Coaxial cable cross-linked core wire insulating layer and preparation method thereof
Through the combination of fluoroplastic and azodiformamide and crosslinking of high-energy ray radiation, the problem of inappropriate particle size and high cost of the nucleating agent of the coaxial cable insulating layer is solved, and the cell uniformity and performance improvement is achieved. in high frequency and high temperature environments.
Patent Information
- Application Number
- CN202410889379.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-04
- Publication Date
- 2024-11-22
AI Technical Summary
The nucleating agent of the insulating layer of the existing coaxial cable has problems such as inappropriate particle size, agglomeration phenomenon and high cost, making it difficult to meet the demands of high-frequency coaxial cables for uniform and delicate bubbles and low cost.
Using the nucleating agent component fluoroplastic with low dielectric loss factor and azodiformamide, the coaxial cable crosslinking with excellent foaming performance is prepared by physical foaming extrusion and high-energy irradiation crosslinking. Core wire insulation layer.
It realizes an insulating layer with large cell density and uniform size distribution, improves tensile strength, temperature resistance level and mechanical properties, reduces costs, and is suitable for high-power, high-frequency signal transmission and frequent welding occasions.
Smart Images

Figure CN118994757A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of coaxial cables, and in particular relates to a coaxial cable cross-linked core wire insulation layer and a preparation method thereof. Background Art
[0002] The coaxial cable market has broad prospects. Not only is there a large demand in the field of mobile communication technology, but with the rapid development of high-speed rail technology, the use of coaxial cables in this field has also increased sharply. At present, coaxial cables mainly use physical foamed polyethylene insulation. The insulation layer is composed of a polyethylene melt composed of a matrix resin, a foaming agent, and a nucleating agent. Physical foaming agents such as CO2 and N2 are injected into the polyethylene melt from the air injection port of the fuselage. Under the push of the screw, it is prepared by extrusion foaming.
[0003] As a modification aid in the polyethylene extrusion foaming process, nucleating agents can improve the nucleation efficiency. A small amount of nucleating agents can provide centers with suitable surface energy for the foaming agent, reduce the surface tension of polyethylene, and when a certain mass fraction of effective nucleating agents is added to the polyethylene matrix resin, the bubbles can be dispersed evenly and finely. The mechanism of action of nucleating agents is mainly: in the molten state, the nucleating agent provides the required crystal nuclei, and polyethylene changes from the original homogeneous nucleation to heterogeneous nucleation, which can effectively reduce the bubble nucleation energy barrier and promote bubble nucleation.
[0004] There are many types of nucleating agents on the market. Due to differences in system, dosage, shape, and size, the final foaming results will vary greatly. Currently, commonly used nucleating agents include inorganic nucleating agents such as talcum powder, iron dioxide, and calcium carbonate. However, when using inorganic nucleating agents, agglomeration is easy to occur when the particle size is small, and the number of nucleation points cannot be increased when the particle size is large. Other additives need to be added to enhance the nucleation effect, resulting in increased product quality. At present, most of the organic nucleating agent masterbatches for coaxial cable physical foaming insulation materials in China are imported from abroad. Therefore, it is urgent to independently develop nucleating agent masterbatches for coaxial cable insulation materials and reduce costs. Summary of the invention
[0005] In order to meet the increasing test frequency of mobile communication, the high-frequency coaxial cable with high transmission efficiency is in great demand, which requires the foaming size of the foamed insulation material to be more uniform and the pores to be more delicate, so the nucleating agent with excellent performance in all aspects is crucial. The present invention adopts the compounding of fluoroplastics and azodicarbonamide (AC) with a nucleating agent component with low dielectric loss factor, and fluoroplastics such as polytetrafluoroethylene (PTFE) as an inert nucleating agent have excellent dielectric properties and heat resistance, because of its low surface energy, good dispersibility, and no change in itself during the foaming process, with higher nucleation rate; azodicarbonamide as an active nucleating agent can be thermally decomposed in the extrusion foaming process, and many nucleation points are formed in the polymer melt, and the compounding of the two can ensure the excellent foaming performance of the cable insulation layer, so that the pore density is large and the pore size is evenly distributed.
[0006] To achieve the above objectives, this application provides the following technical solutions:
[0007] The present invention provides a method for preparing a cross-linked core insulation layer of a coaxial cable, wherein a nucleating agent for insulation foaming and a base material are extruded by physical foaming, and then irradiated and cross-linked to obtain a cross-linked core insulation layer of the coaxial cable; the insulation foaming degree of the physical foaming extrusion is 65-70%; the base material is high-density polyethylene;
[0008] The insulating foaming nucleating agent is obtained by melt extrusion; the insulating foaming nucleating agent comprises, by weight, 100 parts of low-density polyethylene, 10-15 parts of fluoroplastic resin, 0.35-0.85 parts of foaming agent and 4-7 parts of cross-linking agent; wherein the fluoroplastic resin is selected from one of polytetrafluoroethylene (PTFE), tetrafluoroethylene and ethylene copolymer (ETFE), and tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer (PFA); and the cross-linking agent is selected from triallyl isocyanurate (TAIC), triallyl cyanurate (TAC) or tris(trimethylolmethacrylate)propane ester.
[0009] Preferably, the radiation cross-linking is performed by irradiating with high-energy rays (α rays, γ rays, electron rays) to break the CH bonds of polyethylene macromolecules to form polyethylene active chains, which are then cross-linked with each other.
[0010] Preferably, the foaming agent is azodicarbonamide.
[0011] Preferably, by weight, the fluoroplastic resin is 12 parts, the foaming agent is 0.5 parts, and the cross-linking agent is 5.5 parts.
[0012] Preferably, the method for preparing the insulating foaming nucleating agent comprises the following steps:
[0013] S1: Mix 100 parts of low-density polyethylene, 10-15 parts of fluoroplastic resin, 0.35-0.85 parts of foaming agent and 4-7 parts of triallyl isocyanurate by weight, and then melt extrude to obtain a plasticized material;
[0014] S2: Cooling and drying the plasticized material, and granulating it to obtain the insulating foaming nucleating agent.
[0015] Preferably, in step S1, the temperature of melt extrusion is 145-155°C.
[0016] Preferably, in step S2, the cooling method is water cooling.
[0017] Preferably, in step S2, the drying method is blow drying.
[0018] Preferably, in step S2, stirring is performed after granulation.
[0019] The present invention also provides a coaxial cable cross-linked core wire insulation layer prepared by the self-made nucleating agent.
[0020] Specifically, the method for preparing the cross-linked core wire insulation layer of the coaxial cable comprises the following steps:
[0021] A) passing the inner conductor through an insulating extruder head, adding a high-density polyethylene (HDPE) base material and the self-made insulating foaming nucleating agent in a feeding section, foaming and extruding an insulating core wire on a physical foaming machine, and injecting an inert gas during foaming, wherein the inert gas concentration is 99.99% and the foaming degree is 65-70%, to obtain an insulating core wire having a foamed high-density polyethylene insulation layer containing a crosslinking agent;
[0022] B) The insulating core wire is irradiated with high-energy gamma rays to cause cross-linking of the foamed high-density polyethylene insulation layer, the irradiation dose is 13-16 Mrd, and the speed is 60-65 m / min, thereby obtaining a polyethylene insulating core wire that has been irradiated and cross-linked.
[0023] The technical solution of the present invention has the following advantages over the prior art:
[0024] 1. The present invention adopts self-made nucleating agent, which can replace imported nucleating agent masterbatch, has low cost and wide application.
[0025] 2. The self-made nucleating agent has good compatibility with the matrix polyethylene insulation, and the foaming layer has fine and dense pores without perforation. The insulating core wire prepared by the nucleating agent of the present invention meets the standard use requirements, and its temperature resistance level is greatly improved and its mechanical properties are significantly improved.
[0026] 3. Preparation of polyethylene insulated core wire: The high-density polyethylene base material is added with the insulating foaming nucleating agent of the present invention, and the insulating core wire is extruded by physical foaming with inert gas. The HDPE foamed insulating core wire generated by it is cross-linked by γ high-energy ray irradiation, so that carbon cross-linking bonds are generated between polyethylene macromolecules, and the active polyethylene chains are cross-linked to form a three-dimensional network structure, which is transformed from thermoplastic to insoluble and infusible thermosetting cross-linked polyethylene, thereby improving the tensile strength, environmental stress cracking resistance, chemical stability and use temperature of the foamed polyethylene. After testing, the tensile strength is increased by about 1.5 times, and the use temperature is increased from the conventional 80°C to 150°C. The above advantages expand the use occasions of the same cable, which can be applied to high-power and high-frequency signal transmission occasions, and can also be applied to frequent welding occasions of coaxial cables. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 This is a 50-fold magnified image of the cross-linked foamed polyethylene insulated core wire prepared in Example 4.
[0028] Figure 2This is a 50-fold magnified image of the cross-linked foamed polyethylene insulated core wire prepared in Example 5.
[0029] Figure 3 This is a 50-fold magnified image of the cross-linked foamed polyethylene insulated core wire prepared in Comparative Example 4. DETAILED DESCRIPTION
[0030] The present invention is further described below in conjunction with the accompanying drawings and specific embodiments so that those skilled in the art can better understand the present invention and implement it, but the embodiments are not intended to limit the present invention.
[0031] Example 1
[0032] The preparation method of the nucleating agent for insulating foaming is as follows:
[0033] A) Ingredients: The weight ratio of materials is: 100 parts of low-density polyethylene as the base resin, 12 parts of polytetrafluoroethylene resin, 0.5 parts of azodicarbonamide (AC) as the foaming agent and 5.5 parts of triallyl isocyanate (TAIC) as the crosslinking agent.
[0034] B) Add the formulated materials to the feeding section of the extruder screw and mix them evenly. Extrude at 150°C to fully plasticize the mixture. After plasticization, cool it with water and blow it dry. After drying, cut and granulate it into white particles. After stirring evenly, weigh and package it for later use. The specific process flow is as follows:
[0035] The raw materials are mixed in proportion → spiral feeding → melt extrusion at 150℃ → water cooling and drying → slitting and granulation → stirring → inspection → weighing → storage.
[0036] Example 2
[0037] The preparation method of the nucleating agent for insulating foaming is as follows:
[0038] A) Ingredients: The weight ratio of materials is: 100 parts of low-density polyethylene as the base resin, 10 parts of polytetrafluoroethylene resin, 0.35 parts of azodicarbonamide (AC) as the foaming agent and 4 parts of triallyl isocyanate (TAIC) as the crosslinking agent.
[0039] B) Add the formulated amount of materials to the feeding section of the extruder screw and mix them evenly. Extrude at 145°C to fully plasticize the mixture. After plasticization, water cool and blow dry. After drying, cut and granulate to form white granules. After stirring evenly, weigh and package for standby use.
[0040] The specific process is as follows:
[0041] The raw materials are mixed in proportion → spiral feeding → melt extrusion → water cooling and drying → slitting and granulation → stirring → inspection → weighing → storage.
[0042] Example 3
[0043] The preparation method of the nucleating agent for insulating foaming is as follows:
[0044] A) Ingredients: The weight ratio of materials is: 100 parts of low-density polyethylene as the base resin, 15 parts of polytetrafluoroethylene resin, 0.85 parts of azodicarbonamide (AC) as the foaming agent and 7 parts of triallyl isocyanate (TAIC) as the crosslinking agent.
[0045] B) Add the formulated amount of materials to the feeding section of the extruder screw and mix them evenly. Extrude at 155°C to fully plasticize the mixture. After plasticization, water cool and blow dry. After drying, cut and granulate to form white granules. After stirring evenly, weigh and package for standby use.
[0046] The specific process is as follows:
[0047] The raw materials are mixed in proportion → spiral feeding → melt extrusion → water cooling and drying → slitting and granulation → stirring → inspection → weighing → storage.
[0048] Example 4
[0049] In the extruder, a high-density polyethylene base material and the insulating foaming nucleating agent prepared in Example 1 are added to the feeding section, and the insulating core wire is foamed and extruded on a physical foaming machine. 300MPa of inert gas is injected during foaming, and the inert gas concentration is 99.99% to obtain a coaxial cable foam insulation layer.
[0050] The insulating core wire is irradiated with high-energy gamma rays to cause cross-linking of the foamed high-density polyethylene insulation layer, with an irradiation dose of 15 Mrd, a speed of 65 m / min, and a foaming degree of 68%, thereby obtaining a cross-linked foamed high-density polyethylene insulating core wire cross-linked by irradiation.
[0051] Example 5
[0052] The difference between Example 5 and Example 4 is that the foaming degree is 70%.
[0053] Comparative Example 1
[0054] The preparation method of the nucleating agent for insulating foaming is as follows:
[0055] A) Ingredients: The weight ratio of materials is: 100 parts of low-density polyethylene as the base resin, 12 parts of fluoroplastic resin, and 0.5 parts of azodicarbonamide (AC) as the foaming agent.
[0056] B) Add the formulated amount of materials to the feeding section of the extruder screw and mix them evenly. Extrude at 150°C to fully plasticize the mixture. After plasticization, water cool and blow dry. After drying, cut and granulate to form white granules. After stirring evenly, weigh and package for standby use.
[0057] The specific process is as follows:
[0058] The raw materials are mixed in proportion → spiral feeding → melt extrusion at 150℃ → water cooling and drying → slitting and granulation → stirring → inspection → weighing → storage.
[0059] In the extruder, the high-density polyethylene base material and the self-made nucleating agent are added to the feeding section, and the insulating core wire is foamed and extruded on the physical foaming machine. 300MPa of inert gas is injected during foaming, and the inert gas concentration is 99.99% to obtain an insulating core wire with a foamed high-density polyethylene insulation layer.
[0060] The insulating core wire is irradiated with high-energy gamma rays to cause cross-linking of the foamed high-density polyethylene insulation layer, the irradiation dose is 15 Mrd, the speed is 65 m / min, the foaming degree is 68%, and a cross-linked foamed high-density polyethylene insulating core wire is obtained.
[0061] Comparative Example 2
[0062] The difference from Comparative Example 1 is that the base resin for foaming is a high-density and low-density mixed polyethylene (wherein the weight ratio of high-density polyethylene to low-density polyethylene is 7:3).
[0063] Comparative Example 3
[0064] The inner conductor is passed through the insulating extruder head, high-density polyethylene insulation and purchased nucleating agent are added to the feeding section, and the insulating core wire is foamed and extruded on a physical foaming machine. 300MPa of inert gas is injected during foaming, and the inert gas concentration is 99.99% to obtain an insulating core wire with a foamed high and low density polyethylene insulation layer.
[0065] The difference from Comparative Example 1 is that the nucleating agent used for foaming is an externally purchased common nucleating agent and does not contain a cross-linking agent.
[0066] Comparative Example 4
[0067] The preparation method of the nucleating agent for insulating foaming is as follows:
[0068] A) Ingredients: The weight ratio of materials is: 100 parts of low-density polyethylene as the base resin, 12 parts of fluoroplastic resin, and 5.5 parts of triallyl isocyanate (TAIC), a cross-linking agent.
[0069] B) Add the formulated amount of materials to the feeding section of the extruder screw and mix them evenly. Extrude at 150°C to fully plasticize the mixture. After plasticization, water cool and blow dry. After drying, cut and granulate to form white granules. After stirring evenly, weigh and package for standby use.
[0070] The specific process is as follows:
[0071] The raw materials are mixed in proportion → spiral feeding → melt extrusion at 150℃ → water cooling and drying → slitting and granulation → stirring → inspection → weighing → storage.
[0072] In the extruder, the high-density polyethylene base material and the self-made nucleating agent are added to the feeding section, and the insulating core wire is foamed and extruded on the physical foaming machine. 300MPa of inert gas is injected during foaming, and the inert gas concentration is 99.99% to obtain an insulating core wire with a foamed high-density polyethylene insulation layer.
[0073] The insulating core wire is irradiated with high-energy gamma rays to cause cross-linking of the foamed high-density polyethylene insulation layer, the irradiation dose is 15 Mrd, the speed is 65 m / min, the foaming degree is 68%, and a cross-linked foamed high-density polyethylene insulating core wire is obtained.
[0074] Effect evaluation 1
[0075] Sample No. 1 is comparative example 1, which uses full high-density polyethylene insulation, a nucleating agent without a cross-linking agent, and is directly irradiated to 15 Mrad;
[0076] Sample No. 2 is comparative example 2, which uses high-density and low-density mixed polyethylene insulation, and the nucleating agent is directly irradiated to 15 Mrad without adding a cross-linking agent;
[0077] Sample No. 3 is Example 4 of the present invention;
[0078] Sample No. 4 is comparative example 3, which uses full high-density polyethylene insulation, the nucleating agent is purchased from outside, and is not irradiated and cross-linked.
[0079] A) Insulation temperature resistance test
[0080] Table 1 Electric soldering iron test
[0081]
[0082] Table 2 High temperature box test
[0083]
[0084] The heat resistance test shows that sample No. 3 has higher heat resistance than the other three samples. Its shrinkage is the smallest at 150°C, which meets the standard requirements. The shrinkage of the other three samples exceeds the standard requirements. At 300°C, sample No. 3 is slightly damaged. Therefore, the operating temperature of Example 4 can reach 150°C, and the heat resistance level is greatly improved.
[0085] B) Insulation tensile strength test
[0086] Table 3 Mechanical properties test
[0087] Test samples <![CDATA[Tensile strength Mpa > Sample No. 1 6.7 Sample No. 2 6.4 Sample No. 3 8.7 Sample No. 4 5.8
[0088] Mechanical properties tests show that the tensile strength of insulation is improved to a certain extent after radiation cross-linking. Samples 1 and 2 are about 1.2 times higher than the uncross-linked sample 4, and sample 3 is 1.5 times higher than the uncross-linked sample 4. The mechanical properties are significantly improved.
[0089] Effect evaluation 2
[0090] Table 4 Comparison of properties of polyethylene foam with different nucleating agents
[0091] project Example 4 Example 5 Comparative Example 4 <![CDATA[Density (before foaming) g / cm -3 > 0.94 0.94 0.94 <![CDATA[Density (after foaming) g / cm -3 > 0.30 0.28 0.25 Foaming multiple 3.13 3.36 3.76 Foaming degree 68% 70% 73% Average bubble diameter / μm 300 410 495 Foaming effect Fine pores and uniform bubble diameter Large bubble diameter and uniform pores The bubble diameter is large, and the bubble pores have collapsed penetration
[0092] The foaming test results show that after the AC foaming agent is removed from Comparative Example 4, the cells are rough, uneven in size, and have broken cells, indicating that a single fluoroplastic inert nucleating agent is not conducive to uniform cell size. The compound system provided by the present invention is conducive to finer cells and better transmission performance. Both Example 4 and Example 5 can be used normally, meeting the requirements of high-end communication systems such as high temperature resistance, high power, and high-frequency signal transmission.
[0093] Obviously, the above embodiments are merely examples for clear explanation and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived from these are still within the protection scope of the invention.
Claims
1. A method for preparing a cross-linked core insulation layer of a coaxial cable, It is characterized in that The insulating foaming nucleating agent and the base material are extruded by physical foaming, and then irradiated and cross-linked to obtain the cross-linked core wire insulation layer of the coaxial cable; the insulation foaming degree of the physical foaming extrusion is 65-70%; and the base material is high-density polyethylene; The insulating foaming nucleating agent is obtained by melt extrusion; in parts by weight, the insulating foaming nucleating agent comprises 100 parts of low-density polyethylene, 10-15 parts of fluoroplastic resin, 0.35-0.85 parts of foaming agent and 4-7 parts of cross-linking agent; wherein the fluoroplastic resin is selected from one of polytetrafluoroethylene, tetrafluoroethylene and ethylene copolymer, tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer; the cross-linking agent is selected from triallyl isocyanurate, triallyl cyanurate or tri(trimethylolmethacrylate)propane ester.
2. The preparation method according to claim 1, It is characterized in that The radiation cross-linking uses high-energy gamma rays to break the CH bonds of polyethylene macromolecules to form polyethylene active chains, which are then cross-linked with each other.
3. The preparation method according to claim 1, It is characterized in that The foaming agent is azodicarbonamide.
4. The preparation method according to claim 1, It is characterized in that By weight, the fluoroplastic resin is 12 parts, the foaming agent is 0.5 parts, and the cross-linking agent is 5.5 parts.
5. A preparation method according to any one of claims 1 to 4, It is characterized in that The preparation method of the nucleating agent for insulating foaming comprises the following steps: S1: Mix 100 parts of low-density polyethylene, 10-15 parts of fluoroplastic resin, 0.35-0.85 parts of foaming agent and 4-7 parts of triallyl isocyanurate by weight, and then melt extrude to obtain a plasticized material; S2: Cooling and drying the plasticized material, and granulating it to obtain the insulating foaming nucleating agent.
6. The preparation method according to claim 5, It is characterized in that In the step S1, the temperature of the melt extrusion is 145-155°C.
7. The preparation method according to claim 5, It is characterized in that In step S2, the cooling method is water cooling.
8. The preparation method according to claim 5, It is characterized in that In step S2, the drying method is blow drying.
9. The preparation method according to claim 5, It is characterized in that In the step S2, stirring is performed after granulation.
10. The cross-linked core wire insulation layer of the coaxial cable prepared by the preparation method according to any one of claims 1 to 9.