Preparation method of biocompatible porous BC / CS composite material

By using magnetic stirring and low-temperature water bath technology under mild conditions, the problems of high preparation costs of existing porous materials and uneven distribution of chitosan were solved, and biocompatible porous BC/CS composite materials suitable for large-scale production were prepared. The effect of high porosity and high liquid absorption is achieved.

CN118994715APending Publication Date: 2024-11-22XIAN UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411290430.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-14
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

Existing methods for preparing porous materials require high temperature and high pressure environments, which lead to high cost and unsuitable for large-scale production, and the distribution of chitosan in the material is uneven.

Method used

A magnetic mixer stirs bacterial cellulose and chitosan under mild conditions. Through pretreatment, oxidation treatment and compounding steps, ensure uniform distribution of chitosan. A biocompatible porous BC/ is prepared using a low-temperature water bath and freeze-drying process. CS composite material.

Benefits of technology

It realizes the preparation of porous materials with high porosity and high liquid absorption under mild conditions, which is cheap, simple in process, suitable for large-scale production, and improves the biocompatibility and stability of the materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118994715A_ABST
    Figure CN118994715A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a biocompatible porous BC / CS composite material, which comprises the following steps: by taking low-cost bacterial cellulose BC obtained by fermenting coconut product byproducts and chitosan CS produced from aquatic waste shrimp and crab shells as raw materials, and sodium periodate NaIO4 as an oxidant, reacting in a weak acid reaction system to prepare the biocompatible porous BC / CS composite material. The porous BC / CS composite material can be obtained only through low-temperature water bath and then freeze drying; according to the method, two common polysaccharide materials serve as raw materials, the cost is low, the process is simple, reproducibility is good, stability is high, the method is suitable for large-scale production, and the porous BC / CS composite material prepared through the method has the advantages of being high in porosity, high in liquid absorption rate and good in biocompatibility and has wide application prospects in the field of biological medical materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of biomedical materials, and in particular relates to a method for preparing a biocompatible porous BC / CS composite material. Background Art

[0002] Porous materials are materials with special structures, and they have significant advantages in hemostasis, mainly reflected in their high porosity, high liquid absorption, low density and high air permeability. These characteristics enable porous materials to absorb liquid quickly, reduce blood loss, and thus slow down bleeding; activate the coagulation mechanism, promote platelet aggregation and fibrinogen conversion, form blood clots to seal wounds; and maintain a moist healing environment to facilitate wound healing.

[0003] Chinese patent CN202011615887.7 discloses a method for preparing a chitosan microsphere-bacterial cellulose composite material. The chitosan solution treated at 115°C and 0.15Mpa is diffused into the oxidized bacterial cellulose and then immersed in a sulfate aqueous solution or a phosphate aqueous solution. After washing, the chitosan-bacterial cellulose composite material is obtained. The high temperature and high pressure environment makes the preparation cost high. Summary of the invention

[0004] The purpose of the present invention is to provide a method for preparing a biocompatible porous BC / CS composite material, wherein the chitosan is evenly distributed on the product by stirring with a magnetic stirrer under relatively mild conditions. The method is simple and easy to implement, does not require a high temperature and high pressure environment, is low in cost, and is suitable for large-scale production. The prepared chitosan-bacterial cellulose composite material is a very promising porous biomaterial.

[0005] To achieve the above purpose, the technical solution of the present invention is as follows:

[0006] A method for preparing a biocompatible porous BC / CS composite material comprises the following steps:

[0007] Step 1, bacterial cellulose pretreatment:

[0008] The bacterial fiber BC was melted at room temperature, then stirred in an electric stirrer, and then the BC was crushed in an ultrasonic cell disruptor to obtain a uniform BC dispersion, and finally NaOH was added to the dispersion to adjust the pH to 7 to obtain a pretreated BC dispersion;

[0009] Step 2, bacterial cellulose oxidation treatment:

[0010] Adding NaIO4 to the pretreated BC dispersion under light shielding and stirring to obtain an oxidized BC dispersion, and performing a centrifugal impurity removal treatment to obtain oxidized bacterial cellulose;

[0011] Step 3, preparing chitosan solution:

[0012] Weigh 99g of deionized water and 1g of CH3COOH to prepare a 1% acetic acid solution, weigh chitosan CS and add it to the 1% acetic acid solution and stir to dissolve;

[0013] Step 4, bacterial cellulose and chitosan composite:

[0014] The supernatant liquid of the oxidized bacterial cellulose obtained in step 2 is removed, the oxidized bacterial cellulose is weighed, the oxidized bacterial cellulose and the chitosan solution are mixed, and then stirred in a water bath magnetic stirrer to fully react to obtain a BC / CS composite material, and a centrifugal impurity removal treatment is performed to obtain an impurity-free BC / CS composite material;

[0015] Step 5, preparation of porous composite material:

[0016] The impurity-free BC / CS composite material obtained in step 4 is placed in a refrigerator for freezing, and after being completely frozen, is placed in a freeze dryer for freeze drying for 12-36 hours to obtain a porous BC / CS composite material.

[0017] Furthermore, in step 1, the electric stirrer rotates at a speed of 12000-18000 rpm, stirring for 8-12 minutes, and the cells are disrupted in an ultrasonic cell disruptor for 20-30 minutes.

[0018] Furthermore, in step 2, the mixture is stirred for 12 hours under shade.

[0019] Furthermore, the specific method of centrifugal impurity removal in step 2 is: the oxidized BC dispersion is centrifuged at a speed of 7000 rpm for 5 minutes for impurity removal, and the process is repeated three times.

[0020] Furthermore, in step 4, the water bath temperature in the water bath magnetic stirrer is 60° C., and the water bath is stirred for 4 hours.

[0021] Furthermore, the specific method of the centrifugal impurity removal in step 4 is: the porous BC / CS composite material is centrifuged at a speed of 7000 rpm for 5 minutes to remove impurities, and the process is repeated three times.

[0022] Compared with the prior art, the present invention has the following beneficial effects:

[0023] (1) The present invention provides a method for preparing a biocompatible porous BC / CS composite material, using low-cost bacterial cellulose (BC) obtained by fermenting coconut product by-products and chitosan (CS) produced from shrimp and crab shells, which are aquatic waste, as raw materials, and sodium periodate (NaIO4) as an oxidant. In a weak acid reaction system, the porous composite material can be obtained by only passing through a low-temperature water bath and then freeze-drying.

[0024] (2) The porous composite material has the characteristics of high porosity, high liquid absorption rate and good biocompatibility, and can be applied in the biological field to provide a basis for hemostasis, drug delivery, etc.

[0025] (3) This method has low cost, simple process, good reproducibility, high stability, is suitable for large-scale production, and can promote the commercialization of porous materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 The present invention provides a process flow chart of a method for preparing a biocompatible porous BC / CS composite material.

[0027] Figure 2 X-ray diffraction patterns of bacterial cellulose, chitosan and the porous BC / CS composite material prepared in Example 1.

[0028] Figure 3 This is the surface scanning element distribution diagram of Example 1.

[0029] Figure 4 (a) is a live cell detection observation diagram of Example 1, Figure 4 (b) is a dead cell detection observation diagram of Example 1.

[0030] Figure 5 The porosity of Example 1 and pure BC.

[0031] Figure 6 It is the liquid absorption rate of Example 1 and pure BC. DETAILED DESCRIPTION

[0032] The present invention is further described in detail below in conjunction with the accompanying drawings and specific embodiments.

[0033] A method for preparing a biocompatible porous BC / CS composite material, such as Figure 1 As shown in the process flow chart, the specific operation steps are as follows:

[0034] Step 1, pretreatment of bacterial cellulose: melt the bacterial fiber BC at room temperature, then stir it in an electric stirrer at 12000-18000 rpm for 8-12 minutes, then put the BC into an ultrasonic cell disruptor for 20-30 minutes to obtain a uniform BC dispersion, and finally add NaOH to the dispersion to adjust the pH to 7 to obtain a pretreated BC dispersion;

[0035] Step 2, oxidation treatment of bacterial cellulose: add 1-3 g NaIO4 to the pretreated BC dispersion, shield from light and stir for 12 hours to obtain an oxidized BC dispersion, centrifuge the oxidized BC dispersion in a centrifuge at a speed of 7000 rpm for 5 minutes for 3 times to remove impurities, and obtain oxidized bacterial cellulose;

[0036] Step 3, prepare chitosan solution: weigh 99g deionized water and 1g CH3COOH to prepare 1% acetic acid solution, weigh 1-3g chitosan CS and add it to the acetic acid solution and stir to dissolve;

[0037] Step 4, compounding bacterial cellulose and chitosan: remove the supernatant from the oxidized bacterial cellulose obtained in step 2, then weigh 50-150 g of oxidized bacterial cellulose, mix the oxidized bacterial cellulose and chitosan solution, stir in a water bath magnetic stirrer at 60° C. for 4 h to fully react to obtain a BC / CS composite material, then use a centrifuge at a speed of 7000 rpm for 5 min to remove impurities three times to obtain an impurity-free BC / CS composite material.

[0038] Step 5, preparation of porous composite material: freeze the material in a refrigerator for 12 hours, and after it is completely frozen, place it in a freeze dryer and freeze-dry it for 12-36 hours to obtain a porous BC / CS composite material.

[0039] Example 1

[0040] Step 1, pretreatment of bacterial cellulose: melt BC at room temperature, then stir with an electric stirrer at 12000 rpm for 12 min, then put BC into an ultrasonic cell disruptor for 20 min to obtain a uniform BC dispersion, and finally add NaOH to the dispersion to adjust the pH to 7 to obtain a pretreated BC dispersion;

[0041] Step 2, oxidation treatment of bacterial cellulose: add 1 g of NaIO4 to the pretreated BC dispersion, shield from light and stir for 12 hours to obtain an oxidized BC dispersion, centrifuge the oxidized BC dispersion in a centrifuge at a speed of 7000 rpm for 5 minutes for 3 times to remove impurities, and obtain oxidized bacterial cellulose;

[0042] Step 3, prepare chitosan solution: weigh 99g deionized water and 1g CH3COOH to prepare a 1% acetic acid solution, weigh 1g CS and add it to the acetic acid solution and stir to dissolve;

[0043] Step 4, compounding bacterial cellulose and chitosan: remove the supernatant from the oxidized bacterial cellulose obtained in step 2, weigh 50 g of oxidized bacterial cellulose, mix the oxidized bacterial cellulose and chitosan solution, stir in a water bath magnetic stirrer at 60° C. for 4 h to fully react to obtain a BC / CS composite material, then centrifuge at a speed of 7000 rpm for 5 min for 3 times to remove impurities, and obtain an impurity-free BC / CS composite material;

[0044] Step 5, preparation of porous composite material: freeze the material in a refrigerator for 12 hours, and after it is completely frozen, place it in a freeze dryer and freeze-dry it for 12 hours to obtain a porous BC / CS composite sponge.

[0045] Example 2

[0046] Step 1, pretreatment of bacterial cellulose: melt BC at room temperature, then stir with an electric stirrer at 15000 rpm for 10 min, then put BC into an ultrasonic cell disruptor for 25 min to obtain a uniform BC dispersion, and finally add NaOH to the dispersion to adjust the pH to 7 to obtain a pretreated BC dispersion;

[0047] Step 2, oxidation treatment of bacterial cellulose: add 2 g of NaIO4 to the pretreated BC dispersion, shield from light and stir for 12 hours to obtain an oxidized BC dispersion, centrifuge the oxidized BC dispersion in a centrifuge at a speed of 7000 rpm for 5 minutes for 3 times to remove impurities, and obtain oxidized bacterial cellulose;

[0048] Step 3, prepare chitosan solution: weigh 99g deionized water and 1g CH3COOH to prepare a 1% acetic acid solution, weigh 2g CS and add it to the acetic acid solution and stir to dissolve;

[0049] Step 4, compounding bacterial cellulose and chitosan: remove the supernatant from the oxidized bacterial cellulose obtained in step 2, weigh 100 g of oxidized bacterial cellulose, mix the oxidized bacterial cellulose and chitosan solution, stir in a water bath magnetic stirrer at 60° C. for 4 h to fully react to obtain a BC / CS composite material, then centrifuge at a speed of 7000 rpm for 5 min for 3 times to remove impurities, and obtain an impurity-free BC / CS composite material;

[0050] Step 5, preparation of porous composite material: freeze the material in a refrigerator for 12 hours, and after it is completely frozen, place it in a freeze dryer and freeze-dry it for 24 hours to obtain a porous BC / CS composite material.

[0051] Example 3

[0052] Step 1, pretreatment of bacterial cellulose: melt BC at room temperature, then stir with an electric stirrer at 18000 rpm for 8 min, then put BC into an ultrasonic cell disruptor for 30 min to obtain a uniform BC dispersion, and finally add NaOH to the dispersion to adjust the pH to 7 to obtain a pretreated BC dispersion;

[0053] Step 2, oxidation treatment of bacterial cellulose: add 3 g of NaIO4 to the pretreated BC dispersion, shield from light and stir for 12 hours to obtain an oxidized BC dispersion, centrifuge the oxidized BC dispersion in a centrifuge at a speed of 7000 rpm for 5 minutes for 3 times to remove impurities, and obtain oxidized bacterial cellulose;

[0054] Step 3, prepare chitosan solution: weigh 99g deionized water and 1g CH3COOH to prepare a 1% acetic acid solution, weigh 3g CS and add it to the acetic acid solution and stir to dissolve;

[0055] Step 4, compounding bacterial cellulose and chitosan: remove the supernatant from the oxidized bacterial cellulose obtained in step 2, weigh 150 g of oxidized bacterial cellulose, mix the oxidized bacterial cellulose and chitosan solution, stir in a water bath magnetic stirrer at 60° C. for 4 h to fully react to obtain a BC / CS composite material, then centrifuge at a speed of 7000 rpm for 5 min for 3 times to remove impurities, and obtain an impurity-free BC / CS composite material;

[0056] Step 5, preparation of porous composite material: freeze the material in a refrigerator for 12 hours, and after it is completely frozen, place it in a freeze dryer and freeze-dry it for 36 hours to obtain a porous BC / CS composite material.

[0057] X-ray diffraction analysis (XRD) was performed on the porous BC / CS composite material and BC and CS prepared in Example 1 of the present invention (e.g. Figure 2 As shown in the figure, the difference between the diffraction peak of BC and the diffraction peak of the porous BC / CS composite material is mainly reflected in the diffraction peak at 2θ of 16°. After adding CS, the diffraction peak of the material at 2θ of 16° increases, so it can be shown that the present invention successfully prepares the porous BC / CS composite material.

[0058] Using EDS detection, surface scanning was performed on Example 1 to detect the distribution of surface elements (such as Figure 3 As shown), it can be seen from the figure that the N element is evenly distributed on the surface of the material, indicating that the present invention can successfully composite CS on BC.

[0059] The biological properties of Example 1 were determined using live and dead cell assays (e.g. Figure 4 shown), Figure 4 In (a), green indicates living cells. Figure 4 The red cells in (b) are dead cells. It can be seen that the cell death rate is extremely low, which proves that the cell population of the selected cell line maintains a high degree of activity and stability under experimental conditions after specific treatment, thereby proving its good biological performance.

[0060] The Archimedean principle was used to determine the Figure 5As shown), it can be seen that the porosity of pure BC is 79.95%±2.28%, and the porosity of Example 1 becomes 85.77%±1.97%. The addition of CS improves the porosity of the material.

[0061] The liquid absorption rate of Example 1 and pure BC was evaluated using simulated body fluid (eg Figure 6 As shown), it can be seen that the liquid absorption rate of pure BC is 865.8%, the liquid absorption rate of Example 1 is 1314.7%, and the addition of CS improves the liquid absorption rate of the material.

[0062] The above-mentioned embodiments only express the specific implementation of the present invention, and the description thereof is relatively specific and detailed, but it cannot be understood as limiting the scope of the invention patent. It should be pointed out that for ordinary technicians in this field, several modifications and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be based on the attached claims.

Claims

1. A method for preparing a biocompatible porous BC / CS composite material, characterized in that: The following steps are involved: Step 1, bacterial cellulose pretreatment: The bacterial fiber BC was melted at room temperature, then stirred in an electric stirrer, and then the BC was crushed in an ultrasonic cell disruptor to obtain a uniform BC dispersion, and finally NaOH was added to the dispersion to adjust the pH to 7 to obtain a pretreated BC dispersion; Step 2, bacterial cellulose oxidation treatment: Adding NaIO4 to the pretreated BC dispersion under light shielding and stirring to obtain an oxidized BC dispersion, and performing a centrifugal impurity removal treatment to obtain oxidized bacterial cellulose; Step 3, preparing chitosan solution: Weigh 99g of deionized water and 1g of CH3COOH to prepare a 1% acetic acid solution, weigh chitosan CS and add it to the 1% acetic acid solution and stir to dissolve; Step 4, bacterial cellulose and chitosan composite: The supernatant liquid of the oxidized bacterial cellulose obtained in step 2 is removed, the oxidized bacterial cellulose is weighed, the oxidized bacterial cellulose and the chitosan solution are mixed, and then stirred in a water bath magnetic stirrer to fully react to obtain a BC / CS composite material, and a centrifugal impurity removal treatment is performed to obtain an impurity-free BC / CS composite material; Step 5, preparation of porous composite material: The impurity-free BC / CS composite material obtained in step 4 is placed in a refrigerator for freezing, and after being completely frozen, is placed in a freeze dryer for freeze drying for 12-36 hours to obtain a porous BC / CS composite material.

2. The method for preparing a biocompatible porous BC / CS composite material according to claim 1, characterized in that: In step 1, the electric stirrer rotates at a speed of 12000-18000 rpm, stirring for 8-12 minutes, and disrupting in an ultrasonic cell disruptor for 20-30 minutes.

3. The method for preparing a biocompatible porous BC / CS composite material according to claim 1, characterized in that: In step 2, stir for 12 h under shade.

4. The method for preparing a biocompatible porous BC / CS composite material according to claim 1, characterized in that: The specific method of centrifugal impurity removal in step 2 is: the oxidized BC dispersion is centrifuged at a speed of 7000 rpm for 5 minutes for impurity removal, and this is repeated three times.

5. The method for preparing a biocompatible porous BC / CS composite material according to claim 1, characterized in that: In step 4, the water bath temperature in the water bath magnetic stirrer is 60° C., and the water bath is stirred for 4 h.

6. The method for preparing a biocompatible porous BC / CS composite material according to claim 1, characterized in that: The specific method of the centrifugal impurity removal in step 4 is: the porous BC / CS composite material is centrifuged at a speed of 7000 rpm for 5 minutes to remove impurities, and the process is repeated three times.