Barrier explosion-proof polyurethane reticular foam material and preparation method thereof
By introducing MOF flame retardant materials and layered nanozirconium phosphate into polyurethane foam materials, the problems of high density and easy corrosion of traditional metal explosion-proof materials are solved, and a mesh foam material with low density and good explosion-proof effect is prepared, which is suitable for easy Transport and storage of explosive fluids.
Patent Information
- Application Number
- CN202411065127.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-05
- Publication Date
- 2024-11-22
AI Technical Summary
Traditional metal barrier explosion-proof materials have high density, heavy mass, are easily corrosive and costly, making it difficult to meet the transportation and storage safety needs of flammable and explosive fluids.
Develop a mesh polyurethane foam material prepared from polyols, TDI, foaming agents, crosslinking agents, catalysts, antistatic agents, antioxidants, flame retardants, synergists and fillers through MOF flame retardant materials and layers The combination of nano-zirconium phosphate improves the porosity, thermal stability and mechanical properties of the material.
The obtained flame-retardant explosion-proof mesh foam material has a low density and light weight, high porosity and good explosion-proof effect, and can replace metal materials and improve the safety and service life of the fuel tank.
Smart Images

Figure BDA0004979129120000061 
Figure BDA0004979129120000071
Abstract
Description
Technical Field
[0001] The present application relates to the field of organic barrier explosion-proof technology, and in particular to a barrier explosion-proof polyurethane reticulated foam material and a preparation method thereof. Background Art
[0002] There are certain dangers in the transportation and storage of liquid and gaseous fuels such as petroleum, propane, acetylene, ether, and flammable and explosive fluids, which are prone to explosion, thus causing certain harm to personal safety and the surrounding environment. After installing certain gap materials in the storage containers of these flammable and explosive fluids, the heat absorption and blocking effects of this material can effectively increase the safety of the container in accidents.
[0003] Traditional barrier explosion-proof materials are a kind of mesh material made of metal foil by cutting and stretching. However, traditional metal barrier explosion-proof materials also have certain disadvantages, such as relatively high density and heavy weight; they will react with certain organic solvents and then corrode them; in addition, the cost of metal materials is also relatively high.
[0004] The advantage of using reticulated polyurethane foam in fuel tanks is that the material contains 97% of space, occupies a small tank capacity, and the criss-crossing meridians in the reticulated polyurethane can reduce the sloshing of fuel, thereby preventing the generation and accumulation of static electricity; it is flame retardant and has a high specific surface area. The foam meridians can absorb oil mist to form an oil film, so that the fuel mixed vapor in the gaps between the meridians is in an oil-rich state, reducing the possibility of combustion and explosion. Therefore, the development of a reticulated polyurethane foam material with good barrier and explosion-proof properties for use in fuel tanks is of great significance for solving the transportation and storage of flammable and explosive fluids in this field. Summary of the invention
[0005] In order to solve the above technical problems, a reticulated polyurethane foam material with light weight and strong ability to suppress flame and explosion spread is developed. The present application provides a barrier explosion-proof polyurethane reticulated foam material and a preparation method.
[0006] In the first aspect, the present application provides a barrier and explosion-proof polyurethane reticulated foam material, comprising the following raw materials in parts by weight: 100 parts of polyol, 70-110 parts of TDI, 5-15 parts of foaming agent, 2-10 parts of cross-linking agent, 0.5-2 parts of catalyst, 5-10 parts of antistatic agent, 0.1-1 parts of foaming agent, 0.05-0.5 parts of antioxidant, 5-20 parts of flame retardant, 6-11 parts of synergist, 2-3 parts of colorant, and 2-4 parts of filler; the flame retardant is a MOF flame retardant material, and the MOF flame retardant material is made of a phosphorus-nitrogen flame retardant and MOF; the synergist is vanillin.
[0007] Furthermore, the polyol includes polyether polyol and polymer polyol, and the polyether polyol includes a first polyether polyol and a second polyether polyol.
[0008] Furthermore, the first polyether polyol is a propylene oxide-ethylene oxide copolyether having a hydroxyl value of 80-150 mgKOH / g, the second polyether polyol is a propylene oxide polyether polyol having a hydroxyl value of 300-600 mgKOH / g, and the polymer polyol is one or more of polyethylene adipate, polyneopentyl adipate, polyneopentyl succinate, polybutylene succinate, polybutylene isophthalate or polyneopentyl isophthalate.
[0009] By adopting the above technical scheme, in the present application, the pores of the polyurethane reticulated foam material obtained by foaming and reticulating a specific type of polyether polyol, polymer polyol and TDI (toluene diisocyanate) are uniform, the open-cell degree is good, and the porosity is high. The polyurethane reticulated foam material is modified using MOF flame retardant material, which is prepared by phosphorus nitrogen flame retardant and MOF reaction, and the surface of MOF flame retardant material contains a large amount of active chemical groups such as amino and hydroxyl groups, which can enhance the combination of MOF flame retardant material and polyurethane reticulated foam matrix material, and the reticulated polyurethane matrix material also has a good reinforcement effect. MOF material, with its highly ordered pore structure and large specific surface area, can form a uniform flame retardant network in the foam material, which helps to improve the thermal stability of the reticulated polyurethane matrix material. In addition, vanillin is used as a synergist. The aldehyde group in vanillin and the amine group in the MOF flame retardant material can form a polymer containing a Schiff base structure. The Schiff base structure also has high thermal stability. The aldehyde group in vanillin can also bond with active groups such as hydroxyl groups in the polyurethane matrix material, which can further improve the mechanical properties of the prepared polyurethane reticulated foam material, thereby improving its barrier and explosion suppression properties.
[0010] Furthermore, the raw materials of the MOF flame retardant material include a phosphorus-nitrogen flame retardant and MOF in a weight ratio of 1:1.5-2.5.
[0011] Furthermore, the raw materials of the MOF include metal salts, organic ligand molecules, solvents and organic acids, the metal salts include one of zinc acetate dihydrate, aluminum nitrate nonahydrate, iron nitrate nonahydrate and cobalt nitrate hexahydrate, and the organic ligand molecules are 2-amino-p-dibenzoic acid.
[0012] Furthermore, the preparation method of the MOF flame retardant material comprises the following steps: 1) Add metal salt, organic ligand molecule, solvent and organic acid into a hydrothermal reactor, heat to 160-190°C, stir to react, centrifuge, wash with solvent several times, and dry to obtain MOF; 2) Dispersing the phosphorus-nitrogen flame retardant and MOF in a solvent, heating to reflux, cooling, centrifuging the product, washing with a solvent several times, and drying to obtain a MOF flame retardant material.
[0013] Furthermore, the catalyst is an amine catalyst or an organic metal catalyst.
[0014] Specifically, the amine catalyst includes one or more of triethylenediamine, triethylamine, ethanolamine, triethanolamine, diethylenetriamine, dimethylbenzylamine, and dimethylhexadecylamine.
[0015] Specifically, the organic metal catalyst includes one or more of stannous octoate, dibutyltin dilaurate, and dibutyltin dioctanoate.
[0016] Furthermore, the filler is layered nano zirconium phosphate.
[0017] By adopting the above technical solution, layered nano zirconium phosphate is evenly dispersed in the foam matrix as a reinforcing material, and has strong thermal stability and corrosion resistance. It can be combined with MOF flame retardant materials in the polyurethane matrix material to enhance the matrix strength of the foam material. When the polyurethane matrix material is damaged, it can still serve as a skeleton to maintain the hollow structure of the foam material, thereby improving the barrier performance and service life of the product.
[0018] In a second aspect, the present application provides a method for preparing the above-mentioned barrier explosion-proof polyurethane reticulated foam material, comprising the following steps: S1, placing polyols in a reaction container and stirring to obtain a polyol mixture, adding a foaming agent, a foaming agent, a cross-linking agent, an antistatic agent, a flame retardant, an antioxidant, a colorant, and a filler to the polyol mixture, stirring at a constant temperature to obtain a mixed solution a; S2, adding a catalyst and a synergist to the mixed solution a obtained in step S1, stirring at a constant temperature, to obtain an intermediate solution b; S3, adding TDI to the intermediate solution b obtained in step S2 to obtain a mixed solution c, stirring, and stirring until the mixed solution c becomes milky white, and continuing to stir until it begins to foam. At this time, pour the mixed solution into a mold or template for curing, demoulding, and maturing to obtain a polyurethane soft foam; S4, reticulating the polyurethane foam obtained in step S3 by an explosion method to obtain a flame retardant and explosion-proof reticulated foam material.
[0019] In summary, the present invention includes at least one of the following beneficial technical effects: The flame retardant and explosion-proof reticulated foam material prepared in the present application has high porosity, uniform pores, and a good degree of opening. It has the advantages of low density, light weight, and good barrier and explosion-proof effect. The material can replace metal barrier and explosion-proof materials and is widely used in various fuel tanks and tanks to play a safety role in barrier and explosion-proof. DETAILED DESCRIPTION
[0020] The present application designs a barrier and explosion-proof polyurethane reticulated foam material, comprising the following raw materials in parts by weight: 100 parts of polyol, 70-110 parts of TDI, 5-15 parts of blowing agent, 2-10 parts of cross-linking agent, 0.5-2 parts of catalyst, 5-10 parts of antistatic agent, 0.1-1 parts of foaming agent, 0.05-0.5 parts of antioxidant, 5-20 parts of flame retardant, 6-11 parts of synergist, 2-3 parts of colorant, and 2-4 parts of filler; the flame retardant is a MOF flame retardant material, and the MOF flame retardant material is prepared by reacting a phosphorus-nitrogen flame retardant and MOF; the synergist is vanillin.
[0021] The barrier explosion-proof polyurethane reticulated foam material of the present application is prepared by the following method, comprising the following steps: S1, placing polyols in a reaction container and stirring to obtain a polyol mixture, adding a foaming agent, a foaming agent, a cross-linking agent, an antistatic agent, a flame retardant, an antioxidant, a colorant, and a filler to the polyol mixture, stirring at a constant temperature to obtain a mixed solution a; S2, adding a catalyst and a synergist to the mixed solution a obtained in step S1, stirring at a constant temperature, to obtain an intermediate solution b; S3, adding TDI to the intermediate solution b obtained in step S2 to obtain a mixed solution c, stirring, and stirring until the mixed solution c becomes milky white, and continuing to stir until it begins to foam. At this time, pour the mixed solution into a mold or template for curing, demoulding, and maturing to obtain a polyurethane soft foam; S4, reticulating the polyurethane foam obtained in step S3 by an explosion method to obtain a flame retardant and explosion-proof reticulated foam material.
[0022] The technical problem solved by the present application is that traditional metal barrier explosion-proof materials also have the disadvantages of high density, heavy weight and easy corrosion. The reticulated polyurethane foam material prepared in the present application has low density, light weight and good barrier explosion-proof effect. It is used in fuel tanks, which is of great significance for solving the transportation and storage of flammable and explosive fluids.
[0023] The present application is further described in detail below in conjunction with specific embodiments.
[0024] Example 1 The barrier explosion-proof polyurethane reticulated foam material in Example 1 comprises the following raw materials in parts by weight: 100 parts of polyol, 70 parts of TDI, 15 parts of blowing agent, 2 parts of cross-linking agent, 0.5 parts of catalyst, 5 parts of antistatic agent, 1 part of foam leveling agent, 0.05 parts of antioxidant, 5 parts of flame retardant, 6 parts of synergist, 2 parts of colorant and 4 parts of filler.
[0025] In Example 1, the polyol includes 20 parts of propylene oxide-ethylene oxide copolyether, 50 parts of propylene oxide polyether polyol and 30 parts of polyneopentyl adipate. Among them, the propylene oxide-ethylene oxide copolyether uses the Wanhua Chemical F3135 model, the hydroxyl value is 35 mgKOH / g, and the molecular weight is 4800, the propylene oxide polyether polyol uses the Tianjin Sanshihua Company 450L model, the hydroxyl value is 350 mgKOH / g, and the polyneopentyl adipate is purchased from Delta Biological Reagent Company.
[0026] In Example 1, TDI is TDI 80 / 20; the blowing agent is difluorodichloromethane; the cross-linking agent is triethanolamine; the catalyst is a mixture of stannous octoate and dibutyltin dilaurate in a weight ratio of 1:1; the antistatic agent is aluminum powder; the foaming agent is SH-431; the antioxidant is Irganox1010; the synergist is vanillin purchased from Nanjing Bermuda with a CAS number of 121-33-5; the filler is layered nano zirconium phosphate purchased from Fujian Ruisen New Materials; the colorant is titanium dioxide purchased from NR9503 titanium dioxide of Jinpu Titanium Industry.
[0027] The flame retardant in Example 1 is a MOF flame retardant material, which is prepared from a phosphorus-nitrogen flame retardant and MOF; wherein the phosphorus-nitrogen flame retardant is melamine cyclophosphate, CAS: 15541-60-3. The preparation process of the MOF flame retardant in Example 1 includes the following steps: 1) Add zinc acetate dihydrate, 2-amino-p-dibenzoic acid, DMF solvent and terephthalic acid in a weight ratio of 1:1.5:30:12 into a hydrothermal reactor, heat to 180°C, stir to react for 10 hours, cool to room temperature, centrifuge, wash and dry to obtain MOF; 2) Dispersing melamine cyclophosphate and MOF in a weight ratio of 1:2 in a methanol solvent, heating to 80° C., reflux for 12 h, cooling, centrifuging, washing, and drying the product to obtain a MOF flame retardant material.
[0028] The method for preparing the barrier explosion-proof polyurethane reticulated foam material in Example 1 comprises the following steps: S1. Place polyol in a reaction container and stir at 10° C. to obtain a polyol mixture, add a homogenizing agent, a foaming agent, a cross-linking agent, an antistatic agent, a flame retardant, an antioxidant, a colorant, and a filler to the polyol mixture, and stir at a constant temperature of 10° C. for 20 minutes to obtain a mixed solution a; S2, adding the catalyst and the synergist to the mixed solution a obtained in step S1, stirring at a constant temperature of 10° C. for 20 min, to obtain an intermediate solution b; S3, adding TDI to the intermediate liquid b obtained in step S2 to obtain a mixed liquid c, stirring at a constant temperature of 10°C, until the mixed liquid c turns milky white, maintaining the temperature at 10°C and continuing to stir until it starts to foam, then pouring the mixed liquid into a mold for curing, demoulding, and maturing to obtain a polyurethane soft foam; S4, reticulating the polyurethane soft foam obtained in step S3 by an explosion method to obtain a flame retardant and explosion-proof reticulated foam material.
[0029] Example 2 Embodiment 2 is based on Embodiment 1, except that: The barrier explosion-proof polyurethane reticulated foam material in Example 2 comprises the following raw materials in parts by weight: 100 parts of polyol, 85 parts of TDI, 9 parts of blowing agent, 7 parts of cross-linking agent, 1.5 parts of catalyst, 7 parts of antistatic agent, 0.5 parts of foaming agent, 0.3 parts of antioxidant, 14 parts of flame retardant, 9 parts of synergist, 2.5 parts of colorant and 3.5 parts of filler.
[0030] Example 3 Embodiment 3 is based on Embodiment 1, except that: The barrier explosion-proof polyurethane reticulated foam material in Example 3 comprises the following raw materials in parts by weight: 100 parts of polyol, 110 parts of TDI, 5 parts of blowing agent, 10 parts of cross-linking agent, 2 parts of catalyst, 10 parts of antistatic agent, 0.1 parts of foam leveling agent, 0.5 parts of antioxidant, 20 parts of flame retardant, 11 parts of synergist, 3 parts of colorant and 2 parts of filler.
[0031] Example 4 Example 4 is based on Example 2, except that the polyol in Example 4 includes 10 parts of propylene oxide-ethylene oxide copolyether, 40 parts of propylene oxide polyether polyol and 50 parts of polyneopentyl adipate.
[0032] Example 5 Example 5 is based on Example 2, except that the polyol in Example 5 includes 40 parts of propylene oxide-ethylene oxide copolyether, 40 parts of propylene oxide polyether polyol and 20 parts of polyneopentyl adipate.
[0033] Example 6 Example 6 is based on Example 2, except that the polyol in Example 6 includes 20 parts of propylene oxide-ethylene oxide copolyether, 50 parts of propylene oxide polyether polyol and 30 parts of polybutylene succinate. Among them, the propylene oxide-ethylene oxide copolyether adopts Wanhua Chemical A210, with a functionality of 2, a hydroxyl value of 112 mgKOH / g, and a molecular weight of 1000; the polymer polyol is polybutylene succinate, purchased from Aladdin Chemical Reagent Company, product number P341826.
[0034] Example 7 Example 7 is based on Example 2, except that the phosphorus-nitrogen flame retardant used to prepare the MOF flame retardant material in Example 7 is replaced by an equal amount of melamine cyclophosphate with ammonium polyphosphate (APP-0S giant ammonium phosphate purchased from Shandong Xinda Chemical).
[0035] Embodiment 8-9 Example 8 is based on Example 2, except that the amount of the flame retardant in Example 8 is changed to 10 parts by weight, and the amount of the filler is changed to 4 parts by weight.
[0036] Example 9 is based on Example 2, except that the amount of the flame retardant in Example 9 is changed to 13 parts by weight, and the amount of the filler is changed to 1 part by weight.
[0037] Comparative Example 1 Comparative Example 1 is based on Example 2, except that no synergist is added in Comparative Example 1.
[0038] Comparative Example 2 Comparative Example 2 is based on Example 2, except that the amount of flame retardant in Comparative Example 2 is changed to 25 parts by weight.
[0039] Performance Testing 1. The flame retardant properties of the barrier and explosion-proof polyurethane reticulated foam materials prepared in Examples 1-9 and Comparative Examples 1-2 were determined with reference to standard GB / T 2406.2-2009 "Determination of Combustion Performance of Plastics Part 2: Oxygen Index Method".
[0040] 2. Determine the density of the barrier and explosion-proof polyurethane reticulated foam materials prepared in Examples 1-9 and Comparative Examples 1-2.
[0041] 3. The volume resistivity (Ω·cm) of the barrier and explosion-proof polyurethane reticulated foam materials prepared in Examples 1-9 and Comparative Examples 1-2 was determined with reference to Standard GJB8455-2015 "General Technical Specifications for Barrier and Explosion-Proof Materials for Filling Oil Tanks and Oil Tanks".
[0042] 4. The tensile strength of the barrier and explosion-proof polyurethane reticulated foam materials prepared in Examples 1-9 and Comparative Examples 1-2 was determined with reference to the standard GB / T6344-2008, and the tear strength of the barrier and explosion-proof polyurethane reticulated foam materials prepared in Examples 1-9 and Comparative Examples 1-2 was determined with reference to the standard GB / T10808-2006.
[0043] 5. Shock tube test: According to the industry standard "AQ3001-2005" (Technical requirements for barrier explosion-proof storage tanks for automobile gas stations, light fuel and liquefied petroleum gas-tank trucks), a one-dimensional horizontal shock tube was used to measure the explosion boost value of the barrier explosion-proof polyurethane reticulated foam material prepared in Examples 1-9 and Comparative Examples 1-2. The oil vapor concentration in the test was 4.5% and the ignition energy was about 100J.
[0044] The test results are shown in Table 1.
[0045] Table 1 By analyzing the data in Table 1, it can be obtained by comparing Examples 1-9 with Comparative Examples 1-2 that the barrier and explosion-proof polyurethane reticulated foam material prepared in the present application has the characteristics of low density, good mechanical strength and good barrier and explosion-proof effect. By comparing Example 2 with Examples 8-9, it can be obtained that the weight ratio of the flame retardant to the filler has a certain influence on the density, volume resistivity and mechanical strength of the polyurethane reticulated foam material. By comparing Examples 1-9 with Comparative Examples 1-2, it can be obtained that the addition of the synergist and the addition and dosage of the flame retardant have an influence on the flame retardancy, density and mechanical strength of the polyurethane reticulated foam material, thereby further affecting the explosion-proof performance of the polyurethane reticulated foam material.
[0046] The above are all preferred embodiments of the present application, and the protection scope of the present application is not limited thereto. Therefore, any equivalent changes made according to the structure, shape, and principle of the present application should be included in the protection scope of the present application.
Claims
1. A barrier explosion-proof polyurethane reticulated foam material, It is characterized in that The invention comprises the following raw materials in parts by weight: 100 parts of polyol, 70-110 parts of TDI, 5-15 parts of foaming agent, 2-10 parts of cross-linking agent, 0.5-2 parts of catalyst, 5-10 parts of antistatic agent, 0.1-1 parts of foam leveling agent, 0.05-0.5 parts of antioxidant, 5-20 parts of flame retardant, 6-11 parts of synergist, 2-3 parts of colorant and 2-4 parts of filler; The flame retardant is a MOF flame retardant material, and the MOF flame retardant material is made of a phosphorus-nitrogen flame retardant and MOF; The synergist is vanillin.
2. The barrier explosion-proof polyurethane reticulated foam material according to claim 1, It is characterized in that The polyol includes a polyether polyol and a polymer polyol, and the polyether polyol includes a first polyether polyol and a second polyether polyol.
3. The barrier explosion-proof polyurethane reticulated foam material according to claim 2, It is characterized in that The first polyether polyol is propylene oxide-ethylene oxide copolyether, the second polyether polyol is propylene oxide polyether polyol, and the polymer polyol is one or more of polyethylene adipate, polyneopentyl adipate, polyneopentyl succinate, polybutylene succinate, polybutylene isophthalate or polyneopentyl isophthalate.
4. The barrier explosion-proof polyurethane reticulated foam material according to claim 1, It is characterized in that The raw materials of the MOF flame retardant material include a phosphorus-nitrogen flame retardant and MOF in a weight ratio of 1:1.5-2.
5.
5. The barrier explosion-proof polyurethane reticulated foam material according to claim 1, It is characterized in that The raw materials of the MOF include metal salt, organic ligand molecule, solvent and organic acid, the metal salt includes one of zinc acetate dihydrate, aluminum nitrate nonahydrate, iron nitrate nonahydrate and cobalt nitrate hexahydrate, and the organic ligand molecule is 2-amino-p-dibenzoic acid.
6. The barrier explosion-proof polyurethane reticulated foam material according to claim 5, It is characterized in that The preparation method of the MOF flame retardant material comprises the following steps: 1) Add metal salt, organic ligand molecule, solvent and organic acid into a hydrothermal reactor, heat to 160-190°C, stir to react, centrifuge, wash with solvent several times, and dry to obtain MOF; 2) Dispersing the phosphorus-nitrogen flame retardant and MOF in a solvent, heating to reflux, cooling, centrifuging the product, washing with a solvent several times, and drying to obtain a MOF flame retardant material.
7. The barrier explosion-proof polyurethane reticulated foam material according to claim 1, It is characterized in that The catalyst is an amine catalyst or an organic metal catalyst.
8. The barrier explosion-proof polyurethane reticulated foam material according to claim 1, It is characterized in that The filler is layered nano zirconium phosphate.
9. A method for preparing the barrier explosion-proof polyurethane reticulated foam material according to any one of claims 1 to 8, It is characterized in that The following steps are involved: S1, placing polyols in a reaction container and stirring to obtain a polyol mixture, adding a foaming agent, a foaming agent, a cross-linking agent, an antistatic agent, a flame retardant, an antioxidant, a colorant, and a filler to the polyol mixture, stirring at a constant temperature to obtain a mixed solution a; S2, adding a catalyst and a synergist to the mixed solution a obtained in step S1, stirring at a constant temperature, to obtain an intermediate solution b; S3, adding TDI to the intermediate solution b obtained in step S2 to obtain a mixed solution c, stirring, and stirring until the mixed solution c becomes milky white, and continuing to stir until it begins to foam. At this time, pour the mixed solution into a mold or template for curing, demoulding, and maturing to obtain a polyurethane soft foam; S4, reticulating the polyurethane foam obtained in step S3 by an explosion method to obtain a flame retardant and explosion-proof reticulated foam material.