Lignosulfonate rapid decolorization method and application thereof
Through a two-stage reaction method, hydrogen peroxide and sulfuric acid are used to generate chromophore reaction between peracetic acid and lignin sulfonate, which solves the problem of difficult decolorization of lignin sulfonate in the prior art, and achieves efficient decolorization and stability The dye dispersant effect is suitable for a variety of dye applications.
Patent Information
- Application Number
- CN202411078765.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-07
- Publication Date
- 2024-11-22
AI Technical Summary
The prior art is difficult to effectively decolorize lignin sulfonate, which causes it to affect dye brightness and fiber dyeing during dye dispersion, and the oxidation capacity of hydrogen peroxide is weak under acidic conditions, making it difficult to decompose efficiently.
Two-stage reaction method is adopted: the first stage reacts with hydrogen peroxide in aqueous ethanol to form acetic acid and sulfuric acid, and the second stage is generated by sulfuric acid catalyzing, which synergistically reacts with the chromophore of lignin sulfonate to achieve Quickly decolorize.
Improves the decolorization efficiency and yield of lignin sulfonate, reduces the contamination rate of fibers, and the dispersion and high temperature stability of dye dispersants after decolorization are basically the same as those of login, suitable for high saturation dyes and shallow Color textile dyeing.
Smart Images

Figure CN118994630A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of dye dispersants, and in particular to a method for quickly decolorizing lignin sulfonate and application thereof. Background Art
[0002] Disperse dyes account for the largest share of the global dye market, but because they are difficult to disperse in water, they require dispersants to improve their dispersibility in water. Dispersants need to have both hydrophilic and lipophilic groups, and commonly used dispersants are surfactants. Lignin sulfonate is the main component of pulping wastewater. Lignin sulfonate has excellent water solubility, which is conducive to the dispersion of disperse dyes in water. However, the dark color of lignin sulfonate is the main obstacle for it to be used as a dye dispersant, which not only affects the brightness of the dye itself, but also stains the fiber. Therefore, decolorization of industrial lignin sulfonate is one of the problems that need to be solved urgently.
[0003] Lignin sulfonate is a polymer containing aromatic rings that is abundant in nature. It is originally colorless in plants, and the source of the color of lignin sulfonate is that chromophores are introduced into the structure of lignin sulfonate during pulping and separation. The main chromophores are carbon-carbon double bonds, o-quinones, chalcone and other structures conjugated with aromatic rings. The auxochromophores are mainly phenolic hydroxyl, hydroxyl and carboxyl groups. The first two chromophores contribute most of the color of lignin sulfonate. Therefore, it is a feasible way to reduce the color of lignin sulfonate by removing the main chromophores and blocking the connection between the auxochromophores and the chromophores. The decolorization methods for lignin sulfonate currently mainly include oxidative decolorization, reductive decolorization and other decolorization methods.
[0004] So far, hydrogen peroxide has been favored by researchers as a mild green oxidant. Hydrogen peroxide can react under acidic and alkaline conditions. Hydrogen peroxide is often used in alkaline conditions because it is difficult to decompose hydrogen peroxide under acidic conditions, so its oxidizing ability is very weak. However, under alkaline conditions, due to OH - The presence of perhydroxyl anion HOO - The generation of H2O2 causes it to decompose too quickly and become unstable, resulting in ineffective decomposition of hydrogen peroxide. Summary of the invention
[0005] The purpose of the present invention is to provide a method for rapid decolorization of lignin sulfonate and its application. The decolorization method consists of two reaction stages: in the first stage, lignin sulfonate is degraded to produce acetic acid and a small amount of sulfuric acid; in the second stage, hydrogen peroxide and the acetic acid generated in the first stage are catalyzed by sulfuric acid to generate peracetic acid, and the peracetic acid can quickly react with the chromophore of lignin sulfonate. The decolorized lignin sulfonate of the present invention is used as a dye dispersant to reduce the contamination rate of fibers, and its dispersibility and high temperature stability are basically consistent with those of the original lignin.
[0006] In order to achieve the above object, the technical solution of the present invention is as follows:
[0007] In one aspect, the present invention provides a method for rapid decolorization of lignin sulfonate, the method comprising the following steps:
[0008] Step 1: dissolving lignin sulfonate in an ethanol aqueous solution, adding hydrogen peroxide to the solution, reacting at 150-200° C. for 30-90 minutes in a sealed reactor, cooling to room temperature, and then taking out the solution;
[0009] Step 2: Add hydrogen peroxide and a catalyst to the solution obtained in step 1, react at 70-90° C. for 20-60 minutes, and obtain decolorized lignin sulfonate after drying.
[0010] In step 1, the lignin sulfonate is derived from acid pulping waste liquor.
[0011] In the above technical solution, further, in step 1, the mass ratio of the lignin sulfonate to hydrogen peroxide is 20:1-60:1;
[0012] The mass ratio of the lignin sulfonate to the volume of the ethanol aqueous solution is 1g:5ml-1g:10mL, wherein the volume ratio of ethanol to water in the ethanol aqueous solution is 1:10-10:1.
[0013] In the above technical solution, further, in step 2, the mass ratio of hydrogen peroxide to lignin sulfonate is 1:3-1:12.
[0014] In the above technical solution, further, in step 2, the catalyst is sulfuric acid.
[0015] In the above technical solution, further, in step 2, the mass ratio of sulfuric acid to hydrogen peroxide is 1:2-1:3.
[0016] In the above technical solution, further, in step 2, the drying is rotary evaporation or freeze drying.
[0017] Another aspect of the present invention provides a use of the decolorized lignin sulfonate obtained by the above decolorization method as a dye dispersant.
[0018] The decolorization principle is:
[0019] The method of the present invention consists of two reaction stages: in the first stage, lignin sulfonate is degraded to produce acetic acid and a small amount of sulfuric acid; in the second stage, hydrogen peroxide and the acetic acid generated in the first stage are catalyzed by sulfuric acid to generate peracetic acid, and hydrogen peroxide and peracetic acid release HOO respectively. - , HO + ions, which react rapidly with the lignin chromophore under synergistic action.
[0020] The beneficial effects of the present invention are:
[0021] 1. The present invention proposes a novel decolorization method for lignin sulfonate, which consists of two reaction stages: in the first stage, lignin sulfonate is degraded to produce acetic acid and a small amount of sulfuric acid; in the second stage, hydrogen peroxide and the acetic acid generated in the first stage are catalyzed by sulfuric acid to generate peracetic acid, and hydrogen peroxide and peracetic acid release HOO and H2O2, respectively. - , HO + ions, the two can react quickly with the chromophore of lignin sulfonate under synergistic effect, and the decolorization efficiency of lignin sulfonate is higher and the yield is greater than that of using hydrogen peroxide alone under alkaline conditions.
[0022] 2. After decolorization, lignin sulfonate was used as a dye dispersant, which reduced the fiber contamination rate from 32.63% to 15.23%, a decrease of 17.4%. The dispersibility and high-temperature stability were basically the same as those of the original lignin sulfonate, indicating that decolorized lignin sulfonate can be used as a dispersant in the field of dyeing high-saturation dyes and light-colored textiles. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 The color comparison and UV spectrum of lignin sulfonate before and after bleaching in Example 1, a is before bleaching, b is UV spectrum;
[0024] Figure 2 is the change in particle size of the dye in Example 4 before and after high temperature treatment;
[0025] Figure 3 Comparison of the dispersibility of the dyes after treatment at 130°C in Example 4, a is the dye without any dispersant, b is the dye mixed with LS, and c is the dye mixed with LS2. DETAILED DESCRIPTION
[0026] The present invention is described in detail below with reference to the embodiments, but the embodiments of the present invention are not limited thereto. Obviously, the embodiments described below are only partial embodiments of the present invention. For those skilled in the art, other similar embodiments obtained without creative labor all fall within the protection scope of the present invention.
[0027] Unless otherwise specified, the materials used in the embodiments of the present invention can be obtained through commercial channels or prepared according to conventional methods well known to those skilled in the art.
[0028] The present invention provides a method for rapid decolorization of lignin sulfonate, comprising the following steps:
[0029] Step 1: dissolving lignin sulfonate in an ethanol aqueous solution, adding hydrogen peroxide to the solution, reacting at 150-200° C. for 30-90 minutes in a sealed reactor, cooling to room temperature, and then taking out the solution;
[0030] Step 2: Add hydrogen peroxide and a catalyst to the solution obtained in step 1, react at 70-90° C. for 20-60 minutes, and obtain decolorized lignin sulfonate after drying.
[0031] The raw material lignin sulfonate is recorded as LS, and the lignin obtained in the first stage (step 1) and the second stage (step 2) are recorded as LS1 and LS2 respectively. The reaction process is:
[0032]
[0033] Example 1
[0034] Step 1: Dissolve 2 g of lignin sulfonate in 20 mL of ethanol-water solution (the volume ratio of ethanol to water is 1:1), add 0.1 mL of 30 wt% hydrogen peroxide to the solution, put it into a 25 mL polytetrafluoroethylene tank, and then seal the reactor, set the oil bath temperature to 150 ° C, keep it for 30 minutes, cool it to room temperature, and then take out the solution;
[0035] Step 2: Add 0.5 mL of 30 wt% hydrogen peroxide and 0.036 mL of 98 wt% sulfuric acid to the solution of step 1, heat at 90°C for 30 min, and evaporate to dryness by rotary evaporation at 50°C to obtain decolorized lignin sulfonate.
[0036] The raw material lignin sulfonate is recorded as LS, and the lignin obtained in the first stage (step 1) and the second stage (step 2) are recorded as LS1 and LS2 respectively. The reaction process is:
[0037] Figure 1 (a) is a comparison photo of lignin sulfonate before and after decolorization. Figure 1 (b) is the spectral absorption curve of decolorized lignin sulfonate. The whiteness was tested using i1 pro spectrophotometer. The test results are shown in Table 1.
[0038] The whiteness of lignin sulfonate is calculated according to the following formula:
[0039] W=3.14·(mSRD)0.36-1.27
[0040] Wherein: W is the whiteness of lignin sulfonate; mSRD is the sum of the visible spectrum reflectance of lignin sulfonate.
[0041] Table 1 Whiteness values of lignin sulfonate before and after decolorization in Example 1
[0042] Test items LS <![CDATA[LS2]]> growth rate / % W 1.9161 3.9461 105.94
[0043] It can be seen from Table 1 that after the bleaching treatment, the whiteness of the lignin sulfonate increased from 1.9161 to 3.9461, and the whiteness of the lignin sulfonate increased by about 105.9%.
[0044] The quality of lignin sulfonate before and after bleaching treatment is shown in Table 2.
[0045] Table 2 The mass of lignin sulfonate before and after decolorization in Example 1
[0046] sample Weight(g) LS 2 <![CDATA[LS1]]> 1.834 <![CDATA[LS2]]> 1.496
[0047] It can be seen from Table 2 that the yield of lignin sulfonate is 74.8%.
[0048] Example 2
[0049] Step 1: Dissolve 2 g of lignin sulfonate in 10 mL of ethanol-water solution (the volume ratio of ethanol to water is 1:1), add 0.3 mL of 30 wt% hydrogen peroxide to the solution, put it into a 25 mL polytetrafluoroethylene tank, and then seal the reactor, set the oil bath temperature to 200 ° C, keep it for 30 minutes, cool it to room temperature, and then take out the solution;
[0050] Step 2: Add 2 mL of 30 wt% hydrogen peroxide and 0.144 mL of 98 wt% sulfuric acid to the solution of step 1, heat at 90°C for 30 min, and evaporate to dryness by rotary evaporation at 50°C to obtain decolorized lignin sulfonate.
[0051] The raw material lignin sulfonate is denoted as LS, and the lignin obtained in the first stage (step 1) and the second stage (step 2) are denoted as LS1 and LS2, respectively. The whiteness is tested using an i1 pro spectrophotometer, and the test results are shown in Table 3.
[0052] Table 3 Whiteness values of lignin sulfonate before and after decolorization in Example 2
[0053] Test items LS <![CDATA[LS2]]> growth rate / % W 1.9161 4.1147 114.74
[0054] It can be seen from Table 3 that after the bleaching treatment, the whiteness of the lignin sulfonate increased from 1.9161 to 4.1147, and the whiteness of the lignin sulfonate increased by about 114.74%.
[0055] The quality of lignin sulfonate before and after bleaching treatment is shown in Table 4.
[0056] Table 4 The mass of lignin sulfonate before and after decolorization in Example 2
[0057]
[0058]
[0059] It can be seen from Table 4 that the yield of lignin sulfonate is 66.2%.
[0060] Comparative Example 1
[0061] 2 g of lignin sulfonate was dissolved in 10 mL of deionized water, 2.3 mL of 30 wt% hydrogen peroxide was added to the solution, and the mixture was reacted at 90° C. for 120 min to obtain decolorized lignin sulfonate.
[0062] The whiteness was measured using the i1 pro spectrophotometer. The test results are shown in Table 5.
[0063] Table 5 Whiteness value before and after bleaching of comparative example 1
[0064] Test items Original lignin sulfonate Bleached lignin sulfonate growth rate / % W 1.9161 2.3536 23.6
[0065] Comparative Example 2
[0066] 2 g of lignin sulfonate was dissolved in 10 mL of deionized water, 2.3 mL of 30 wt% hydrogen peroxide was added to the solution, and the mixture was reacted at 90° C. for 48 hours to obtain decolorized lignin sulfonate.
[0067] The whiteness was tested using an i1 pro spectrophotometer. The test results are shown in Table 6.
[0068] Table 6 Whiteness value of comparative example 1 before and after bleaching
[0069] Test items Original lignin sulfonate Bleached lignin sulfonate growth rate / % Whiteness W 1.9161 4.1100 114.5%
[0070] It can be seen from Table 6 that, to achieve a similar decolorization effect using hydrogen peroxide alone, at least 48 hours of reaction are required.
[0071] The quality of lignin sulfonate before and after bleaching treatment is shown in Table 7.
[0072] Table 7 The quality of lignin sulfonate before and after decolorization in Comparative Example 2
[0073] sample Weight(g) Original lignin sulfonate 2.0 Bleached lignin sulfonate 0.4
[0074] It can be seen from Table 7 that most of the lignin sulfonate has been reduced, and the yield is only 20%.
[0075] Example 3
[0076] In order to test the effect of lignin sulfonate on the contamination rate of fiber, 0.1g of the decolorized lignin sulfonate sample obtained in Example 1 and Comparative Example 1 was added to 50ml volume to prepare a lignin dispersant solution with a concentration of 2g / L, and acetic acid was used to adjust the pH to 5.0. 25mL of the solution was added to a polytetrafluoroethylene tank together with a 5cm×5cm white polyester fiber textile, and then the tank was placed in a reactor for high temperature treatment; the temperature was raised to 130℃ at a heating rate of 30℃ / min and maintained for 30min, and the lignin dispersant solution was cooled to 85℃. Without adding dye, the white polyester fiber textile was cooked with a 2g / L lignin dispersant solution, and the white polyester fiber textile was used as a blank sample.
[0077] The spectral reflectance of polyester fiber was tested using an Xrite spectrometer, and the stain rate was calculated using the following formula:
[0078]
[0079] Where: R0 is the reflectance of the blank sample at 450nm; R i is the reflectivity of the sample at 450nm.
[0080] As shown in Table 8, the reflectivity of the bleached lignin sulfonate (LS2) at 450nm is significantly higher than that of the original lignin sulfonate (LS) at this time, indicating that the dyeing rate of LS2 on the fiber is significantly reduced, and the staining rate of polyester fiber is reduced from 32.63% to 15.23%, and the staining rate is reduced by 17.4%. This shows that the bleached lignin sulfonate can not only replace commercial lignin sulfonate as a dispersant for ordinary dyes, but also can be used for dyeing light and saturated color dyes.
[0081] Table 8 Reflectivity of polyester fiber at 450nm
[0082] Number of tests blank LS <![CDATA[LS2]]> 1 0.7583 0.5031 0.6432 2 0.7506 0.5194 0.6408 3 0.7603 0.5065 0.6395 Contamination rate / % -- 32.63 15.23
[0083] Example 4
[0084] In order to test the effect of lignin sulfonate on dye, m(dye) = 0.3333 g, m(lignin) = 0.5 g were weighed according to the mass ratio of m(dye): m(lignin) = 1:1.5, and distilled water was added to prepare a dye solution with a mass fraction of 16.67%. The solution was magnetically stirred (30±2°C) for 10 min, and placed in an ultrasonic machine for ultrasonication at 30±2°C for 30 min to obtain a dye dispersion for use.
[0085] (1) Determination of high temperature stability of disperse blue dye by lignin sulfonate before and after bleaching
[0086] Take 0.75 mL of the prepared dye dispersion and add it to a 250 mL volumetric flask to prepare a dye solution with a concentration of 0.5 g / L. Adjust the pH to 5.0 with glacial acetic acid. Take 30 mL of the dye solution with a concentration of 0.5 g / L and add it to a polytetrafluoroethylene tank and put it into a reactor for reaction. Heat it to 130 ° C, keep it warm for 30 minutes, then cool it to 85 ° C and take it out. Dilute the solution to 1 mg / L, and test the particle size change of the dye after high temperature treatment with a laser particle size analyzer.
[0087] Dyes will aggregate to a certain extent after boiling at high temperatures, so the particle size of dyes will increase after high temperature heating. In contrast, the particle size of dyes with good dispersion increases less. Figure 2 As shown, the particle size of the dye without lignin added increases the most, while the particle size of the dye with LS and LS2 added increases the least, and the particle sizes of the dye are basically the same. The dye with lignin sulfonate added after decolorization can still remain stable after high temperature heating, indicating that the decolorization process does not affect its dispersibility.
[0088] (2) Determination of dye dispersion
[0089] According to the HG / T3399-2001 standard, the dispersibility and stability of lignin sulfonate at high temperature were also tested. Weigh 0.50g of the mixture of lignin sulfonate and disperse blue dye into a 150mL beaker, add distilled water and stir to prepare a 100mL fixed volume solution, transfer the prepared mixture into a sealed tank and heat to 130℃, and keep it at this temperature for 30min.
[0090] Dispersion test: Lay a piece of filter paper flat on a surface dish, take 0.2mL of the dye suspension heated at high temperature, and drop it drop by drop at the center of the filter paper. After the dye solution is completely penetrated, drop another drop. It should be noted that each drop of liquid should be placed in the same position to allow it to diffuse naturally, and the dispersion level is evaluated by the diffusion diameter.
[0091] When the dye diffuses, a permeation ring is formed on the filter paper. The presence of the permeation ring indicates poor dispersion. This is because the dye tends to aggregate and cannot be dispersed as far as water. Use the "Dye Diffusion Performance Test Card" to evaluate the dye deposition in the center of the permeation ring and qualitatively evaluate the dye diffusion performance.
[0092] like Figure 3 As shown, the circles formed by the dye suspension without lignin sulfonate showed obvious edge gaps of about 5 mm ( Figure 3 a), the circle is downgraded to level 2 to 3 compared with the test card, which means that the dye alone is not suitable for staining. Figure 3 b and Figure 3c are the dye suspensions with LS and LS2 added, respectively. The two dyed circles are uniform, and no obvious edge separation is observed. Compared with the test card, both reach level 4 to 5, indicating that the dye dispersion is appropriate.
[0093] The above embodiments are only preferred embodiments of the present invention and are not intended to limit the implementation methods. The protection scope of the present invention shall be subject to the scope defined in the claims. Other different forms of changes or modifications may be made based on the above description. Obvious changes or modifications derived therefrom are still within the protection scope of the present invention.
Claims
1. A method for rapid decolorization of lignin sulfonate, characterized in that: The method comprises the following steps: Step 1: dissolving lignin sulfonate in an ethanol aqueous solution, adding hydrogen peroxide to the solution, reacting at 150-200° C. for 30-90 minutes in a sealed reactor, cooling to room temperature, and then taking out the solution; Step 2: Add hydrogen peroxide and a catalyst to the solution obtained in step 1, react at 70-90° C. for 20-60 minutes, and obtain decolorized lignin sulfonate after drying.
2. The method for rapid decolorization of lignin sulfonate according to claim 1, characterized in that: In step 1, the mass ratio of the lignin sulfonate to hydrogen peroxide is 20:1-60:1; The ratio of the mass of the lignin sulfonate to the volume of the ethanol aqueous solution is 1g:5ml-1g:10mL.
3. The method for rapid decolorization of lignin sulfonate according to claim 1, characterized in that: In step 2, the mass ratio of hydrogen peroxide to lignin sulfonate is 1:3-1:
12.
4. The method for rapid decolorization of lignin sulfonate according to claim 1, characterized in that: In step 2, the catalyst is sulfuric acid.
5. The method for rapid decolorization of lignin sulfonate according to claim 1, characterized in that: In step 2, the mass ratio of hydrogen peroxide to sulfuric acid is 1:2-1:
3.
6. The method for rapid decolorization of lignin sulfonate according to claim 1, characterized in that: In step 2, the drying is rotary evaporation or freeze drying.
7. Use of the decolorized lignin sulfonate obtained by the decolorization method according to any one of claims 1 to 6 as a dye dispersant.