Polypropylene composite material as well as preparation method and application thereof

By adding mica, flake graphite and alpha nucleating agent to polypropylene, the strength and dynamic friction performance of polypropylene composite materials are improved, and the problems of demand in demand and high price of polyformaldehyde are solved, and the performance and low cost of polyformaldehyde are achieved. Effect.

CN118994774APending Publication Date: 2024-11-22EAST ASIA ELECTRICAL EQUIP CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310547253.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-16
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The problem of supply and high price of polyformaldehyde has caused environmental supervision in production plants, resulting in temporary shutdowns and high costs.

Method used

By adding mica, flake graphite and α nucleating agent to the polypropylene matrix, the strength, modulus and dynamic friction properties of the polypropylene composite material are improved, making it comparable to polyformaldehyde, and the formation of stable use of high-crystalline polypropylene and α nucleating agent is carried out. The alpha crystal form increases the tensile strength and damage resistance of the material, and forms a solid surface and multi-layer structure during injection molding.

Benefits of technology

The polypropylene composite material has a low cost and a comparable performance to polyformaldehyde, and can be used as a substitute in electronics, automotive parts and industrial mechanical devices, reducing production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004229997890000011
    Figure BDA0004229997890000011
  • Figure BDA0004229997890000031
    Figure BDA0004229997890000031
  • Figure BDA0004229997890000041
    Figure BDA0004229997890000041
Patent Text Reader

Abstract

The invention relates to a polypropylene composite material as well as a preparation method and application thereof. The polypropylene composite material comprises the following components in parts by weight: 90-96 parts of polypropylene, 2-5 parts of mica, 2-5 parts of crystalline flake graphite, 0.1-0.4 part of an alpha nucleating agent and 0-1 part of other additives. The high-crystallinity homo-polypropylene is adopted, and the alpha nucleating agent is added, so that the crystallinity of the material is improved, a stable alpha crystal form is formed, the tensile strength of the material is improved, and the damage resistance is improved; meanwhile, the mica and the crystalline flake graphite are added, so that the rigidity and the dimensional stability of the material are improved, the material is endowed with certain self-lubricating property, parts formed by the material have good dimensional stability and lubricating property, and the material can replace POM materials in some application fields.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polymer composite materials, in particular to a polypropylene composite material and a preparation method and application thereof. Background Art

[0002] Polyoxymethylene (POM), also known as acetal resin, polyoxymethylene, and polyacetal, is a thermoplastic crystalline polymer known as "super steel" or "sport steel". It is an engineering plastic with excellent comprehensive performance, high mechanical properties such as strength, modulus, wear resistance, toughness, fatigue resistance and creep resistance, as well as excellent electrical insulation, solvent resistance and processability. It is widely used in electronic appliances, automotive parts, industrial machinery and devices, etc. However, due to the VOC problem in the production process of polyoxymethylene, production plants are often subject to supervision by government environmental protection departments, and are prone to temporary suspension of production for rectification, resulting in a shortage of polyoxymethylene resin and high prices. Therefore, it is necessary to seek a low-cost alternative product with comparable performance to polyoxymethylene.

[0003] Polypropylene (PP) and polyoxymethylene belong to the five major general-purpose engineering plastics. Polypropylene has the advantages of low production cost, good comprehensive mechanical properties, non-toxicity, corrosion resistance, and easy recycling. It is widely used in chemical, construction, packaging, automobile and other fields.

[0004] Therefore, polypropylene is modified so that its properties (including strength, modulus, toughness, dynamic friction performance, etc.) are equivalent to those of polyoxymethylene, and it can be used as a substitute for polyoxymethylene to reduce costs. Summary of the invention

[0005] Based on this, the purpose of the present invention is to provide a polypropylene composite material with equivalent strength and wear resistance to polyoxymethylene in order to solve the problem that the existing polyoxymethylene is in short supply and expensive. The present invention adds mica, flake graphite and a nucleating agent to a polypropylene matrix, so that the obtained polypropylene composite material has equivalent strength, modulus and dynamic friction performance to those of polyoxymethylene.

[0006] A polypropylene composite material comprises the following components calculated in parts by weight:

[0007]

[0008] The polypropylene composite material adopts high crystalline polypropylene and adds an α nucleating agent to improve the crystallinity of the material, forming a stable α crystal form, increasing the tensile strength of the material and improving the ability to resist damage. The mica and flake graphite added in the present invention further improve the tensile strength and bending modulus of the polypropylene material. A small amount of the added mica and flake graphite will migrate to the surface of the polypropylene material during the injection molding process to form a solid surface, and under the action of the multi-layer structure of the flake graphite, it has good lubricity and wear resistance.

[0009] Conventional α nucleating agents can be used in the present invention, and the α nucleating agent includes but is not limited to at least one of an aromatic amine nucleating agent or an aromatic phosphate nucleating agent. The α nucleating agent is more stable than the β nucleating agent, so that the crystallization performance of the obtained polypropylene is also more stable.

[0010] In one of the embodiments, the melt mass flow rate of the polypropylene at 230° C. and a load of 2.16 kg is 5 to 50 g / 10 min.

[0011] In one embodiment, the mesh number of the mica is greater than 325 mesh.

[0012] In one embodiment, the mesh number of the flake graphite is greater than 325 mesh.

[0013] In one embodiment, the diameter of the glass fiber is ≤13 μm.

[0014] In one embodiment, the α-nucleating agent is at least one of an aromatic amine nucleating agent or an aromatic phosphate nucleating agent.

[0015] In one embodiment, the other additives include at least one of an antioxidant, a light stabilizer or a lubricant.

[0016] The present invention also provides a method for preparing a polypropylene composite material, which is characterized by comprising the following steps: uniformly mixing polypropylene, mica, flake graphite, α nucleating agent and other additives, and melt-extruding at 180-230° C. to obtain the polypropylene composite material.

[0017] In one embodiment, the mixing is performed in a high-speed mixer.

[0018] In one embodiment, the melt extrusion is carried out in a twin-screw extruder, the screw aspect ratio of the twin-screw extruder is (48-56):1, and the screw speed is 350-450 rpm.

[0019] The present invention also provides an application of the polypropylene composite material in the preparation of electronic appliances, automobile parts or industrial machinery devices.

[0020] Compared with the prior art, the present invention has the following beneficial effects:

[0021] The polypropylene composite material of the present invention adopts low-flow polypropylene and adds an alpha nucleating agent to improve the crystallinity of the material, form a stable alpha crystal form, increase the tensile strength of the material, improve the ability to resist damage, and the physical properties can be equivalent to those of polyoxymethylene, and the cost is low. The tensile strength of the polypropylene composite material of the present invention can be maintained at 40-47MPa, the impact strength can be maintained at 4.2-5.9MPa, and the molding shrinkage rate can be maintained at 0.17-0.20%, which is equivalent to the performance of polyoxymethylene. DETAILED DESCRIPTION

[0022] To better illustrate the purpose, technical solutions and advantages of the present invention, the present invention will be further described below in conjunction with specific examples, but the examples do not limit the present invention in any form. Unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in the art. Unless otherwise specified, the reagents and materials used in the present invention are commercially available.

[0023] The following raw materials are selected in the embodiments of the present invention:

[0024] Polypropylene:

[0025] PP1, C30S, at 230℃, 2.16kg load, melt index 5g / 10min, Liaoning Huajin;

[0026] PP2, HP500N, at 230℃, 2.16kg load, melt index 11.5g / 10min, CNOOC Shell;

[0027] PP3, Z30S, at 230℃, 2.16kg load, melt index 25g / 10min, Zhenhai Refining and Chemical;

[0028] PP4, H9018, at 230℃, 2.16kg load, melt index 51g / 10min, Lanzhou Petrochemical.

[0029] Flake Graphite

[0030] Mica, 325 mesh, Qingdao Tianheda Graphite Co., Ltd.

[0031] Aryl phosphate nucleating agent, NA-11, was purchased from Aidico.

[0032] Other additives:

[0033] Antioxidant 1010: commercially available;

[0034] Antioxidant 168: Commercially available;

[0035] PTFE: Dongguan Lixin Plastics;

[0036] Lubricant: Calcium stearate, commercially available.

[0037] It should be noted that, in the present invention, the above-mentioned other additives (such as antioxidants and lubricants) are the same substance in parallel tests.

[0038] Examples 1 to 8

[0039] The embodiments of the present invention provide a series of polypropylene composite materials, which are prepared according to a preparation method comprising the following steps:

[0040] According to the formulation in Tables 1 and 2, polypropylene, α-nucleating agent and other additives are added to a high-speed mixer, mixed evenly, and then fed into a twin-screw extruder (screw aspect ratio is 48:1), the screw speed is 350-450 rpm, and melt extrusion is performed at 170-230° C. (wherein, the temperatures of the zones from the die to the discharge port in the twin-screw extruder are: the temperatures of the ten zones from the feeding section to the die are 170° C., 180° C., 190° C., 200° C., 210° C., 210° C., 210° C., 220° C., and 230° C., respectively), to obtain the polypropylene composite material.

[0041] Table 1 Raw material formula of polypropylene composite material of embodiment 1~8 (weight part)

[0042]

[0043] Comparative Example 1

[0044] This comparative example provides a polypropylene composite material, which is prepared according to the preparation method of Example 5. The difference from Example 1 is that the polypropylene is replaced by PP5 with a lower melt mass flow rate.

[0045] Comparative Example 2

[0046] This comparative example provides a polypropylene composite material, which is prepared according to the preparation method of Example 5. The difference from Example 1 is that the polypropylene is replaced by PP6 with a higher melt mass flow rate.

[0047] Comparative Example 3

[0048] This comparative example provides a polypropylene composite material, which is prepared according to the preparation method of Example 5. The difference from Example 5 is that the formula does not contain mica.

[0049] Comparative Example 4

[0050] This comparative example provides a polypropylene composite material, which is prepared according to the preparation method of Example 5. The difference from Example 5 is that the formula does not contain flake graphite.

[0051] Comparative Example 5

[0052] This comparative example provides a polypropylene composite material, which is prepared according to the preparation method of Example 5. The difference from Example 5 is that the formula does not contain mica and flake graphite.

[0053] Comparative Example 6

[0054] This comparative example provides a polypropylene composite material, which is prepared according to the preparation method of Example 5. The difference from Example 5 is that the formula does not contain PTFE.

[0055] Comparative Example 7

[0056] This comparative example provides a polypropylene composite material, which is prepared according to the preparation method of Example 5. The difference from Example 5 is that the mica in the formula is replaced by talc.

[0057] Table 2

[0058]

[0059]

[0060] Experimental example

[0061] The properties of the polypropylene composite materials and polyoxymethylene (M90, purchased from Yuntianhua) obtained in the above examples and comparative examples were tested. The specific test items, test methods and results are as follows:

[0062] 1. Tensile strength (MPa): The composite material was injection molded into a tensile specimen (IB type), and the test was carried out according to the method in the standard "ISO527-1-2010". The tensile strength was 50 mm / min at room temperature (25°C). The test results are shown in Table 3.

[0063] 2. Bending properties: The composite materials were injection molded into impact specimens, and the bending strength (MPa) and bending modulus (MPa) were tested according to the method in the standard "ISO178-2011". The test results are shown in Table 3;

[0064] 3. Toughness: The composite materials were injection molded into impact specimens and tested according to the method in ISO179-2010. The notch type of the specimen was A-type. The notch impact strength (kJ / m 2 ), the test results are shown in Table 3;

[0065] 4. Dynamic friction coefficient: GB / T-10006-2021, test speed 100±10mm / min.

[0066] Table 3 Performance test results

[0067]

[0068] From the above results we can see that:

[0069] The physical property bending modulus of the polypropylene composite material prepared in each embodiment of the present invention is equivalent to that of polyoxymethylene, and the dynamic friction coefficient is at the same level as that of polyoxymethylene. It can be used as a substitute for polyoxymethylene in related application fields to reduce production costs.

[0070] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0071] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A polypropylene composite material, characterized in that: The composition includes the following components calculated by weight:

2. The polypropylene composite material according to claim 1, characterized in that: The melt mass flow rate of the polypropylene at 230° C. and a load of 2.16 kg is 5 to 50 g / 10 min.

3. The polypropylene composite material according to claim 1, characterized in that: The mesh number of the mica is greater than 325 meshes.

4. The polypropylene composite material according to claim 1, characterized in that: The mesh number of the flake graphite is greater than 325 meshes.

5. The polypropylene composite material according to claim 1, characterized in that: The diameter of the glass fiber is ≤13 μm.

6. The polypropylene composite material according to claim 1, characterized in that: The α nucleating agent is at least one of an aromatic amine nucleating agent or an aromatic phosphate nucleating agent.

7. The polypropylene composite material according to claim 1, characterized in that: The other additives include at least one of an antioxidant, a light stabilizer or a lubricant.

8. The method for preparing the polypropylene composite material according to any one of claims 1 to 7, characterized in that: The method comprises the following steps: uniformly mixing polypropylene, mica, flake graphite, alpha nucleating agent and other additives, and then melt-extruding at 180-230 DEG C to obtain the polypropylene composite material.

9. Use of the polypropylene composite material according to any one of claims 1 to 7 in the preparation of electronic appliances, automobile parts or industrial machinery devices.