device, add benzoic acid and benzyl chloride in a certain proportion, then add deionized water, turn on an electric stirrer for stirring, and heat with an electric heating mantle. During heating, control the reaction temperature. When no gas is generated, stop heating. Absorb the tail gas with a NaOH solution. Remove the spherical condenser and the stirring device, replace them with a fractionating device and connect a straight condenser. Then add the magnetic particles in step (2) and start heating. After heating for a period of time, cool to obtain benzoyl chloride.
[0012] Step (4) Preparation of diphenylmethane diisocyanate trimer (MDI)
[0013] MDI, ethyl acetate (EAC), and an antioxidant were added to a dry four-necked flask equipped with a thermometer, a stirring paddle, and a reflux condenser, and nitrogen was introduced for protection. Stirring was started, heating was performed, and deionized water was gradually added dropwise. Then, the benzoyl chloride in step (3) was added as an inhibitor to terminate the reaction, thereby obtaining diphenylmethane diisocyanate trimer (MDI);
[0014] Step (5) Preparation of slow rebound foam
[0015] First, weigh a small amount of quartz sand powder, red phosphorus, and polyether polyol, put them into a glass cup, stir them thoroughly with a glass rod, then add the diphenylmethane diisocyanate trimer (MDI) and deionized water in step (4), stir them quickly with a glass rod, and after mixing evenly, put them into a container and let them stand to fully foam and set to obtain a slow-rebound foam.
[0016] Preferably, step (1) preparation of basic copper carbonate
[0017] The copper-based precursor and water are placed in a round-bottom flask in a ratio of 1-5:2-5, and a vacuum pump is used for filtration, and the vacuum degree is controlled to be 0.01-0.08 MPa. The electric heating mantle is heated to 60-100° C., and a three-stage absorption bottle is used to absorb ammonia tail gas, and water is used as the tail gas absorption liquid. After the ammonia is evaporated, the solid is filtered and washed to obtain basic copper carbonate.
[0018] The advantage of adopting the present invention is that by distilling ammonia under vacuum conditions and using a multi-stage absorption system to absorb ammonia tail gas, the generation of by-products is effectively avoided, so that the output product maintains a high purity, and the ammonia can be efficiently distilled, laying a solid foundation for the next step of preparation.
[0019] Preferably, in step (2), the preparation of magnetic particles
[0020] First, weigh 0.5-1g of hydrated ammonium ferrous sulfate, 0.5-1g of hydrated ferric chloride (FeCl3·6H2O), and 5-10g of basic copper carbonate of step (1), dissolve them in 100-200mL of distilled water, control the reaction temperature to 2-5°C, stir to obtain a mixed solution, weigh 2-5g of hydrazine hydrate under argon protection, slowly add it dropwise to the mixed solution, stir the reaction for 1-5h, centrifuge to obtain a brown-black solid, wash with distilled water until the pH of the mixed solution is The reaction mixture is stirred for 24 hours at 200-500 ℃ for 24-48 hours, and then the mixture is washed with anhydrous ethanol and dried to obtain a precursor FeO(OH). Then 1-5 g of the precursor FeO(OH) is added to a hydrothermal kettle, and 20-50 mL of 0.6-1% ammonia water is added. The mixture is reacted at 200-500 ℃ for 24-48 hours, and then naturally cooled to room temperature. The reactant is taken out and centrifuged to obtain a black solid precipitate. The mixture is repeatedly washed with distilled water until the pH value of the solution is 7-10, and then washed with anhydrous ethanol and dried to obtain Fe3O4 particles.
[0021] The invention has the advantages that, by using basic copper carbonate as a precipitant, iron ions can be completely precipitated, and additional impurities can be effectively isolated; hydrazine hydrate is used as a reducing agent to reduce FeO(OH) to Fe3O4 particles; and the reaction is carried out under the protection of argon gas to prevent oxidation of Fe3O4.
[0022] Preferably, step (3) preparation of benzoyl chloride
[0023] In a 250-500 mL three-necked flask equipped with a spherical condenser and a stirring device, add benzoic acid and benzyl chloride in a ratio of 1-5:1-5, then add 10-20 mL of deionized water, turn on an electric stirrer for stirring, and heat with an electric heating mantle. During heating, control the reaction temperature to be between 65-120° C. When no gas is generated, stop heating, absorb the tail gas with a NaOH solution, remove the spherical condenser and the stirring device, replace them with a fractionating device and connect it to a straight condenser, then add 10-20 g of the magnetic particles in step (2) and start heating. After heating for 40-60 min, cool to obtain benzoyl chloride.
[0024] The advantages of the present invention are that the energy consumption is reduced by controlling the reaction temperature, while the selectivity and yield of the reaction are improved. Water is used as the absorption liquid to reduce the emission of toxic and harmful substances. The tail gas is absorbed by the NaOH solution to reduce the emission of harmful gases. The added magnetic particles are helpful for the separation and purification of the product, and the catalytic effect is also improved, thereby improving the reaction efficiency.
[0025] Preferably, step (4) preparation of diphenylmethane diisocyanate trimer (MDI)
[0026] In a dry four-necked flask equipped with a thermometer, a stirring paddle and a reflux condenser, add 10-20 g of MDI, 5-10 g of ethyl acetate (EAC), 20-40 mL of an antioxidant and introduce nitrogen protection, start stirring, heat to 40-50° C., gradually add deionized water dropwise until 20-50 mL is reached, and then add 2-5 g of the inhibitor benzoyl chloride in step (3) to terminate the reaction to obtain diphenylmethane diisocyanate trimer (MDI).
[0027] The invention has the advantages that ethyl acetate is used as the solvent, because its polarity is weaker than that of water, so that it can interact with polar molecules and thus has excellent solubility; an antioxidant is added to effectively prevent the oxidative degradation of raw materials and products during the reaction process, thereby ensuring the stability of the product; the entire reaction system is operated under nitrogen protection, thereby effectively isolating oxygen and moisture in the air and avoiding oxidation of the raw materials and intermediates.
[0028] Preferably, in step (5), the preparation of slow rebound foam
[0029] First, weigh 4-10 g of quartz sand powder, 2-10 g of red phosphorus, and 5-15 g of polyether polyol respectively, put them into a glass cup, stir them thoroughly with a glass rod, then add 5-10 g of diphenylmethane diisocyanate trimer (MDI) and 20-50 mL of deionized water in step (4), stir them quickly with a glass rod for 1-5 min, and after mixing evenly, put them into a container and let them stand for 2-5 h to fully foam and shape them, so as to obtain a slow-rebound foam.
[0030] The invention has the advantage that, because the diphenylmethane diisocyanate trimer has extremely high reactivity and structural stability, it can form a tight and regular polymer network at the molecular level, thereby enhancing the performance of the slow-rebound foam.
[0031] In summary, the present invention has the following beneficial effects:
[0032] 1. The advantage of the present invention is that by distilling ammonia under vacuum conditions and using a multi-stage absorption system to absorb ammonia tail gas, the generation of by-products is effectively avoided, so that the output product maintains a high purity, and the ammonia can be efficiently distilled, laying a solid foundation for the next step of preparation.
[0033] 2. The present invention has the advantages that, by using basic copper carbonate as a precipitant, iron ions can be completely precipitated, and additional impurities can be effectively isolated. Hydrazine hydrate is used as a reducing agent to reduce FeO(OH) to Fe3O4 particles. The reaction is carried out under the protection of argon gas to prevent oxidation of Fe3O4.
[0034] 3. The advantages of the present invention are that by controlling the reaction temperature, energy consumption is reduced, while at the same time it is beneficial to improve the selectivity and yield of the reaction. Using water as the absorption liquid reduces the emission of toxic and harmful substances, and using NaOH solution to absorb tail gas can reduce the emission of harmful gases. The added magnetic particles help to separate and purify the product, and also improve the catalytic effect and the reaction efficiency.
[0035] 4. The present invention has the advantages that ethyl acetate is used as the solvent because its polarity is weaker than that of water, so that it can interact with polar molecules and thus has excellent solubility. The addition of an antioxidant effectively prevents the oxidative degradation of the raw materials and products during the reaction, thereby ensuring the stability of the product. The entire reaction system is operated under nitrogen protection, effectively isolating oxygen and moisture in the air, thereby avoiding oxidation of the raw materials and intermediates.
[0036] 5. The advantage of the present invention is that, because the diphenylmethane diisocyanate trimer has extremely high reactivity and structural stability, it can form a tight and regular polymer network at the molecular level, thereby enhancing the performance of the slow-rebound foam. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] Figure 1 The present invention is a process flow chart of preparing slow-rebound foam with magnetic effect. DETAILED DESCRIPTION
[0038] The following examples are used to illustrate the present invention, but are not intended to limit the scope of the present invention. Without departing from the spirit and substance of the present invention, modifications or substitutions made to the methods, steps or conditions of the present invention are within the scope of the present invention.
[0039] If not specifically stated, the technical means used in the examples are conventional means known to those skilled in the art. In addition, all the raw materials used in the examples are known commercial products.
[0040] Example 1
[0041] Step (1) Preparation of basic copper carbonate
[0042] The copper-based precursor and water are placed in a round-bottom flask in a ratio of 1:2, and a vacuum pump is used for filtration. The vacuum degree is controlled at 0.01 MPa, and the electric heating mantle is heated to 60°C. A three-stage absorption bottle is used to absorb ammonia tail gas, and water is used as the tail gas absorption liquid. After the ammonia is evaporated, the solid is filtered and washed to obtain basic copper carbonate;
[0043] Step (2) Preparation of magnetic particles
[0044] First, 0.5 g of hydrated ammonium ferrous sulfate, 0.5 g of hydrated ferric chloride (FeCl3·6H2O), and 5 g of basic copper carbonate of step (1) were weighed and dissolved in 100 mL of distilled water. The reaction temperature was controlled to be 2°C and stirred to obtain a mixed solution. Under argon protection, 2 g of hydrazine hydrate was weighed and slowly added dropwise to the mixed solution. The mixture was stirred for reaction for 1 hour and centrifuged to obtain a brown-black solid. The solid was washed with distilled water until the pH of the mixed solution was 7. The solid was then washed with anhydrous ethanol and dried to obtain a precursor FeO(OH). Then, 1 g of the precursor FeO(OH) was added to a hydrothermal reactor, 20 mL of 0.6% ammonia water was added, the mixture was reacted at 200°C for 24 hours, and the mixture was naturally cooled to room temperature. The reactant was taken out and centrifuged to obtain a black solid precipitate. The solid was repeatedly washed with distilled water until the pH of the solution was 7. The solid was once again washed with anhydrous ethanol and dried to obtain Fe3O4 particles.
[0045] Step (3) Preparation of benzoyl chloride
[0046] In a 250 mL three-necked flask equipped with a spherical condenser and a stirring device, add benzoic acid and benzyl chloride in a ratio of 1:1, then add 10 mL of deionized water, turn on the electric stirrer for stirring, and heat with an electric heating mantle. During heating, control the reaction temperature to be between 65°C. When no gas is generated, stop heating, absorb the tail gas with a NaOH solution, remove the spherical condenser and the stirring device, replace them with a fractionating device and connect it to a straight condenser, then add 10 g of the magnetic particles in step (2) and start heating. After heating for 40 min, cool to obtain benzoyl chloride;
[0047] Step (4) Preparation of diphenylmethane diisocyanate trimer (MDI)
[0048] In a dry four-necked flask equipped with a thermometer, a stirring paddle and a reflux condenser, 10 g of MDI, 5 g of ethyl acetate (EAC) and 20 mL of an antioxidant were added, and nitrogen was introduced for protection. Stirring was started, and the mixture was heated to 40° C. Deionized water was gradually added dropwise until 20 mL was reached. Then, 2 g of the inhibitor benzoyl chloride from step (3) was added to terminate the reaction, thereby obtaining diphenylmethane diisocyanate trimer (MDI);
[0049] Step (5) Preparation of slow rebound foam
[0050] First, weigh 4 g of quartz sand powder, 2 g of red phosphorus, and 5 g of polyether polyol respectively, put them together into a glass cup, stir them thoroughly with a glass rod, then add 5 g of diphenylmethane diisocyanate trimer (MDI) from step (4) and 20 mL of deionized water, stir them quickly with a glass rod for 1 min, and after mixing evenly, put them into a container and let them stand for 2 h to allow them to fully foam and set, thereby obtaining a slow-rebound foam.
[0051] Example 2
[0052] Step (1) Preparation of basic copper carbonate
[0053] The copper-based precursor and water are placed in a round-bottom flask in a ratio of 2:3, and the vacuum pump is used for filtration. The vacuum degree is controlled at 0.03 MPa, and the electric heating mantle is heated to 70°C. A three-stage absorption bottle is used to absorb the ammonia tail gas, and water is used as the tail gas absorption liquid. After the ammonia is evaporated, the solid is filtered and washed to obtain basic copper carbonate;
[0054] Step (2) Preparation of magnetic particles
[0055] First, 0.6 g of hydrated ammonium ferrous sulfate, 0.6 g of hydrated ferric chloride (FeCl3·6H2O), and 6 g of basic copper carbonate obtained in step (1) were weighed and dissolved in 110 mL of distilled water. The reaction temperature was controlled to be 3°C and stirred to obtain a mixed solution. Under argon protection, 3 g of hydrazine hydrate was weighed and slowly added dropwise to the mixed solution. The mixture was stirred for reaction for 2 h and centrifuged to obtain a brown-black solid. The solid was washed with distilled water until the pH of the mixed solution was 8. The solid was then washed with anhydrous ethanol and dried to obtain a precursor FeO(OH). Then, 2 g of the precursor FeO(OH) was added to a hydrothermal reactor, 30 mL of 0.7% ammonia water was added, the mixture was reacted at 300°C for 30 h, and the mixture was naturally cooled to room temperature. The reactant was taken out and centrifuged to obtain a black solid precipitate. The solid was repeatedly washed with distilled water until the pH of the solution was 8. The solid was once again washed with anhydrous ethanol and dried to obtain Fe3O4 particles.
[0056] Step (3) Preparation of benzoyl chloride
[0057] In a 300 mL three-necked flask equipped with a spherical condenser and a stirring device, add benzoic acid and benzyl chloride in a ratio of 2:2, then add 12 mL of deionized water, turn on the electric stirrer for stirring, and heat with an electric heating mantle. During heating, control the reaction temperature to be between 70°C. When no gas is generated, stop heating, absorb the tail gas with a NaOH solution, remove the spherical condenser and the stirring device, replace them with a fractionating device and connect it to a straight condenser, then add 11 g of the magnetic particles in step (2) and start heating. After heating for 45 min, cool to obtain benzoyl chloride;
[0058] Step (4) Preparation of diphenylmethane diisocyanate trimer (MDI)
[0059] In a dry four-necked flask equipped with a thermometer, a stirring paddle and a reflux condenser, 12 g of MDI, 6 g of ethyl acetate (EAC) and 25 mL of an antioxidant were added, and nitrogen was introduced for protection. Stirring was started, and the mixture was heated to 45° C. Deionized water was gradually added dropwise until the mixture reached 25 mL. Then, 3 g of the inhibitor benzoyl chloride from step (3) was added to terminate the reaction, thereby obtaining diphenylmethane diisocyanate trimer (MDI);
[0060] Step (5) Preparation of slow rebound foam
[0061] First, 5 g of quartz sand powder, 3 g of red phosphorus, and 7 g of polyether polyol were weighed respectively, and put into a glass cup together. After being fully stirred with a glass rod, 6 g of diphenylmethane diisocyanate trimer (MDI) in step (4) and 25 mL of deionized water were added, and the mixture was quickly stirred with a glass rod for 2 min. After being evenly mixed, the mixture was placed in a container and allowed to stand for 3 h to fully foam and set, thereby obtaining a slow-rebound foam.
[0062] Example 3
[0063] Step (1) Preparation of basic copper carbonate
[0064] The copper-based precursor and water are placed in a round-bottom flask in a ratio of 3:4, and the vacuum pump is used for filtration. The vacuum degree is controlled at 0.04 MPa, and the electric heating mantle is heated to 80°C. A three-stage absorption bottle is used to absorb the ammonia tail gas, and water is used as the tail gas absorption liquid. After the ammonia is evaporated, the solid is filtered and washed to obtain basic copper carbonate;
[0065] Step (2) Preparation of magnetic particles
[0066] First, 0.7 g of hydrated ammonium ferrous sulfate, 0.8 g of hydrated ferric chloride (FeCl3·6H2O), and 7 g of basic copper carbonate of step (1) were weighed and dissolved in 150 mL of distilled water. The reaction temperature was controlled to 5°C and stirred to obtain a mixed solution. Under argon protection, 4 g of hydrazine hydrate was weighed and slowly added dropwise to the mixed solution. The mixture was stirred and reacted for 4 h. The mixture was centrifuged to obtain a brown-black solid. The solid was washed with distilled water until the pH of the mixed solution was 12. The solid was then washed with anhydrous ethanol and dried to obtain a precursor FeO(OH). Then, 4 g of the precursor FeO(OH) was added to a hydrothermal reactor, and 40 mL of 0.8% ammonia water was added. The mixture was reacted at 400°C for 40 h. The mixture was naturally cooled to room temperature. The reactant was taken out and centrifuged to obtain a black solid precipitate. The solid was repeatedly washed with distilled water until the pH of the solution was 9. The solid was once again washed with anhydrous ethanol and dried to obtain Fe3O4 particles.
[0067] Step (3) Preparation of benzoyl chloride
[0068] In a 400 mL three-necked flask equipped with a spherical condenser and a stirring device, add benzoic acid and benzyl chloride in a ratio of 3:3, then add 15 mL of deionized water, turn on the electric stirrer for stirring, and heat with an electric heating mantle. During heating, control the reaction temperature to be between 80°C. When no gas is generated, stop heating, absorb the tail gas with a NaOH solution, remove the spherical condenser and the stirring device, replace them with a fractionating device and connect it to a straight condenser, then add 15 g of the magnetic particles in step (2) and start heating. After heating for 50 min, cool to obtain benzoyl chloride;
[0069] Step (4) Preparation of diphenylmethane diisocyanate trimer (MDI)
[0070] In a dry four-necked flask equipped with a thermometer, a stirring paddle and a reflux condenser, 15 g of MDI, 9 g of ethyl acetate (EAC) and 30 mL of an antioxidant were added, and nitrogen was introduced for protection. Stirring was started, and the mixture was heated to 45° C. Deionized water was gradually added dropwise until the mixture reached 30 mL. Then, 4 g of the inhibitor benzoyl chloride from step (3) was added to terminate the reaction, thereby obtaining diphenylmethane diisocyanate trimer (MDI);
[0071] Step (5) Preparation of slow rebound foam
[0072] First, weigh 6 g of quartz sand powder, 5 g of red phosphorus, and 10 g of polyether polyol respectively, put them into a glass cup, stir them thoroughly with a glass rod, then add 8 g of diphenylmethane diisocyanate trimer (MDI) from step (4) and 30 mL of deionized water, stir them quickly with a glass rod for 3 min, and after mixing evenly, put them into a container and let them stand for 4 h to fully foam and set, thereby obtaining a slow-rebound foam.
[0073] Example 4
[0074] Step (1) Preparation of basic copper carbonate
[0075] A copper-based precursor and water in a ratio of 4:5 are placed in a round-bottom flask, and a vacuum pump is used for filtration. The vacuum degree is controlled at 0.07 MPa, and the electric heating mantle is heated to 90°C. A three-stage absorption bottle is used to absorb ammonia tail gas, and water is used as the tail gas absorption liquid. After the ammonia is evaporated, the solid is filtered and washed to obtain basic copper carbonate;
[0076] Step (2) Preparation of magnetic particles
[0077] First, 0.9 g of hydrated ammonium ferrous sulfate, 0.9 g of hydrated ferric chloride (FeCl3·6H2O), and 9 g of basic copper carbonate of step (1) were weighed and dissolved in 200 mL of distilled water. The reaction temperature was controlled to be 5°C and stirred to obtain a mixed solution. Under argon protection, 5 g of hydrazine hydrate was weighed and slowly added dropwise to the mixed solution. The mixture was stirred and reacted for 5 h. The mixture was centrifuged to obtain a brown-black solid. The solid was washed with distilled water until the pH of the mixed solution was 15. The solid was then washed with anhydrous ethanol and dried to obtain a precursor FeO(OH). 5 g of the precursor FeO(OH) was then added to a hydrothermal reactor. 50 mL of 0.9% ammonia water was added. The mixture was reacted at 500°C for 48 h. The mixture was naturally cooled to room temperature. The reactant was taken out and centrifuged to obtain a black solid precipitate. The solid was repeatedly washed with distilled water until the pH of the solution was 10. The solid was once again washed with anhydrous ethanol and dried to obtain Fe3O4 particles.
[0078] Step (3) Preparation of benzoyl chloride
[0079] In a 500 mL three-necked flask equipped with a spherical condenser and a stirring device, add benzoic acid and benzyl chloride in a ratio of 5:5, then add 20 mL of deionized water, turn on the electric stirrer for stirring, and heat with an electric heating mantle. During heating, control the reaction temperature to be between 100°C. When no gas is generated, stop heating, absorb the tail gas with a NaOH solution, remove the spherical condenser and the stirring device, replace them with a fractionating device and connect it to a straight condenser, then add 20 g of the magnetic particles in step (2) and start heating. After heating for 60 min, cool to obtain benzoyl chloride;
[0080] Step (4) Preparation of diphenylmethane diisocyanate trimer (MDI)
[0081] In a dry four-necked flask equipped with a thermometer, a stirring paddle and a reflux condenser, 20 g of MDI, 10 g of ethyl acetate (EAC) and 40 mL of an antioxidant were added, and nitrogen was introduced for protection. Stirring was started, and the mixture was heated to 50° C. Deionized water was gradually added dropwise until the mixture reached 40 mL. Then, 5 g of the inhibitor benzoyl chloride from step (3) was added to terminate the reaction, thereby obtaining diphenylmethane diisocyanate trimer (MDI);
[0082] Step (5) Preparation of slow rebound foam
[0083] First, 8 g of quartz sand powder, 9 g of red phosphorus, and 14 g of polyether polyol were weighed respectively, put into a glass cup, and stirred thoroughly with a glass rod. Then, 9 g of diphenylmethane diisocyanate trimer (MDI) from step (4) and 40 mL of deionized water were added, and the mixture was quickly stirred for 4 min with a glass rod. After the mixture was evenly mixed, the mixture was placed in a container and allowed to stand for 5 h to fully foam and set, thereby obtaining a slow-rebound foam.
[0084] Comparative Example 1
[0085] Step (1) Preparation of basic copper carbonate
[0086] A copper-based precursor and water are placed in a round-bottom flask at a ratio of 9:10, and a vacuum pump is used for filtration. The vacuum degree is controlled to be 1 MPa, and the electric heating mantle is heated to 100°C. A three-stage absorption bottle is used to absorb ammonia tail gas, and water is used as the tail gas absorption liquid. After the ammonia is evaporated, the solid is filtered and washed to obtain basic copper carbonate;
[0087] Step (2) Preparation of benzoyl chloride
[0088] In a 600 mL three-necked flask equipped with a spherical condenser and a stirring device, add benzoic acid and benzyl chloride in a ratio of 6:7, then add 50 mL of deionized water, turn on an electric stirrer for stirring, and heat with an electric heating mantle. During heating, control the reaction temperature to be between 200 °C. When no gas is generated, stop heating, absorb the tail gas with a NaOH solution, remove the spherical condenser and the stirring device, replace them with a fractionating device and connect a straight condenser, then add 30 g of the basic copper carbonate prepared in step (1) and start heating. After heating for 90 min, cool to obtain benzoyl chloride;
[0089] Step (3) Preparation of diphenylmethane diisocyanate trimer (MDI)
[0090] In a dry four-necked flask equipped with a thermometer, a stirring paddle and a reflux condenser, 50 g of MDI, 30 g of ethyl acetate (EAC) and 55 mL of an antioxidant were added, and nitrogen was introduced for protection. Stirring was started, and the mixture was heated to 70° C. Deionized water was gradually added dropwise until the mixture reached 50 mL. Then, 9 g of the inhibitor benzoyl chloride from step (2) was added to terminate the reaction, thereby obtaining diphenylmethane diisocyanate trimer (MDI);
[0091] Step (4) Preparation of slow rebound foam
[0092] First, 11 g of quartz sand powder, 15 g of red phosphorus, and 18 g of polyether polyol were weighed respectively, and put into a glass cup together. After being fully stirred with a glass rod, 19 g of diphenylmethane diisocyanate trimer (MDI) in step (3) and 60 mL of deionized water were added, and the mixture was quickly stirred with a glass rod for 8 min. After being evenly mixed, the mixture was placed in a container and allowed to stand for 9 h to fully foam and set, thereby obtaining a slow-rebound foam.
[0093] Comparative Example 2
[0094] Step (1) Preparation of magnetic particles
[0095] First, 0.9 g of hydrated ammonium ferrous sulfate, 0.9 g of hydrated ferric chloride (FeCl3·6H2O), and 9 g of basic copper carbonate were weighed and dissolved in 350 mL of distilled water. The reaction temperature was controlled to 9 ° C. Stirring to obtain a mixed solution. Under argon protection, 9 g of hydrazine hydrate was weighed and slowly added dropwise to the mixed solution. The mixture was stirred for reaction for 9 h and centrifuged to obtain a brown-black solid. The solid was washed with distilled water until the pH of the mixed solution was 30. The solid was then washed with anhydrous ethanol and dried to obtain a precursor FeO(OH). Then, 7 g of the precursor FeO(OH) was added to a hydrothermal reactor, and 90 mL of 1% ammonia water was added. The mixture was reacted at 600 ° C for 50 h. The mixture was naturally cooled to room temperature. The reactant was taken out and centrifuged to obtain a black solid precipitate. The solid was repeatedly washed with distilled water until the pH of the solution was 20. The solid was washed with anhydrous ethanol again and dried to obtain Fe3O4 particles.
[0096] Step (2) Preparation of benzoyl chloride
[0097] In a 600 mL three-necked flask equipped with a spherical condenser and a stirring device, add benzoic acid and benzyl chloride in a ratio of 9:11, then add 70 mL of deionized water, turn on the electric stirrer for stirring, and heat with an electric heating mantle. During heating, control the reaction temperature to be between 150°C. When no gas is generated, stop heating, absorb the tail gas with a NaOH solution, remove the spherical condenser and the stirring device, replace them with a fractionating device and connect it to a straight condenser, then add 50 g of the magnetic particles in step (1) and start heating. After heating for 70 min, cool to obtain benzoyl chloride;
[0098] Step (3) Preparation of diphenylmethane diisocyanate trimer (MDI)
[0099] In a dry four-necked flask equipped with a thermometer, a stirring paddle and a reflux condenser, 50 g of MDI, 40 g of ethyl acetate (EAC) and 60 mL of an antioxidant were added, and nitrogen was introduced for protection. Stirring was started, and the mixture was heated to 90° C. Deionized water was gradually added dropwise until the mixture reached 80 mL. Then, 9 g of the inhibitor benzoyl chloride from step (2) was added to terminate the reaction, thereby obtaining diphenylmethane diisocyanate trimer (MDI);
[0100] Step (4) Preparation of slow rebound foam
[0101] First, 16 g of quartz sand powder, 20 g of red phosphorus, and 18 g of polyether polyol were weighed respectively, and put into a glass cup together. After being fully stirred with a glass rod, 10 g of diphenylmethane diisocyanate trimer (MDI) and 60 mL of deionized water were added, and the mixture was quickly stirred with a glass rod for 9 min. After being evenly mixed, the mixture was placed in a container and allowed to stand for 8 h to fully foam and set, thereby obtaining a slow-rebound foam.
[0102] Comparison of detection experiments:
[0103] The slow-rebound foams with magnetic effects obtained in Examples 1 to 4 and Comparative Examples 1 and 2 were tested. The specific testing method is as follows:
[0104] Magnetic performance analysis
[0105] Magnetic property analysis is a method used to analyze the magnetic properties of prepared materials. It tests the superparamagnetism in slow-rebound foam with magnetic effect. If the coercive force of Fe3O4 particles in the prepared material approaches 0, it means that the Fe3O4 particles in the prepared material have no hysteresis, and each particle is in a single domain state, showing good superparamagnetism and strong magnetism. If the coercive force of Fe3O4 particles in the prepared material does not approach 0, then on the contrary, the magnetism is not strong.
[0106] Foam air permeability analysis method
[0107] The foam air permeability analysis method is used to evaluate and analyze the air permeability of slow-rebound foam materials. It is very important for pillows and other bedding products that require good ventilation and comfort. The air permeability range is 100-1100mm. 3 ▪s -1 If the value is larger, it means that the air permeability of the prepared slow-rebound foam material is better. If the value is smaller, on the contrary, the air permeability is poor.
[0108] Opening performance test method
[0109] The open cell performance test method, also known as the compression recovery (fallback distance) of the foam, refers to the ability of the slow-recovery foam material to return to its original shape after being subjected to pressure. When the slow-recovery foam material is subjected to pressure, the shape will slowly deform and gradually return to its original shape after the pressure is removed.
[0110] The open-cell performance test method is closely related to the fallback distance of the foam. The numerical range of the fallback distance is 1-15 mm. The larger the fallback distance, the better the prepared slow-rebound foam material can restore its original shape after compression, and the better the rebound effect. The smaller the fallback distance, the worse the rebound effect.
[0111] Table 1 Magnetic properties analysis method
[0112] Example <![CDATA[M / (emu▪g -1 )]]> 1 1 2 5 3 15 4 25 Comparative Example 1 50 Comparative Example 2 55
[0113] As can be seen from Table 1, Example 1 is the best, while Comparative Example 2 is the worst. In Example 1, the coercive force is close to 0, indicating that the prepared Fe3O4 particles have a lower magnetic moment. Because the particle size is small, the magnetic moment of a single particle is relatively small, showing good superparamagnetism and strong magnetism. In Comparative Example 2, the coercive force is 55, indicating that the prepared Fe3O4 particles have a multi-domain structure, which increases the coercive force, reduces the superparamagnetism, and has poor magnetism.
[0114] Table 2 Foam air permeability analysis method
[0115] Example <![CDATA[Air permeability / (mm 3 ▪s -1 )]]> 1 1100 2 1000 3 900 4 800 Comparative Example 1 300 Comparative Example 2 100
[0116] As shown in Table 2, Example 1 is the best and Comparative Example 2 is the worst. In Example 1, the air permeability is 1100 mm 3 ▪s -1 The prepared foam molecular structure is good, indicating that the slow rebound foam material of Example 1 has good air permeability. In Comparative Example 2, the air permeability is 100mm 3 ▪s -1 , the molecular structure of the prepared foam material is poor, so the air permeability of the prepared slow-rebound foam material is poor.
[0117] Table 3 Opening performance test method
[0118] Example Falling distance / mm 1 13 2 12 3 11 4 10 Comparative Example 1 5 Comparative Example 2 4
[0119] As can be seen from Table 3, Example 1 is the best, and Comparative Example 2 is poor. In Example 1, the fall-back distance is 13 mm, indicating that the particle structure of the prepared slow-rebound foam material is more complete and the particle distribution is more uniform, so the prepared slow-rebound foam material has better rebound performance. In Comparative Example 2, the fall-back distance is 4 mm, indicating that the particle distribution of the prepared slow-rebound foam material is uneven. The uneven particle distribution will make the internal structure of the slow-rebound foam material inconsistent, resulting in poor compression recovery performance.
[0120] This specific embodiment is merely an explanation of the present invention and is not a limitation of the present invention. After reading this specification, those skilled in the art can make non-creative modifications to the present embodiment as needed, but they are protected by patent law as long as they are within the scope of the claims of the present invention.
Claims
1. A process for preparing slow-rebound foam with magnetic effect, characterized in that: include: Preparation of basic copper carbonate, preparation of magnetic particles, preparation of benzoyl chloride, preparation of diphenylmethane diisocyanate trimer (MDI), preparation of slow-rebound foam.
2. The process for preparing a slow-rebound foam with magnetic effect according to claim 1, characterized in that: Step (1) Preparation of basic copper carbonate A certain proportion of copper-based precursor and water are placed in a round-bottom flask, filtered by a vacuum pump, the vacuum degree is controlled, the electric heating jacket is heated at high temperature, ammonia tail gas is absorbed by a three-stage absorption bottle, water is used as the tail gas absorption liquid, and after the ammonia is evaporated, the solid is filtered and washed to obtain basic copper carbonate; Step (2) Preparation of magnetic particles First, weigh a small amount of hydrated ammonium ferrous sulfate and a small amount of hydrated ferric chloride (FeCl3·6H2O), and a certain amount of basic copper carbonate in step (1), dissolve them in distilled water, control the reaction temperature, stir, and obtain a mixed solution. Under argon protection, weigh hydrazine hydrate, slowly add it dropwise to the mixed solution, stir to react, centrifuge, and obtain a brown-black solid. Wash with distilled water until the pH value of the mixed solution is within a certain range, then wash with anhydrous ethanol and dry to obtain a precursor FeO(OH). Then add the precursor FeO(OH) to a hydrothermal autoclave, add a small amount of ammonia water, react at high temperature for a period of time, cool naturally to room temperature, take out the reactant, centrifuge, and obtain a black solid precipitate. Wash with distilled water repeatedly until the pH value of the solution is within a certain range, wash with anhydrous ethanol again and dry to obtain Fe3O4 particles. Step (3) Preparation of benzoyl chloride In a three-necked flask equipped with a spherical condenser and a stirring device, add benzoic acid and benzyl chloride in a certain proportion, then add deionized water, turn on an electric stirrer for stirring, and heat with an electric heating mantle. During heating, control the reaction temperature. When no gas is generated, stop heating. Absorb the tail gas with a NaOH solution. Remove the spherical condenser and the stirring device, replace them with a fractionating device and connect a straight condenser. Then add the magnetic particles in step (2) and start heating. After heating for a period of time, cool to obtain benzoyl chloride. Step (4) Preparation of diphenylmethane diisocyanate trimer (MDI) MDI, ethyl acetate (EAC), and an antioxidant were added to a dry four-necked flask equipped with a thermometer, a stirring paddle, and a reflux condenser, and nitrogen was introduced for protection. Stirring was started, heating was performed, and deionized water was gradually added dropwise. Then, the benzoyl chloride in step (3) was added as an inhibitor to terminate the reaction, thereby obtaining diphenylmethane diisocyanate trimer (MDI); Step (5) Preparation of slow rebound foam First, weigh a small amount of quartz sand powder, red phosphorus, and polyether polyol, put them into a glass cup, stir them thoroughly with a glass rod, then add the diphenylmethane diisocyanate trimer (MDI) and deionized water in step (4), stir them quickly with a glass rod, and after mixing evenly, put them into a container and let them stand to fully foam and set to obtain a slow-rebound foam.
3. The process for preparing a slow-rebound foam with magnetic effect according to claim 2, characterized in that: Step (1) Preparation of basic copper carbonate The copper-based precursor and water are placed in a round-bottom flask in a ratio of 1-5:2-5, and a vacuum pump is used for filtration, and the vacuum degree is controlled to be 0.01-0.08 MPa. The electric heating mantle is heated to 60-100° C., and a three-stage absorption bottle is used to absorb ammonia tail gas, and water is used as the tail gas absorption liquid. After the ammonia is evaporated, the solid is filtered and washed to obtain basic copper carbonate.
4. The process for preparing a slow-rebound foam with magnetic effect according to claim 3, characterized in that: Step (2) Preparation of magnetic particles First, weigh 0.5-1g of hydrated ammonium ferrous sulfate, 0.5-1g of hydrated ferric chloride (FeCl3·6H2O), and 5-10g of basic copper carbonate of step (1), dissolve them in 100-200mL of distilled water, control the reaction temperature to 2-5°C, stir to obtain a mixed solution, weigh 2-5g of hydrazine hydrate under argon protection, slowly add it dropwise to the mixed solution, stir the reaction for 1-5h, centrifuge to obtain a brown-black solid, wash with distilled water until the pH of the mixed solution is The reaction mixture is stirred for 24 hours at 200-500 ℃ for 24-48 hours, and then the mixture is washed with anhydrous ethanol and dried to obtain a precursor FeO(OH). Then 1-5 g of the precursor FeO(OH) is added to a hydrothermal kettle, and 20-50 mL of 0.6-1% ammonia water is added. The mixture is reacted at 200-500 ℃ for 24-48 hours, and then naturally cooled to room temperature. The reactant is taken out and centrifuged to obtain a black solid precipitate. The mixture is repeatedly washed with distilled water until the pH value of the solution is 7-10, and then washed with anhydrous ethanol and dried to obtain Fe3O4 particles.
5. The process for preparing a slow-rebound foam with magnetic effect according to claim 4, characterized in that: Step (3) Preparation of benzoyl chloride In a 250-500 mL three-necked flask equipped with a spherical condenser and a stirring device, add benzoic acid and benzyl chloride in a ratio of 1-5:1-5, then add 10-20 mL of deionized water, turn on an electric stirrer for stirring, and heat with an electric heating mantle. During heating, control the reaction temperature to be between 65-120° C. When no gas is generated, stop heating, absorb the tail gas with a NaOH solution, remove the spherical condenser and the stirring device, replace them with a fractionating device and connect it to a straight condenser, then add 10-20 g of the magnetic particles in step (2) and start heating. After heating for 40-60 min, cool to obtain benzoyl chloride.
6. The process for preparing a slow-rebound foam with magnetic effect according to claim 5, characterized in that: Step (4) Preparation of diphenylmethane diisocyanate trimer (MDI) In a dry four-necked flask equipped with a thermometer, a stirring paddle and a reflux condenser, add 10-20 g of MDI, 5-10 g of ethyl acetate (EAC), 20-40 mL of an antioxidant and introduce nitrogen protection, start stirring, heat to 40-50° C., gradually add deionized water dropwise until 20-50 mL is reached, and then add 2-5 g of the inhibitor benzoyl chloride in step (3) to terminate the reaction to obtain diphenylmethane diisocyanate trimer (MDI).
7. The process for preparing a slow-rebound foam with magnetic effect according to claim 6, characterized in that: Step (5) Preparation of slow rebound foam First, weigh 4-10 g of quartz sand powder, 2-10 g of red phosphorus, and 5-15 g of polyether polyol respectively, put them into a glass cup, stir them thoroughly with a glass rod, then add 5-10 g of diphenylmethane diisocyanate trimer (MDI) and 20-50 mL of deionized water in step (4), stir them quickly with a glass rod for 1-5 min, and after mixing evenly, put them into a container and let them stand for 2-5 h to fully foam and shape them, so as to obtain a slow-rebound foam.