Rubber for large ship fender and production method thereof
By combining natural rubber and bio-based rubber and using carbon black and nanocarbon black fillers, the problems of insufficient wear resistance, aging resistance and tear resistance of ship fender rubber materials are solved, and its overall performance and use are improved life.
Patent Information
- Application Number
- CN202411242647.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-05
- Publication Date
- 2024-11-22
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing rubber materials for ship fenders have problems such as insufficient wear resistance, poor anti-aging performance, poor tear resistance and poor processing performance, and other properties may be sacrificed while improving one performance.
By combining natural rubber and bio-based rubber and adding fillers such as carbon black and nanocarbon black, the formulation is optimized to improve the elasticity, impact resistance and anti-aging properties of the rubber while improving processing properties.
It significantly improves the wear resistance, tear resistance and aging resistance of rubber, improves processing performance, extends service life, and achieves a comprehensive balance of performance.
Abstract
Description
Technical Field
[0001] The invention mainly relates to the technical field, in particular to a rubber for large ship fenders and a production method thereof. Background Art
[0002] Large ship fenders are a device used to protect ships and piers from collision damage, preventing damage to each other by mitigating the impact caused by contact. Since these fenders minimize the damage to the hull caused by ship-to-pier or ship-to-ship collisions, their role is very important and the Ministry of Maritime Affairs and Fisheries requires fenders to be installed around ships.
[0003] Fenders are usually made of rubber materials, which are required to have high elasticity, good impact resistance, wear resistance, anti-aging performance and processing performance. Existing rubber materials for ship fenders usually have the following problems: 1. Insufficient wear resistance: Fenders frequently come into contact with the ship structure during use, causing severe wear of the rubber material and reducing its service life.
[0004] 2. Poor anti-aging performance: Ship fender rubber is easily affected by ultraviolet rays, oxygen and ozone in the marine environment, which leads to material aging and performance degradation.
[0005] 3. Poor tear resistance: Large ships may exert a large impact force on the fender during berthing, causing the rubber to tear.
[0006] 4. Poor processing performance: Rubber materials may have processing difficulties during the manufacturing process, such as poor fluidity and easy burning.
[0007] 5. The problem of comprehensive performance balance: while improving a certain property (such as wear resistance), other properties (such as elasticity or tear resistance) may be sacrificed.
[0008] In view of the problems existing in the existing rubber materials for ship fenders and the existing environmental protection needs, it is necessary to develop a rubber material for large ship fenders, which has excellent wear resistance, weather resistance, and excellent anti-aging and tear resistance comprehensive properties. Summary of the invention
[0009] In view of the problems of current fender rubber materials mentioned in the background technology, the present invention mainly provides a rubber for large ship fenders and a production method thereof. By combining natural rubber and bio-based rubber and adding fillers such as carbon black and nano carbon black, the prepared rubber material has high elasticity and good impact resistance and wear resistance, and has excellent comprehensive properties such as anti-aging performance and processing performance.
[0010] The technical solution adopted by the present invention to solve the above technical problems is: In a first aspect, the present invention provides a rubber for large ship fenders, comprising the following components in the following amounts: natural rubber J: 20kg~35kg, natural rubber G: 10kg~20kg, bio-based rubber: 5kg~10kg, calcium carbonate: 10kg~18kg, carbon black: 4kg~8kg, nano carbon black: 0.2kg~0.8kg, zinc oxide 1100g~1250g, MRT antiozonant: 100g~125g, rubber vulcanization accelerator DPG: 115g~130g, antioxidant: 100g~125g, stearic acid 265g~300g, coumarone resin 270g~290g, peptizer double T: 40g~55g, sulfur particles: 105g~115g.
[0011] The functions of each component in the above rubber are as follows: Natural rubber J has good elasticity and processing performance, while natural rubber G has higher purity and lower impurity content, which can improve the comprehensive performance of rubber. The combination of the two can give full play to their respective advantages, improve the overall elasticity and processing performance of fender rubber, make it easier to shape and vulcanize, and have better durability and environmental resistance. In addition, by reasonably mixing the two natural rubbers, it is possible to optimize costs while maintaining product performance and maximize economic benefits.
[0012] In the present invention, by adding bio-based rubber, natural rubber can be partially replaced, thus reducing costs and improving environmental protection; Calcium carbonate is used as a filler to improve the wear resistance and hardness of rubber. Its usage is within the range of 10-18kg, which can ensure performance and control costs; Carbon black improves the wear resistance, tear resistance and strength of rubber. By using different types of natural rubber (J and G) in combination with carbon black, the tear resistance of rubber is significantly improved, making it better able to withstand impact and tearing forces.
[0013] The interaction mechanism between natural rubber and carbon black includes physical adsorption, chemical crosslinking and steric hindrance effect. Carbon black particles can adsorb rubber molecular chains to form a physical network structure; the active sites on the carbon black surface can react chemically with rubber molecular chains to form chemical bonds; carbon black particles can restrict the movement of rubber molecular chains and improve the strength and elasticity of rubber.
[0014] In the present invention, the wear resistance, tear resistance and aging resistance of the fender rubber are significantly improved by adding nano-carbon black. The reasons are: 1. Nano-carbon black has a higher specific surface area and active sites, and can form stronger physical adsorption and chemical cross-linking with the rubber molecular chain, thereby significantly improving the wear resistance of the rubber; 2. Nano-carbon black can enhance the physical network structure of the rubber, improve the strength and toughness of the rubber, thereby improving the tear resistance of the rubber; 3. Nano-carbon black can block the invasion of ultraviolet rays and ozone, and capture free radicals, thereby delaying the aging process of the rubber and improving the anti-aging performance of the rubber. In addition, nano-carbon black can also reduce the viscosity of the rubber and improve the fluidity of the rubber, thereby improving the processing performance of the rubber. Zinc oxide acts as an active agent to promote the cross-linking of sulfur and rubber, and improve the strength and wear resistance of rubber. The dosage is within the range of 1100-1250g, which can ensure the cross-linking effect of rubber.
[0015] MRT antiozonant is used as an antiozonant to prevent rubber from aging due to ozone. The dosage is within the range of 100-125g, which can effectively improve the anti-aging performance of rubber. Rubber vulcanization accelerator DPG acts as an accelerator to accelerate the cross-linking reaction between sulfur and rubber, thus ensuring the vulcanization effect of rubber.
[0016] Anti-aging agents improve the anti-aging properties of rubber and extend its service life. Specifically, environmentally friendly antioxidants can be used to replace traditional antioxidants to reduce the impact on the environment, such as antioxidant 1010 or hindered phenol antioxidants.
[0017] Stearic acid acts as a lubricant to improve the processing properties of rubber.
[0018] Coumarone resin improves the toughness and adhesion of rubber. The dosage is within the range of 270-290g, which helps to improve the overall performance of rubber. Peptizer double T is used as a peptizer to improve the processing performance of rubber. The amount used is within the range of 40-55g, which can make the rubber easier to plasticize during processing. Stearic acid and peptizer double T are added in the present invention, and these ingredients can improve the processing performance of rubber, increase fluidity, reduce scorch phenomenon, and make the production process smoother.
[0019] Sulfur particles act as a vulcanizing agent, giving rubber good elasticity and strength.
[0020] In summary, the fender rubber formula of the present application is improved in terms of wear resistance, aging resistance, tear resistance and toughness compared with the prior art, and the dosage and working principle of each component are carefully designed to achieve optimal performance.
[0021] The interaction mechanism between zinc oxide and sulfur is that zinc oxide can form an active vulcanization system with sulfur, accelerate the cross-linking reaction of sulfur, and improve the performance of the vulcanized rubber.
[0022] The interaction mechanism between accelerator DPG and sulfur is that DPG can provide active hydrogen atoms, which react with sulfur to generate active sulfur, thereby accelerating the vulcanization process.
[0023] The interaction mechanism between antioxidants and natural rubber is that antioxidants can capture free radicals or react with oxidants to prevent the breakage and cross-linking of rubber molecular chains, thereby delaying the aging process. The amount of nano carbon black used needs to be balanced according to the performance requirements and cost of the rubber. Adding too much nano carbon black will increase the cost of the rubber and may cause the rubber to become hard and brittle. Adding too little nano carbon black will not fully play its reinforcing role.
[0024] In some achievable embodiments of the first aspect, the natural rubber J is at least one of standard latex RSS or particle rubber CR; And / or, the natural rubber G is at least one of concentrated latex CNR or smoked rubber sheet SMR.
[0025] In some achievable embodiments of the first aspect, the bio-based rubber is selected from at least one of bio-based polyisoprene rubber, bio-based styrene butadiene rubber (SBR), or bio-based butadiene rubber (BR).
[0026] In some achievable embodiments of the first aspect, the ratio of the addition amount of the natural rubber to the carbon black is within the range of 5:1 to 8.75:1, which can ensure that the rubber has both good elasticity and sufficient strength and wear resistance. The natural rubber provides the basic elasticity and toughness of the rubber, while the carbon black, as a reinforcing filler, can significantly improve the strength, wear resistance and tear resistance of the rubber.
[0027] And / or, the ratio of the amount of zinc oxide to sulfur particles added is in the range of 10:1 to 11.4:1, which can ensure that the sulfur is fully vulcanized, and at the same time, the zinc oxide will not be excessive, thereby avoiding adverse effects on the rubber properties. Zinc oxide is used as an activator, and zinc oxide can form an active vulcanization system with sulfur, accelerate the cross-linking reaction of sulfur, and improve the performance of the vulcanized rubber.
[0028] In some achievable methods of the first aspect, the particle size distribution of the nano carbon black is controlled between 10 and 50 nanometers. Too fine a particle size of the nano carbon black (<10 nanometers) may cause a sharp increase in the viscosity of the rubber, poor fluidity, difficulty in processing and molding, and increase the risk of scorching; too coarse a particle size (>50 nanometers) will weaken the wear resistance and anti-aging effects of the rubber, and have a greater impact on other properties of the rubber (such as elasticity and tear resistance).
[0029] And / or, the carbon black is selected from medium-sized carbon black. Medium-sized non-structural carbon black, such as N550 or N660, has certain wear resistance and tear resistance, good compatibility with rubber, good processing performance, and can provide better comprehensive performance.
[0030] In some achievable embodiments of the first aspect, the ratio of the amount of the rubber vulcanization accelerator DPG to the sulfur particles is in the range of 1:1 to 1.15:1, which can ensure that the sulfur is rapidly vulcanized at a suitable temperature. DPG can provide active hydrogen atoms and react with sulfur to generate active sulfur, thereby accelerating the vulcanization process.
[0031] Through the mutual promotion between these components, the final rubber product can be comprehensively improved in terms of wear resistance, aging resistance, tear resistance and processing performance.
[0032] Optimization of filler and reinforcement system: The wear resistance and tear resistance of rubber are improved by accurately matching natural rubber and carbon black, as well as an appropriate amount of calcium carbonate, which is superior to existing formulas that only use a single type of filler or reinforcement.
[0033] Enhanced anti-aging performance: Antioxidant (A) and MRT are added. These ingredients help improve the durability of rubber in harsh marine environments and are more innovative than formulas that rely solely on traditional antioxidants.
[0034] Improvement of the vulcanization system: Zinc oxide and DPG are used as activators and accelerators, combined with sulfur to form a more efficient vulcanization system.
[0035] In a second aspect, the present invention provides a method for producing a rubber for a large ship fender, characterized in that the method is used to prepare the rubber for a large ship fender, and the production method comprises the following steps: S1: weigh the raw materials according to the formula ratio; S2: uniformly dispersing various raw materials through mixing to form a rubber material with desired properties; Using a co-rotating twin-screw mixer or continuous mixer to replace the traditional open mixer or internal mixer has better material conveying and dispersion capabilities, can achieve higher mixing uniformity in a shorter time, and reduce energy consumption and material loss. Introduce sensors and control systems during the mixing process to monitor the mixing temperature, pressure and mixing degree in real time. Through real-time data feedback, the mixing conditions can be accurately controlled to ensure the consistency of mixing quality and avoid over-mixing or under-mixing.
[0036] S3: Segmented vulcanization treatment: S301: Put the mixed rubber material into a vulcanizer or vulcanizing tank for preheating, the preheating temperature is 50-70°C, and the preheating time is 5-10 minutes; the purpose of preheating is to remove bubbles in the rubber, reduce internal stress during the vulcanization process, and prepare for the subsequent vulcanization stage.
[0037] S302: Primary vulcanization: after preheating, gradually increase the temperature to the primary vulcanization temperature, and the primary vulcanization temperature is about 110-130°C, the primary vulcanization time is 5-15 minutes, and the pressure in the vulcanizer or vulcanizing tank is kept moderate; the purpose of primary vulcanization is to make the rubber begin to cross-link, form a preliminary network structure, and provide basic physical properties.
[0038] S303: Intermediate vulcanization. After the primary vulcanization is completed, the temperature is further raised to the intermediate vulcanization temperature, and the intermediate vulcanization temperature is 140-160°C, the intermediate vulcanization time is 10-30 minutes, and the pressure in the vulcanizer or vulcanizing tank is appropriately increased; the purpose of intermediate vulcanization is to deepen the crosslinking degree of the rubber and improve the strength and elasticity of the rubber.
[0039] S304: Deep vulcanization. After the intermediate vulcanization is completed, the temperature is continued to rise to the deep vulcanization temperature, and the deep vulcanization temperature is 160-180°C, the deep vulcanization time is 20-60 minutes, and the pressure is maintained or slightly reduced; the purpose of deep vulcanization is to ensure that the rubber reaches the optimal cross-linking density and obtains the best comprehensive performance.
[0040] S305: Post-vulcanization: After deep vulcanization is completed, the temperature is gradually lowered to allow the rubber to slowly cool to room temperature. The cooling rate is 5-10°C / minute. The purpose of post-vulcanization is to reduce the stress inside the vulcanized rubber and prevent deformation and performance degradation during the cooling process.
[0041] By gradually heating, the staged vulcanization makes the vulcanization degree inside and outside the rubber tend to be consistent, avoiding stress concentration and uneven vulcanization caused by temperature difference. Adjusting the pressure at different vulcanization stages helps the rubber flow during the vulcanization process, ensures uniform vulcanization, and reduces internal bubbles. By controlling the vulcanization temperature and time in stages, the cross-linking degree of the rubber can be more accurately controlled, thereby optimizing its physical and chemical properties. The slow cooling process helps to reduce the thermal stress inside the rubber and prevent rubber deformation or cracks caused by rapid cooling.
[0042] Through the above-mentioned segmented vulcanization process, the performance of rubber products can be more effectively controlled, production efficiency and product quality can be improved, and it is especially suitable for large and complex rubber products, such as ship fenders.
[0043] S4: Post-processing: After vulcanization, take out the rubber product, remove the burrs and excess sulfur; inspect the rubber product, including appearance inspection, dimensional measurement and physical property testing. S5: Finished product inspection, conduct physical property tests such as tensile strength, tear strength, abrasion resistance, hardness, etc. on the rubber fender, check the appearance of the rubber fender to ensure there are no defects, and conduct necessary aging resistance tests to verify its long-term performance.
[0044] S6: Packaging and storage: Clean the qualified rubber fenders, then pack them and store them in a dry, ventilated and light-proof warehouse to avoid contact with oil, acid, alkali and other substances.
[0045] Through the above production process steps, it can be ensured that the rubber produced for large ship fenders has excellent wear resistance, aging resistance, tear resistance and processing performance, meeting the stringent requirements of offshore operations.
[0046] In some achievable embodiments of the second aspect, the mixing in S2 comprises the following steps: S201: In the plasticizing stage, the weighed natural rubber and bio-based rubber are put into an open mill for plasticizing to soften them for subsequent mixing operations; S202: In the mixing stage, carbon black, nano carbon black and calcium carbonate filler are added and mixed until uniform; the purpose of mixing is to uniformly mix the natural rubber with other components (such as carbon black, filler, vulcanizer, accelerator, etc.) to form a rubber material with the required properties.
[0047] S203: Refining stage, adding zinc oxide, stearic acid, antioxidant, MRT, DPG, coumarone resin and peptizer double T small material, continue mixing, the purpose of refining is to further improve the uniformity and dispersibility of the rubber material, and remove bubbles; S204: In the sheeting stage, sulfur particles are added at the end, and the mixed rubber is sheeted after being uniformly mixed. The purpose of sheeting is to make the mixed rubber material into sheets for the convenience of subsequent vulcanization operations.
[0048] In some achievable modes of the second aspect, the mixing is performed using a co-rotating twin-screw mixer or a continuous mixer; And / or, the temperature, time and pressure of each stage of mixing are different, wherein the temperature of the plasticizing stage is 40-60°C, the time is 5-10 minutes, and the pressure is 1MPa-3MPa; the appropriate temperature and time can break the natural rubber molecular chain, reduce the molecular weight, and thus improve its plasticity and fluidity. The pressure can help to compact the rubber molecular chain and promote the plasticization process.
[0049] The temperature of the mixing stage is 80~120°C, the time is 10~30 minutes, and the pressure is 3MPa~7MPa; the appropriate temperature and time can make the rubber and other components fully mixed to form a uniform mixture. The pressure range of 3MPa~7MPa can help compact the rubber and other components and promote the mixing process.
[0050] The temperature in the refining stage is 80~120°C, the time is 5~10 minutes, and the pressure is 3~7MPa; higher temperature and pressure are usually used in the refining stage, which can make the rubber material more uniform and help remove bubbles, thereby improving the performance of the vulcanized rubber.
[0051] The unloading stage adopts the automatic unloading method with a pressure of 3~5MPa. The rubber material needs to have good fluidity to facilitate the unloading operation.
[0052] In some achievable embodiments of the second aspect, the pressures at various stages of the segmented vulcanization are different: The pressure in the preheating stage is moderate and maintained in the range of 1-2 MPa. The use of low pressure in the preheating stage can prevent the rubber from being vulcanized prematurely and is conducive to the discharge of bubbles, thereby improving the density and physical properties of the vulcanized rubber.
[0053] The pressure in the primary vulcanization stage is gradually increased and maintained in the range of 3-5 MPa, which can promote the flow of rubber, make the rubber fill the mold more evenly, and help further discharge bubbles, thereby improving the density and physical properties of the vulcanized rubber.
[0054] The pressure in the intermediate vulcanization stage is appropriately increased and maintained within the range of 5-7 MPa, which can ensure that the rubber maintains a certain fluidity during the vulcanization process, thereby ensuring the density and physical properties of the vulcanized rubber.
[0055] The pressure is maintained or slightly reduced in the deep vulcanization stage within the range of 4-6 MPa, which can prevent the rubber from being over-vulcanized and help shrink the vulcanized rubber, thereby improving the dimensional stability of the vulcanized rubber.
[0056] The pressure in the post-vulcanization stage is gradually reduced to zero, which can prevent the vulcanized rubber from deforming or cracking and help cool the vulcanized rubber, thereby improving the dimensional stability and physical properties of the vulcanized rubber.
[0057] 1. The present invention effectively resists the damage of ultraviolet rays and ozone by adding an antioxidant, thereby extending the service life of the rubber. In addition, the active vulcanization system of zinc oxide and sulfur also helps to improve the anti-aging performance of the rubber, and can solve the problem that the ship fender rubber is affected by ultraviolet rays, oxygen and ozone in the marine environment, resulting in material aging and performance degradation.
[0058] 2. By using different types of natural rubber (J and G) and combining it with carbon black, the formula significantly improves the rubber's tear resistance, enabling the fenders of large ships to better withstand greater impact and tearing forces, avoiding problems such as fender rubber tearing, and extending the service life of the fender rubber.
[0059] 3. The invention adds additives such as stearic acid and peptizer double T, which can improve the processing performance of rubber, increase fluidity, reduce scorch phenomenon, and make the production process smoother.
[0060] 4. By optimizing the components and proportions, the problems of existing large ship fender rubber in terms of wear resistance, aging resistance, tear resistance, processing performance and comprehensive performance balance are effectively solved, thereby improving the service life and reliability of ship fenders.
[0061] The present invention will be explained in detail below in conjunction with specific embodiments. DETAILED DESCRIPTION
[0062] To facilitate understanding of the present invention, the present invention will be described more comprehensively below with reference to the relevant text. Several embodiments of the present invention are given in the text, but the present invention can be implemented in different forms and is not limited to the embodiments described in the text. On the contrary, these embodiments are provided to make the content disclosed in the present invention more thorough and comprehensive.
[0063] Embodiment 1: A method for producing a rubber for a large ship fender provided in an embodiment of the present invention comprises the following steps: S1: Weigh the raw materials according to the formula ratio. The specific formula is: natural rubber J: 25kg, natural rubber G: 15kg, bio-based rubber: 7.5kg, carbon black: 5kg, nano carbon black: 0.5kg, zinc oxide: 1200g, MRT antiozonant: 110g, rubber vulcanization accelerator DPG: 125g, antioxidant: 115g, stearic acid: 285g, coumarone resin: 280g, plasticizer double T: 45g, sulfur granules: 120g.
[0064] Among them, natural rubber J is standard latex RSS, natural rubber G is concentrated latex CNR, bio-based rubber is bio-based polyisoprene rubber, and carbon black is medium particle size carbon black N660.
[0065] The addition ratio of the above-mentioned natural rubber to carbon black is 8:1, the addition ratio of zinc oxide to sulfur particles is 10:1, and the addition ratio of rubber vulcanization accelerator DPG to sulfur particles is 1.042:1.
[0066] S2: uniformly dispersing various raw materials through mixing to form a rubber material with desired properties; Specifically, the mixing comprises the following steps: S201: In the plasticizing stage, the weighed natural rubber J, G and bio-based rubber are put into an open mill for plasticizing to soften them. The temperature of the plasticizing stage is 55° C., the time is 10 minutes, and the pressure is 3 MPa.
[0067] S202: In the mixing stage, carbon black, nano carbon black and calcium carbonate filler are added and mixed until uniform. The temperature of the mixing stage is 100° C., the time is 25 minutes and the pressure is 5 MPa.
[0068] S203: In the refining stage, zinc oxide, stearic acid, antioxidant, MRT, DPG, coumarone resin and plasticizer double T small materials are added and mixing is continued. The temperature of the refining stage is 100°C, the time is 8 minutes, and the pressure is 6MPa.
[0069] S204: In the sheeting stage, sulfur particles are finally added, and the sheets are sheeted after being mixed evenly. Specifically, in this embodiment, the sheeting stage adopts an automatic sheeting method with a pressure of 3 MPa.
[0070] S3: Segmented vulcanization treatment: S301: putting the mixed rubber material into a vulcanizer or a vulcanizing tank for preheating at a temperature of 50° C. for 7 minutes, and maintaining the pressure within the range of 1 to 2 MPa; S302: Primary vulcanization: after preheating, gradually increase the temperature to the primary vulcanization temperature, and the primary vulcanization temperature is about 120°C, the primary vulcanization time is 10 minutes, and the pressure in the vulcanizer or vulcanization tank is kept moderate and maintained in the range of 3~5MPa. S303: Intermediate vulcanization: after the primary vulcanization is completed, the temperature is further increased to the intermediate vulcanization temperature, and the intermediate vulcanization temperature is 155°C, the intermediate vulcanization time is 15 minutes, and the pressure in the vulcanizer or vulcanizing tank is appropriately increased and maintained in the range of 5-7MPa; S304: Deep vulcanization, after the intermediate vulcanization is completed, the temperature is continued to be raised to the deep vulcanization temperature, and the deep vulcanization temperature is 175°C, the deep vulcanization time is 20 minutes, and the pressure is maintained or slightly reduced, and maintained in the range of 4-6MPa; S305: post-vulcanization, after deep vulcanization is completed, the temperature is gradually reduced to allow the rubber to slowly cool to room temperature. The pressure in the post-vulcanization stage is gradually reduced until it is zero, and the cooling rate is 8°C / minute.
[0071] S4: Post-treatment: After vulcanization is completed, take out the rubber product and remove the burrs and excess sulfur.
[0072] S5: Finished product inspection, physical property test of the rubber fender, check the appearance of the rubber fender to ensure there are no defects; S6: Packaging and storage: Clean the qualified rubber fenders, then pack them and store them in a dry, ventilated and light-proof warehouse.
[0073] Example 2: The production method of rubber for large ship fenders in this example is consistent with Example 1 in basic steps. The difference lies in that the production parameters of the formulation, mixing and vulcanization stages in this example are different. First, the raw material formula is as follows: natural rubber J: 35kg, natural rubber G: 18kg, bio-based rubber: 10kg, carbon black: 10kg, nano carbon black: 0.8kg, zinc oxide: 1250g, MRT antiozonant: 125g, rubber vulcanization accelerator DPG: 130g, antioxidant: 120g, stearic acid: 300g, coumarone resin: 290g, plasticizer double T: 50g, sulfur particles: 115g.
[0074] The addition ratio of natural rubber to carbon black is 5.3:1, the addition ratio of zinc oxide to sulfur particles is 10.87:1; the addition ratio of rubber vulcanization accelerator DPG to sulfur particles is 1.13:1.
[0075] Secondly, the parameters of the mixing stage are as follows: The temperature of the plasticizing stage is 60°C, the time is 8 minutes, and the pressure is 2MPa; The temperature in the mixing stage was 100°C, the time was 18 minutes, and the pressure was 6 MPa; The temperature in the refining stage was 80°C, the time was 6 minutes, and the pressure was 7 MPa; The unloading stage adopts the automatic unloading method with a pressure of 3MPa.
[0076] Finally, the parameters of the staged vulcanization process are as follows: (1) The preheating temperature is 50°C and the preheating time is 10 minutes; (2) The primary vulcanization temperature is about 110°C and the primary vulcanization time is 15 minutes; (3) The intermediate vulcanization temperature is 160°C and the intermediate vulcanization time is 15 minutes; (4) The deep vulcanization temperature is 180°C and the deep vulcanization time is 30 minutes; (5) The cooling rate in the post-vulcanization stage is 10°C / min.
[0077] Example 3: The production method of rubber for large ship fenders in this embodiment has the same basic steps as Example 1, except that the production parameters of the formulation, mixing and vulcanization stages in this embodiment are different. First, the raw material formula is as follows: natural rubber J: 20kg, natural rubber G: 10kg, bio-based rubber: 5kg, carbon black: 5kg, nano carbon black: 0.3kg, zinc oxide: 1100g, MRT antiozonant: 100g, rubber vulcanization accelerator DPG: 115g, antioxidant: 100g, stearic acid: 265g, coumarone resin: 272g, plasticizer double T: 40g, sulfur particles: 105g.
[0078] The addition ratio of natural rubber to carbon black is 6:1, the addition ratio of zinc oxide to sulfur particles is 10.48:1; the addition ratio of rubber vulcanization accelerator DPG to sulfur particles is 1.095:1.
[0079] Secondly, the parameters of the mixing stage are as follows: (1) The temperature of the plasticizing stage is 40°C, the time is 10 minutes, and the pressure is 2 MPa; (2) The temperature of the mixing stage is 80°C, the time is 30 minutes, and the pressure is 6 MPa; (3) The temperature of the refining stage is 100°C, the time is 6 minutes, and the pressure is 7 MPa; (4) The unloading stage adopts the automatic unloading method with a pressure of 4 MPa.
[0080] Finally, the parameters of the staged vulcanization process are as follows: (1) The preheating temperature is 70°C and the preheating time is 6 minutes; (2) The primary vulcanization temperature is about 130°C and the primary vulcanization time is 10 minutes; (3) The intermediate vulcanization temperature is 140°C and the intermediate vulcanization time is 20 minutes; (4) The deep vulcanization temperature is 160°C and the deep vulcanization time is 45 minutes; (5) The cooling rate in the post-vulcanization stage is 10°C / min.
[0081] Example 4: The production method of rubber for large ship fenders in this example has the same basic steps as Example 1, except that in this example, the natural rubber J is replaced by granular rubber CR, and the natural rubber G is replaced by smoked rubber sheet SMR.
[0082] Example 5: The production method of rubber for large ship fenders in this example has the same basic steps as Example 1, except that the bio-based rubber in this example is a mixture of bio-based polyisoprene rubber and bio-based styrene-butadiene rubber SBR.
[0083] Example 6: The production method of rubber for large ship fenders in this example has the same basic steps as Example 1, except that the carbon black in this example is replaced by medium particle size carbon black N550.
[0084] Comparative Example 1: The rubber for large ship fenders in this comparative example is basically consistent with that in Example 1, except that this comparative example does not contain carbon black and nano carbon black, and adopts the existing production method.
[0085] Comparative Example 2: The rubber for large ship fenders in this comparative example is basically consistent with that in Example 1, except that the natural rubber in this comparative example is a single natural rubber variety and is produced using an existing production method.
[0086] Comparative Example 3: The rubber for large ship fenders in this comparative example is basically consistent with that in Example 1, except that the natural rubber in this comparative example is a single natural rubber variety and is produced using an existing production method.
[0087] Comparative Example 4: The rubber for large ship fenders in this comparative example is basically consistent with Example 1, except that this comparative example does not contain antioxidant and MRT antiozonant, and adopts the existing production method.
[0088] The following tests were performed on the above Examples 1-6 and Comparative Examples 1-4, and the test results are shown in Table 1 below: Table 1 is a comparison table of test performance of Examples 1-6 and Comparative Examples 1-4 Test items Tensile strength / MPa Tear strength KN / m Hardness Shore / A <![CDATA[Wear resistance Mm 3 > Anti-aging performance Performance retention rate after aging / % Processing performance: fluidity, scorch time Example 1 18.5 55.0 70 50 90 excellent Example 2 18.7 55.5 72 50 92 excellent Example 3 18.6 55.3 71 51 91 excellent Example 4 18.3 54.8 69 52 90 excellent Example 5 18.4 54.9 69 51 91 excellent Example 6 18.6 55.1 70 50 90 excellent Comparative Example 1 16.2 47.5 65 78 80 generally Comparative Example 2 16.3 45.3 63 80 82 generally Comparative Example 3 16.8 46.8 64 79 85 Difference Comparative Example 4 16.5 48.2 64 80 83 Difference As can be seen from Table 1 above, the rubber properties in Examples 1-6 are better than those in Comparative Examples 1-4, especially in terms of wear resistance, aging resistance and tear resistance, which meet the expected goals. The rubber properties in Comparative Examples 1-4 are relatively poor, indicating that the traditional production process and the formula of a single type of rubber or filler or reinforcing agent cannot meet the requirements of large ship fenders.
[0089] The above is an exemplary description of the present invention. Obviously, the specific implementation of the present invention is not limited to the above-mentioned method. As long as such non-substantial improvements are made by adopting the method concept and technical solution of the present invention, or the concept and technical solution of the present invention are directly applied to other occasions without improvement, they are all within the protection scope of the present invention.
Claims
1. A rubber for large ship fenders, It is characterized in that The composition comprises the following amounts: Natural rubber J: 20kg~35kg; Natural rubber G: 10kg~20kg; Bio-based rubber: 5kg~10kg; Calcium carbonate: 10kg~18kg; Carbon black: 4kg~8kg; Nano carbon black: 0.2kg~0.8kg; Zinc oxide 1100g~1250g; MRT antiozonant: 100g~125g; Rubber vulcanization accelerator DPG: 115g~130g; Anti-aging agent: 100g~125g; Stearic acid 265g~300g; Coumarone resin 270g~290g; Plasticizer double T: 40g~55g; Sulfur granules: 105g~115g.
2. The large ship fender rubber according to claim 1, It is characterized in that The natural rubber J is at least one of standard latex RSS or particle rubber CR; And / or, the natural rubber G is at least one of concentrated latex CNR or smoked rubber sheet SMR.
3. The large ship fender rubber according to claim 2, It is characterized in that The bio-based rubber is selected from at least one of bio-based polyisoprene rubber, bio-based styrene butadiene rubber (SBR) or bio-based butadiene rubber (BR).
4. The large ship fender rubber according to claim 1, It is characterized in that The addition ratio of the natural rubber to the carbon black is in the range of 5:1 to 8.75:1; And / or, the ratio of the zinc oxide to the sulfur particles added is in the range of 10:1 to 11.4:
1.
5. The large ship fender rubber according to claim 1, It is characterized in that The particle size distribution of the nano carbon black is controlled between 10-50 nanometers; And / or, the carbon black is selected from medium particle size carbon black.
6. The large ship fender rubber according to claim 1, It is characterized in that The addition ratio of the rubber vulcanization accelerator DPG to the sulfur particles is in the range of 1:1 to 1.15:
1.
7. A method for producing rubber for large ship fenders, It is characterized in that Used to prepare the large ship fender rubber according to any one of claims 1 to 6, the production method comprises the following steps: S1: weigh the raw materials according to the formula ratio; S2: uniformly dispersing various raw materials through mixing to form a rubber material with desired properties; S3: Segmented vulcanization treatment: S301: putting the mixed rubber material into a vulcanizer or a vulcanizing tank for preheating at a temperature of 50 to 70° C. for 5 to 10 minutes; S302: Primary vulcanization: after preheating, gradually increase the temperature to the primary vulcanization temperature, and the primary vulcanization temperature is about 110-130° C., the primary vulcanization time is 5-15 minutes, and the pressure in the vulcanizer or vulcanization tank is kept moderate; S303: Intermediate vulcanization: after the primary vulcanization is completed, the temperature is further increased to the intermediate vulcanization temperature, and the intermediate vulcanization temperature is 140-160°C, the intermediate vulcanization time is 10-30 minutes, and the pressure in the vulcanizer or vulcanizing tank is appropriately increased; S304: Deep vulcanization, after the intermediate vulcanization is completed, the temperature is continued to be raised to the deep vulcanization temperature, and the deep vulcanization temperature is 160-180°C, the deep vulcanization time is 20-60 minutes, and the pressure is maintained or slightly reduced; S305: post-vulcanization, after deep vulcanization is completed, gradually lower the temperature to allow the rubber to slowly cool to room temperature; S4: Post-treatment: after vulcanization is completed, the rubber product is taken out and the burrs and excess sulfur are removed; S5: Finished product inspection, physical property test of the rubber fender, check the appearance of the rubber fender to ensure there are no defects; S6: Packaging and storage: Clean the qualified rubber fenders, then pack them and store them in a dry, ventilated and light-proof warehouse.
8. The method for producing the rubber for large ship fenders according to claim 7, It is characterized in that The mixing in S2 includes the following steps: S201: In the plasticizing stage, the weighed natural rubber and bio-based rubber are put into an open mill for plasticizing to soften them; S202: In the mixing stage, carbon black, nano carbon black and calcium carbonate filler are added and mixed until uniform; S203: In the refining stage, zinc oxide, stearic acid, antioxidant, MRT, DPG, coumarone resin and peptizer double T small material are added and mixing is continued; S204: In the sheeting stage, sulfur particles are finally added and mixed evenly before sheeting.
9. The method for producing the rubber for large ship fenders according to claim 8, It is characterized in that The mixing is carried out by a co-rotating twin-screw mixer or a continuous mixer; And / or, the temperature, time and pressure of each mixing stage are different, wherein the temperature of the plasticizing stage is 40-60°C, the time is 5-10 minutes, and the pressure is 1MPa-3MPa; The temperature in the mixing stage is 80-120°C, the time is 10-30 minutes, and the pressure is 3MPa-7MPa; The temperature in the refining stage is 80-120°C, the time is 5-10 minutes, and the pressure is 3-7MPa; The unloading stage adopts the automatic unloading method with a pressure of 3~5MPa.
10. The method for producing the rubber for large ship fenders according to any one of claims 7 to 9, It is characterized in that The pressures at each stage of the segmented vulcanization are different: The pressure in the preheating stage is moderate and maintained in the range of 1-2 MPa; The pressure in the primary vulcanization stage gradually increases and is maintained in the range of 3-5 MPa; The pressure in the intermediate vulcanization stage is appropriately increased and maintained within the range of 5-7 MPa; The pressure in the deep vulcanization stage is maintained or slightly reduced, and maintained in the range of 4-6MPa; The pressure in the post-vulcanization stage is gradually reduced until it reaches zero.
Citation Information
Patent Citations
High-strength rubber fender and manufacturing method thereof
CN111303496A