Black or white vehicle film coated with TPU (thermoplastic polyurethane) and preparation method of black or white vehicle film
The coating process of the laminated structure is simplified to prepare TPU car film, solving the problems of complex processes and high costs in the existing technology, and achieving low-cost and convenient TPU car film production, with good tensile and aging resistance. Suitable for automotive surface use.
Patent Information
- Application Number
- CN202411096156.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-12
- Publication Date
- 2024-11-22
AI Technical Summary
The production process of existing TPU color-changing films is complex and costly, making it difficult to realize a simple and low-cost preparation method.
The coating process of a laminated structure includes a first release film layer, a color layer and a second release film layer, and the black or white organic coloring material and the TPU dissolved material are uniformly coated by extrusion spraying or comma scraping. Direct overlay to form a vehicle film, reducing the production process of TPU particles mixing and extrusion casting and simplifying the process flow.
It realizes the preparation of TPU vehicle membrane with simple process and low cost, has good tensile, toughness and aging resistance, can be easily fitted to the surface of the car, and is not prone to penetration or delamination problems, and has a long service life.
Smart Images

Figure CN118994670A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of automobile films, and in particular to a TPU black or white automobile film coated on an automobile body and a preparation method thereof. Background Art
[0002] With the popularity of vehicles, a car color-changing film has emerged on the market. It uses a film with rich and diverse colors to change the appearance of the entire car or part of it by covering it with a whole piece.
[0003] The existing color-changing films are mainly TPU color-changing films, which are first made into TPU film semi-finished products through a TPU film production process, and then made into color-changing film semi-finished products through a color-changing film production process, and then the TPU film semi-finished products are laminated on the surface of the color-changing film semi-finished products through a laminating film production process to make TPU color-changing film. The production process is complicated and the production material cost is relatively high.
[0004] In order to solve this problem, our company has developed a method for preparing TPU coated black or white vehicle film to solve the problems of complex process and high cost mentioned in the above background technology. Summary of the invention
[0005] In view of the above-mentioned deficiencies in the prior art, the present invention provides a method for preparing a TPU coated black or white vehicle film, which utilizes a black or white base color to block the penetration of the color of the vehicle paint itself.
[0006] A TPU coated black or white vehicle film comprises the following layers stacked in sequence:
[0007] The first release film layer has a thickness of 12 to 188 μm, preferably 12 to 125 μm, and more preferably 16 to 75 μm; the material of the first release film layer is one of TPU, TPH, PET or PP. The release film is a silicone release agent coated on the surface of the environmentally friendly material TPU, TPH, PET or PP film, so that it can show extremely light and stable release force for various organic pressure-sensitive adhesives. Different organic pressure-sensitive adhesives, such as hot melt adhesives, acrylic adhesives, and rubber system pressure-sensitive adhesives, etc., require different release forces of the release film. According to the different viscosities of the isolation product adhesive, the release force is adjusted accordingly by adjusting the tension control of the coating machine, so that it can achieve an extremely light and stable release force when peeling. Preferably, the material of the first release film layer is preferably PET.
[0008] The color layer has a thickness of 2 to 188 μm, preferably 12 to 155 μm, more preferably 20 to 100 μm, and even more preferably 50 to 55 μm; it is composed of any one or a combination of at least two of an organic colorant, an inorganic colorant, and a TPU soluble material;
[0009] The second release film layer has a thickness of 12 to 188 μm, preferably 12 to 125 μm, and more preferably 36 to 100 μm; the second release film layer is one of a PET film, a TPU film or a PU film.
[0010] Furthermore, the first release film layer and the second release film layer are both PET release film layers.
[0011] Furthermore, the color layer is made of black or white organic colorant or inorganic colorant mixed with TPU dissolved material, and the mixed colored TPU dissolved material is evenly coated on the first release film layer by extrusion spraying or comma scraping and laminated to form the color layer.
[0012] The method for preparing the above-mentioned TPU coated black or white vehicle film comprises the following steps:
[0013] (1) applying a layer of TPU black or white dissolved material or a mixed solution of black or white inorganic colorant and TPU dissolved material uniformly on the surface of the first release film layer by extrusion spraying or comma blade coating, and drying the mixture, so that the TPU black or white dissolved material or the mixed solution forms a color layer;
[0014] (2) Laminating a second release film layer on one side of the color layer through a coating process; wherein the second release film layer is a PET film, a TPU film or a PU film.
[0015] This preparation method eliminates the TPU particle mixing and TPU colorant particle mixing extrusion casting production process, and directly mixes black or white organic colorant or inorganic colorant with TPU dissolved material and evenly applies the mixed colored TPU dissolved material on the first release film layer by extrusion spraying or comma scraping and laminates it. The car film prepared by this method is simpler and has lower cost than the traditional TPU car film process.
[0016] Beneficial effects of the present invention: The process for coating the TPU black or white car film provided by the present invention is simple and low in cost. The characteristics of the TPU substrate are easy to stretch, large ductility, large shrinkage, and can be bent arbitrarily. It is easier to fit on the surface of the car during use and construction, and the construction is more convenient. It also has the characteristics of aging resistance. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 It is a schematic diagram of the cross-sectional structure of a vehicle film coated with TPU black or white in an embodiment of the present invention.
[0018] Explanation of reference numerals: 1-first release film layer, 2-color layer, 3-second release film layer. DETAILED DESCRIPTION
[0019] In order to more clearly illustrate the technical features, purposes and effects of the present invention, specific embodiments of the present invention are now described with reference to the accompanying drawings.
[0020] Example 1
[0021] See also Figure 1 In Example 1 of the present invention, a TPU coated black or white vehicle film is provided, which consists of a first release film layer 1, a color layer 2, and a second release film layer 3 from top to bottom.
[0022] The preparation steps of the TPU coated black or white vehicle film of the present invention are described in detail below:
[0023] (1) First, a black or white organic colorant or inorganic colorant and a TPU dissolving material are uniformly mixed to obtain a mixed solution, and a layer of the mixed solution is uniformly applied on the first release film layer 1 by extrusion spraying or comma coating and dried to form a colored color layer 2. Specifically, in the mixed solution, the amount of black or white organic colorant or inorganic colorant is 6 to 8 parts by weight, and the amount of TPU dissolving material is 100 parts by weight; the mixing method is stirring at room temperature, the stirring time at room temperature is 60±5min, the coating speed is 2 to 15m / min, the oven is seven sections, and the drying temperatures are 50°C, 60°C, 70°C, 80°C, 120°C, 140°C, and 150°C respectively (the temperature of each section of the oven can be adjusted by ±10°C according to the actual situation), and the thickness of the color layer 2 is 50μm; the thickness of the first release film layer 1 is 75μm;
[0024] (2) A layer of release film is coated on the surface of the dried TPU color layer through a coating process to form a second release film layer 3. The thickness of the second release film layer 3 is 50 μm.
[0025] It should be noted that the two smearing methods in the present invention are specifically as follows:
[0026] ① Extrusion spraying: Place the release film in the unwinding area of the coating machine, and adjust its tension until the film is completely flat. Deliver the colored mixed solution into the die head at a rate of 9L / min through a screw delivery pump, and spray it evenly on the release film through a slit extrusion die head (an adjustable gasket is installed on the slit extrusion die head to adjust the opening size of the nozzle. A large nozzle opening means a thick film layer, and a small nozzle opening means a thin film layer; and there is a speed control switch on the slit extrusion die head to adjust the spraying speed. A fast spraying speed means a thin film layer, and a slow spraying speed means a thin film layer. The film thickness is 300 μm, the nozzle size of the extrusion spraying used in the present invention is 300 μm, and then it is uniformly sent to the oven for drying at a speed of 5 m / min. The oven has seven sections, and the temperatures are 50°C, 60°C, 70°C, 80°C, 120°C, 140°C, and 150°C (the temperature can be ±10°C according to the actual situation). The TPU dissolved material contains a diluent component that can volatilize when heated. When the diluent in the TPU dissolved material is completely evaporated when heated, a colored color layer 2 is formed on the surface of the first release film layer 1 with the TPU dissolved material. The thickness of the color layer 2 after drying is 50 μm.
[0027] ②Comma scraping: Put the release film in the unwinding area of the coating machine, and adjust its tension until the film is completely flat. The colored mixed solution is quantitatively sent to the comma scraper material tank by a screw conveying pump at 9L / min, and evenly scraped onto the release film by comma scraping, wherein the distance between the scraper and the mirror roller is adjusted to control the thickness of the film layer, then the film layer is thicker when the distance is large, and thinner when the distance is small. The distance between the scraper and the mirror roller used in the present invention is 300μm, and the thickness is moderate. Then, it is uniformly sent to the oven for drying at a speed of 5m / min. The oven has seven sections, and the temperatures are 50℃, 60℃, 70℃, 80℃, 120℃, 140℃, and 150℃ (the temperature can be ±10℃ according to the actual situation). When the diluent is completely evaporated by heat, a colored color layer 2 is formed on the surface of the first release film layer 1 with TPU dissolved material. The thickness of the color layer 2 after drying is 50μm.
[0028] It should be noted that the PET release film used in the present invention does not deform when pulled under a tension of 250 to 300N.
[0029] Compared with the prior art, the TPU black or white car film coated in the present invention has the following advantages:
[0030] First, the car film can be pasted on the surface of the car body, and the color layer can effectively block external stains and corrosive substances, and will not penetrate the original paint color of the car body;
[0031] Second, the film layer is reasonably designed, with moderate thickness, high stretchability and strong toughness. It can fit closely to the surface of all curvatures of the car, and the car body color can be changed according to customer preferences. In extremely harsh temperatures, it will not crack or delaminate. The construction is simple, there will be no blistering or debonding during the film application process, and the service life is long.
[0032] Third, the manufacturing process of this method is simple, easy to mass-produce, and has low cost.
[0033] In this embodiment, a color-changing film with a length of 100 mm, a width of 25 mm, and a thickness of 0.18 mm was tested, and the test results are shown in Table 1 below.
[0034] Table 1 Performance test results of the car film in Example 1
[0035]
[0036] Example 2
[0037] The TPU coated black vehicle film provided in this embodiment includes a first release film layer 1, a color layer 2, and a second release film layer 3 which are overlapped in sequence from top to bottom.
[0038] The preparation steps of coating the TPU black vehicle film in this embodiment are similar to those in Example 1, specifically:
[0039] (1) First, a black organic colorant and a TPU dissolving material are uniformly mixed to obtain a mixed solution, wherein the amount of the black organic colorant is 6 parts by weight and the amount of the TPU dissolving material is 100 parts by weight, and then a layer of the mixed solution is uniformly applied on the first release film layer 1 by extrusion spraying or comma coating and dried to form a colored color layer 2. The mixing method is stirring at room temperature, the stirring time at room temperature is 60±5min, the coating speed is 2-15m / min, the oven is seven sections, and the drying temperatures are 50°C, 60°C, 70°C, 80°C, 120°C, 140°C, and 150°C respectively (the temperature of each section of the oven can be adjusted by ±10°C according to the actual situation). After drying, the color layer 2 is black, and the thickness of the color layer 2 is 50μm; the thickness of the first release film layer 1 is 16μm;
[0040] (2) A layer of release film is coated on the surface of the dried TPU color layer 2 through a coating process to form a second release film layer 3. The thickness of the second release film layer 3 is 36 μm.
[0041] Example 3
[0042] The TPU coated black vehicle film provided in this embodiment includes a first release film layer 1, a color layer 2, and a second release film layer 3 which are overlapped in sequence from top to bottom.
[0043] The preparation steps of coating the TPU black vehicle film in this embodiment are similar to those in Example 1, specifically:
[0044] (1) First, a black inorganic pigment and a TPU dissolving material are uniformly mixed to obtain a mixed solution, wherein the amount of the black inorganic pigment is 8 parts by weight and the amount of the TPU dissolving material is 100 parts by weight, and then a layer of the mixed solution is uniformly applied on the first release film layer 1 by extrusion spraying or comma coating and dried to form a colored color layer 2. The mixing method is stirring at room temperature, the stirring time at room temperature is 60±5min, the coating speed is 2-15m / min, the oven is seven sections, and the drying temperatures are 50°C, 60°C, 70°C, 80°C, 120°C, 140°C, and 150°C respectively (the temperature of each section of the oven can be adjusted by ±10°C according to the actual situation). After drying, the color layer 2 is black, and the thickness of the color layer 2 is 55μm; the thickness of the first release film layer 1 is 125μm;
[0045] (2) A layer of release film is coated on the surface of the dried TPU color layer 2 through a coating process to form a second release film layer 3. The thickness of the second release film layer 3 is 100 μm.
[0046] Example 4
[0047] The TPU coated white vehicle film provided in this embodiment includes a first release film layer 1, a color layer 2, and a second release film layer 3 which are overlapped in sequence from top to bottom.
[0048] The preparation steps of coating the TPU white vehicle film in this embodiment are similar to those in Example 1, specifically:
[0049] (1) First, a white inorganic pigment and a TPU dissolving material are uniformly mixed to obtain a mixed solution, wherein the amount of the white inorganic pigment is 8 parts by weight and the amount of the TPU dissolving material is 100 parts by weight, and then a layer of the mixed solution is uniformly applied on the first release film layer 1 by extrusion spraying or comma coating and dried to form a colored color layer 2. The mixing method is stirring at room temperature, the stirring time at room temperature is 60±5min, the coating speed is 2-15m / min, the oven is seven sections, and the drying temperatures are 50°C, 60°C, 70°C, 80°C, 120°C, 140°C, and 150°C respectively (the temperature of each section of the oven can be adjusted by ±10°C according to the actual situation). After drying, the color layer 2 is white, and the thickness of the color layer 2 is 75μm; the thickness of the first release film layer 1 is 125μm;
[0050] (2) A layer of release film is coated on the surface of the dried TPU color layer 2 through a coating process to form a second release film layer 3. The thickness of the second release film layer 3 is 75 μm.
[0051] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A TPU coated black or white car film, comprising a first release film layer, a color layer, and a second release film layer stacked in sequence, characterized in that: It includes the following layers stacked in sequence: (1) a first release film layer having a thickness of 12 to 188 μm; (2) Color layer, with a thickness of 2 to 188 μm; (3) A second release film layer having a thickness of 12 to 188 μm.
2. The TPU coated black or white vehicle film according to claim 1, characterized in that: The material of the first release film layer is TPU, TPH, PET or PP.
3. The TPU coated black or white vehicle film according to claim 1, characterized in that: The color layer is any one of an organic colorant, an inorganic colorant, and a TPU soluble material, or a combination of at least two of them. The thickness of the color layer after curing is 20-100 μm.
4. The TPU coated black or white vehicle film according to claim 1, characterized in that: The material of the second release film layer is PET, TPU or PU.
5. The TPU coated black or white vehicle film according to claim 3, characterized in that: The thickness of the first release film layer is 16-75 μm, the thickness of the color layer is 50-55 μm, and the thickness of the second release film layer is 36-100 μm.
6. The method for preparing a TPU coated black or white vehicle film according to claim 1, characterized in that: The following steps are involved: (1) applying a color layer of the mixed solution containing TPU black or white organic colorant or inorganic colorant and TPU dissolving material uniformly on the surface of the first release film layer by extrusion spraying or comma scraping, and drying the mixed solution to form a color layer; (2) Laminating a second release film layer on one side of the color layer through a coating process; wherein the second release film layer is a PET film, a TPU film or a PU film.
