Automobile rubber material and preparation method thereof

By combining specific rubber materials and additives, the problems of strong odor, easy wear and poor elasticity of traditional rubber materials under high temperature conditions have been solved, and automotive rubber materials with wear resistance, high safety and good air permeability have been prepared.

CN118994800APending Publication Date: 2024-11-22GUANGXI UNIVERSITY OF TECHNOLOGY
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411361953.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-27
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

Traditional rubber materials have a strong pungent odor, are easily worn, are not breathable, have poor elasticity, and are flammable under high-temperature environments, posing safety hazards.

Method used

Rubber materials for automobiles are prepared by combining EPDM rubber, methyl vinyl phenyl silicone rubber, natural rubber, epoxidized natural rubber, anti-aging agents, lignin, pretreated plant fibers, seaweed extract, bamboo leaf extract, nano zinc oxide, activated carbon, and modified bentonite through a specific process.

Benefits of technology

The prepared rubber material is wear-resistant, highly safe, breathable, elastic, and non-flammable, making it suitable for automotive interior materials and significantly improving user experience and safety performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005065148580000081
    Figure BDA0005065148580000081
Patent Text Reader

Abstract

The invention discloses an automobile rubber material and a preparation method thereof, and relates to the technical field of rubber material preparation. The invention discloses a rubber material for automobiles. Comprising the following raw materials in parts by weight: 60-70 parts of ethylene propylene diene monomer, 6-10 parts of methyl vinyl phenyl silicone rubber, 30-40 parts of natural rubber, 8-10 parts of epoxidized natural rubber, 2-4 parts of an anti-aging agent, 2-4 parts of sulfur, 2-4 parts of lignin, 2-4 parts of pretreated plant fibers, 10-20 parts of a seaweed extract, 5-10 parts of a bamboo leaf extract, 1-2 parts of nano zinc oxide and 1-2 parts of activated carbon. 10-30 parts of modified bentonite and 1-3 parts of carbon black. The invention also provides a preparation method of the automobile rubber material. The rubber material provided by the invention has the advantages of wear resistance, high safety and the like, and effectively solves the problems of strong pungent smell, easy wear, poor elasticity and the like in the prior art.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of rubber material preparation, and in particular to a rubber material for automobiles and a preparation method thereof. Background Art

[0002] Rubber is an important part of the chemical industry. Rubber products such as tires, hoses, tapes, rubber rollers, rubber seals, and tape products are widely used in various industries of the national economy, such as automobile production, aircraft manufacturing, crude oil transportation, electronic communications, and hospitals, and have become one of the important basic industries.

[0003] With the continuous development of society, people's demand for rubber is increasing, but the pungent smell of traditional rubber has always troubled users. Especially in relatively closed spaces under high temperature conditions, such as the driving room of a car, the pungent smell of rubber will be very strong and will gradually accumulate to disturb the driver and passengers. In severe cases, it can cause nausea, vomiting and even car accidents. At the same time, there are defects such as easy wear, airtightness, poor elasticity and flammability, which pose certain safety hazards. Summary of the invention

[0004] In order to solve the above technical problems, the purpose of the present invention is to provide a rubber material for automobiles and a preparation method thereof. The rubber material has the advantages of wear resistance and high safety, and effectively solves the problems of strong irritating odor, easy wear and poor elasticity in the prior art.

[0005] The technical solution of the present invention to solve the above technical problems is as follows: a rubber material for automobiles is provided, comprising the following raw materials in parts by weight: 60-70 parts of ethylene propylene diene rubber, 6-10 parts of methyl vinyl phenyl silicone rubber, 30-40 parts of natural rubber, 8-10 parts of epoxidized natural rubber, 2-4 parts of antioxidant, 2-4 parts of sulfur, 2-4 parts of lignin, 2-4 parts of pretreated plant fibers, 10-20 parts of seaweed extract, 5-10 parts of bamboo leaf extract, 1-2 parts of nano zinc oxide, 1-2 parts of activated carbon, 10-30 parts of modified bentonite and 1-3 parts of carbon black.

[0006] Furthermore, the rubber material for automobiles includes the following raw materials in parts by weight: 65 parts of ethylene propylene diene monomer rubber, 8 parts of methyl vinyl phenyl silicone rubber, 36 parts of natural rubber, 9 parts of epoxidized natural rubber, 3 parts of antioxidant, 3 parts of sulfur, 3 parts of lignin, 3 parts of pretreated plant fiber, 15 parts of seaweed extract, 7 parts of bamboo leaf extract, 1 part of nano zinc oxide, 2 parts of activated carbon, 20 parts of modified bentonite and 2 parts of carbon black.

[0007] Furthermore, the pretreated plant fiber is prepared by the following method: adding bamboo fiber to cellulase for 2-3 hours, then microwave-treating it at 2-3kW for 1-2 minutes, then adding it to ethanol together with nano-silica and silane coupling agent for vacuum impregnation for 1-2 hours, and drying to obtain the pretreated plant fiber.

[0008] Furthermore, the mass ratio of bamboo fiber, cellulase, nano-silica, silane coupling agent and ethanol is 30:200-300:1-2:5-6:50-100.

[0009] Furthermore, the seaweed extract is prepared by the following method: the seaweed is crushed and added into 4-8 times its weight of water, then ultrasonically extracted at 50-60°C for 0.5-1h, then an equal amount of mixed solvent is added for extraction for 24h, and rotary evaporated at 70-80°C for 5-6h to obtain the seaweed extract.

[0010] Furthermore, in the mixed solvent, the volume ratio of methanol, chloroform and water is 4:3:1.

[0011] Furthermore, the bamboo leaf extract is prepared by the following method: the bamboo leaves are crushed and added into 20-50 times the mass of water, stirred evenly, and then microwaved at 0.5-1.5 kW for 2-4 hours, and filtered; the filtered residue is then immersed in anhydrous ethanol, ultrasonically extracted at 50-60° C. for 0.5-1 hour, filtered, the two filtrates are combined, and dried to obtain the bamboo leaf extract.

[0012] Furthermore, the epoxidation degree of the epoxidized natural rubber is 20-40.

[0013] Furthermore, the antioxidant is a p-phenylenediamine antioxidant.

[0014] The present invention also provides a method for preparing the above-mentioned automotive rubber material, comprising the following steps:

[0015] (1) mixing ethylene propylene diene monomer rubber, methyl vinyl phenyl silicone rubber, natural rubber, epoxidized natural rubber, seaweed extract, bamboo leaf extract, modified bentonite and carbon black at 50-80° C. for 0.5-1 h to obtain a mixture;

[0016] (2) adding an anti-aging agent, sulfur, lignin, pretreated plant fiber, nano zinc oxide and activated carbon to the mixture obtained in step (1), mixing at 70-90° C. for 0.2-0.5 h, and sequentially stretching, extruding and hot pressing to obtain a rubber material for automobiles.

[0017] The present invention has the following beneficial effects:

[0018] 1. The rubber material of the present invention has heat resistance, aging resistance, wear resistance and good comprehensive performance, good elasticity and non-flammability, and is suitable for application in automobile interior materials, effectively solving the problems of strong irritating odor, easy wear, poor elasticity and flammability in the prior art.

[0019] 2. In the rubber materials for automobiles, EPDM rubber is matched with methyl vinyl phenyl silicone rubber, natural rubber and epoxidized natural rubber. Both EPDM rubber and natural rubber side chains contain unsaturated double bonds, which have good heat resistance and anti-aging properties. Epoxidized natural rubber not only retains the double bond structure, but also introduces polar epoxy groups, which can improve the heat resistance and anti-aging ability together with other rubbers. At the same time, the addition of lignin and pretreated fibers enhances the elasticity of rubber materials, improves the comfort and safety performance of rubber materials, and the rubber materials can be widely used in various automotive interior materials; and lignin and pretreated fibers can also form a mesh structure in rubber materials, thereby improving the tensile strength and toughness of rubber materials, and improving the comprehensive performance of materials. The pretreated fibers are obtained by treating bamboo fibers with cellulase and microwaves. The fibers have the advantages of loose structure, rich internal pores and strong elasticity, have certain sound absorption and shock absorption capabilities, and further improve the elasticity and comfort of rubber materials. They are very suitable for the use of automotive interior materials, and the treatment of nano-silica and silane coupling agents can also improve the overall mechanical strength, which is convenient for extending the service life of rubber materials.

[0020] 3. The addition of activated carbon makes the rubber material have a certain ability to adsorb and treat volatile or irritating odors; the use of seaweed extract can further improve the adsorption and purification capacity of activated carbon, avoid irritating or volatile odors when the rubber material is used, and seaweed extract can also improve the anti-aging ability of EPDM rubber and natural rubber, further enhancing the service life of rubber materials. The bamboo leaf extract contains bamboo leaf polysaccharides and bamboo leaf flavonoids, which have good biological activity and can play an anti-aging role; the joint use of seaweed extract and bamboo leaf extract, combined with EPDM rubber and natural rubber, significantly improves the heat resistance and anti-aging ability of rubber materials, and expands the application prospects of rubber materials. DETAILED DESCRIPTION

[0021] The principles and features of the present invention are described below, and the examples are only used to explain the present invention and are not used to limit the scope of the present invention. If no specific conditions are specified in the embodiments, they are carried out according to normal conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments is not specified, they are all conventional products that can be purchased commercially.

[0022] Example 1

[0023] A rubber material for automobiles comprises the following raw materials in parts by weight: 60 parts of ethylene propylene diene monomer rubber, 6 parts of methyl vinyl phenyl silicone rubber, 30 parts of natural rubber, 8 parts of epoxidized natural rubber (epoxy degree 30), 2 parts of anti-aging agent (p-phenylenediamine), 2 parts of sulfur, 2 parts of lignin, 2 parts of pretreated plant fibers, 10 parts of seaweed extract, 5 parts of bamboo leaf extract, 1 part of nano zinc oxide, 1 part of activated carbon, 10 parts of modified bentonite and 1 part of carbon black.

[0024] The pretreated plant fiber is prepared by the following method: adding bamboo fiber to cellulase for 2 hours, then microwave-treating it at 2kW for 1 minute, then adding it to ethanol together with nano-silica and silane coupling agent for vacuum impregnation for 1 hour, and drying to obtain the pretreated plant fiber. The mass ratio of bamboo fiber, cellulase, nano-silica, silane coupling agent and ethanol is 30:200:1:5:50.

[0025] The seaweed extract was prepared by the following method: the seaweed was crushed and added to 4 times the weight of water, then ultrasonically extracted at 50°C for 0.5h, then an equal amount of mixed solvent was added for extraction for 24h, and rotary evaporated at 70°C for 5h to obtain the seaweed extract. In the mixed solvent, the volume ratio of methanol, chloroform and water was 4:3:1.

[0026] The bamboo leaf extract is prepared by the following method: the bamboo leaves are crushed and added into 20 times the mass of water, stirred evenly, then microwaved at 0.5 kW for 2 hours, and filtered; the filtered residue is then immersed in anhydrous ethanol, ultrasonically extracted at 50° C. for 0.5 hours, filtered, the two filtrates are combined, and dried to obtain the bamboo leaf extract.

[0027] The method for preparing the above-mentioned rubber material for automobiles comprises the following steps:

[0028] (1) mixing ethylene propylene diene monomer rubber, methyl vinyl phenyl silicone rubber, natural rubber, epoxidized natural rubber, seaweed extract, bamboo leaf extract, modified bentonite and carbon black at 50° C. for 0.5 h to obtain a mixture;

[0029] (2) adding an antioxidant, sulfur, lignin, pretreated plant fiber, nano zinc oxide and activated carbon to the mixture obtained in step (1), mixing at 70° C. for 0.2 h, and sequentially stretching, extruding and hot pressing to obtain a rubber material for automobiles.

[0030] Example 2

[0031] A rubber material for automobiles comprises the following raw materials in parts by weight: 65 parts of EPDM rubber, 8 parts of methyl vinyl phenyl silicone rubber, 36 parts of natural rubber, 9 parts of epoxidized natural rubber (epoxy degree 30), 3 parts of an antioxidant, 3 parts of sulfur, 3 parts of lignin, 3 parts of pretreated plant fibers, 15 parts of seaweed extract, 7 parts of bamboo leaf extract, 1 part of nano zinc oxide, 2 parts of activated carbon, 20 parts of modified bentonite and 2 parts of carbon black.

[0032] The pretreated plant fiber is prepared by the following method: adding bamboo fiber to cellulase for 2 hours, then microwave-treating it at 2 kW for 2 minutes, then adding it to ethanol together with nano-silica and silane coupling agent for vacuum impregnation for 2 hours, and drying to obtain the pretreated plant fiber. The mass ratio of bamboo fiber, cellulase, nano-silica, silane coupling agent and ethanol is 30:250:1:6:80.

[0033] The seaweed extract is prepared by the following method: the seaweed is crushed and added to 4-8 times the weight of water, then ultrasonically extracted at 55°C for 0.5h, then an equal amount of mixed solvent is added for extraction for 24h, and rotary evaporated at 75°C for 6h to obtain the seaweed extract. In the mixed solvent, the volume ratio of methanol, chloroform and water is 4:3:1.

[0034] The bamboo leaf extract is prepared by the following method: the bamboo leaves are crushed and added into 30 times the mass of water, stirred evenly, and then microwaved for 3 hours under 1kW conditions, and filtered; the filtered residue is then immersed in anhydrous ethanol, ultrasonically extracted at 55°C for 0.7 hours, filtered, the two filtrates are combined, and dried to obtain the bamboo leaf extract.

[0035] The method for preparing the above-mentioned rubber material for automobiles comprises the following steps:

[0036] (1) mixing ethylene propylene diene monomer rubber, methyl vinyl phenyl silicone rubber, natural rubber, epoxidized natural rubber, seaweed extract, bamboo leaf extract, modified bentonite and carbon black at 60° C. for 0.7 h to obtain a mixture;

[0037] (2) adding an antioxidant, sulfur, lignin, pretreated plant fiber, nano zinc oxide and activated carbon to the mixture obtained in step (1), mixing at 80° C. for 0.3 h, and sequentially stretching, extruding and hot pressing to obtain a rubber material for automobiles.

[0038] Example 3

[0039] A rubber material for automobiles comprises the following raw materials in parts by weight: 68 parts of ethylene propylene diene monomer rubber, 8 parts of methyl vinyl phenyl silicone rubber, 37 parts of natural rubber, 9 parts of epoxidized natural rubber (epoxy degree 30), 3 parts of anti-aging agent (p-phenylenediamine), 3 parts of sulfur, 3 parts of lignin, 3 parts of pretreated plant fiber, 18 parts of seaweed extract, 8 parts of bamboo leaf extract, 2 parts of nano zinc oxide, 2 parts of activated carbon, 25 parts of modified bentonite and 2 parts of carbon black.

[0040] The pretreated plant fiber is prepared by the following method: adding bamboo fiber to cellulase for 3 hours, then microwave-treating it at 2.5 kW for 2 minutes, then adding it to ethanol together with nano-silica and silane coupling agent for vacuum impregnation for 2 hours, and drying to obtain the pretreated plant fiber. The mass ratio of bamboo fiber, cellulase, nano-silica, silane coupling agent and ethanol is 30:260:2:6:90.

[0041] The seaweed extract was prepared by the following method: the seaweed was crushed and added to 7 times the weight of water, then ultrasonically extracted at 55°C for 0.8h, then an equal amount of mixed solvent was added for extraction for 24h, and rotary evaporated at 75°C for 6h to obtain the seaweed extract. In the mixed solvent, the volume ratio of methanol, chloroform and water was 4:3:1.

[0042] The bamboo leaf extract is prepared by the following method: the bamboo leaves are crushed and added into 40 times the mass of water, stirred evenly, and then microwaved for 3 hours under 1.2 kW conditions, and filtered; the filtered residue is then immersed in anhydrous ethanol, ultrasonically extracted at 58° C. for 0.8 hours, filtered, the two filtrates are combined, and dried to obtain the bamboo leaf extract.

[0043] The method for preparing the above-mentioned rubber material for automobiles comprises the following steps:

[0044] (1) mixing ethylene propylene diene monomer rubber, methyl vinyl phenyl silicone rubber, natural rubber, epoxidized natural rubber, seaweed extract, bamboo leaf extract, modified bentonite and carbon black at 70° C. for 0.8 h to obtain a mixture;

[0045] (2) adding an antioxidant, sulfur, lignin, pretreated plant fiber, nano zinc oxide and activated carbon to the mixture obtained in step (1), mixing at 85° C. for 0.4 h, and sequentially stretching, extruding and hot pressing to obtain a rubber material for automobiles.

[0046] Example 4

[0047] A rubber material for automobiles comprises the following raw materials in parts by weight: 70 parts of ethylene propylene diene monomer rubber, 10 parts of methyl vinyl phenyl silicone rubber, 40 parts of natural rubber, 10 parts of epoxidized natural rubber (epoxy degree 30), 4 parts of anti-aging agent (p-phenylenediamine), 4 parts of sulfur, 4 parts of lignin, 4 parts of pretreated plant fiber, 20 parts of seaweed extract, 10 parts of bamboo leaf extract, 2 parts of nano zinc oxide, 2 parts of activated carbon, 30 parts of modified bentonite and 3 parts of carbon black.

[0048] The pretreated plant fiber is prepared by the following method: adding bamboo fiber to cellulase for 3 hours, then microwave-treating it at 3 kW for 2 minutes, then adding it to ethanol together with nano-silica and silane coupling agent for vacuum impregnation for 2 hours, and drying to obtain the pretreated plant fiber. The mass ratio of bamboo fiber, cellulase, nano-silica, silane coupling agent and ethanol is 30:300:2:6:100.

[0049] The seaweed extract was prepared by the following method: the seaweed was crushed and added to 8 times the weight of water, then ultrasonically extracted at 60°C for 1 hour, then an equal amount of mixed solvent was added for extraction for 24 hours, and rotary evaporated at 80°C for 6 hours to obtain the seaweed extract. In the mixed solvent, the volume ratio of methanol, chloroform and water was 4:3:1.

[0050] The bamboo leaf extract is prepared by the following method: the bamboo leaves are crushed and added into 50 times the mass of water, stirred evenly, and then microwaved for 4 hours under 1.5 kW conditions, and filtered; the filtered residue is then immersed in anhydrous ethanol, ultrasonically extracted at 60° C. for 1 hour, filtered, the two filtrates are combined, and dried to obtain the bamboo leaf extract.

[0051] The method for preparing the above-mentioned rubber material for automobiles comprises the following steps:

[0052] (1) mixing ethylene propylene diene monomer rubber, methyl vinyl phenyl silicone rubber, natural rubber, epoxidized natural rubber, seaweed extract, bamboo leaf extract, modified bentonite and carbon black at 80° C. for 1 h to obtain a mixture;

[0053] (2) adding an antioxidant, sulfur, lignin, pretreated plant fiber, nano zinc oxide and activated carbon to the mixture obtained in step (1), mixing at 90° C. for 0.5 h, and sequentially stretching, extruding and hot pressing to obtain a rubber material for automobiles.

[0054] Comparative Example 1

[0055] The difference between Comparative Example 1 and Example 2 is that Comparative Example 1 does not contain pretreated plant fibers.

[0056] Comparative Example 2

[0057] The difference between Comparative Example 2 and Example 2 is that Comparative Example 2 does not contain seaweed extract.

[0058] Comparative Example 3

[0059] The difference between Comparative Example 3 and Example 2 is that Comparative Example 3 does not contain bamboo leaf extract.

[0060] Comparative Example 4

[0061] The difference between Comparative Example 4 and Example 2 is that Comparative Example 2 does not contain epoxidized natural rubber.

[0062] The performance tests were performed on the rubber materials obtained in Examples 1-4 and Comparative Examples 1-4, and the results are shown in Table 1.

[0063] Table 1 Performance test results statistics

[0064]

[0065] As can be seen from Table 1, the rubber material for automobiles obtained by the present invention has good tensile strength, tear strength and other properties, good elasticity, and can be suitable for the application of automobile interior materials; it also has good sound absorption and shock absorption functions, is wear-resistant, and prolongs the service life of the rubber material, and has very excellent comprehensive performance.

[0066] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A rubber material for automobiles, characterized in that: The invention comprises the following raw materials in parts by weight: 60-70 parts of ethylene propylene diene rubber, 6-10 parts of methyl vinyl phenyl silicone rubber, 30-40 parts of natural rubber, 8-10 parts of epoxidized natural rubber, 2-4 parts of antioxidant, 2-4 parts of sulfur, 2-4 parts of lignin, 2-4 parts of pretreated plant fiber, 10-20 parts of seaweed extract, 5-10 parts of bamboo leaf extract, 1-2 parts of nano zinc oxide, 1-2 parts of activated carbon, 10-30 parts of modified bentonite and 1-3 parts of carbon black.

2. The rubber material for automobiles according to claim 1, wherein: The invention comprises the following raw materials in parts by weight: 65 parts of EPDM rubber, 8 parts of methyl vinyl phenyl silicone rubber, 36 parts of natural rubber, 9 parts of epoxidized natural rubber, 3 parts of antioxidant, 3 parts of sulfur, 3 parts of lignin, 3 parts of pretreated plant fiber, 15 parts of seaweed extract, 7 parts of bamboo leaf extract, 1 part of nano zinc oxide, 2 parts of activated carbon, 20 parts of modified bentonite and 2 parts of carbon black.

3. The rubber material for automobiles according to claim 1, wherein: The pretreated plant fiber is prepared by the following method: adding bamboo fiber to cellulose enzyme for 2-3 hours, then microwave treatment for 1-2 minutes under 2-3kW conditions, then adding nano-silicon dioxide and silane coupling agent to ethanol for vacuum impregnation for 1-2 hours, and drying to obtain the pretreated plant fiber.

4. The rubber material for automobiles according to claim 3, characterized in that: The mass ratio of the bamboo fiber, the cellulase, the nano-silicon dioxide, the silane coupling agent and the ethanol is 30:200-300:1-2:5-6:50-100.

5. The rubber material for automobiles according to claim 1, wherein: The seaweed extract is prepared by the following method: crushing the seaweed and adding it to 4-8 times the weight of water, then ultrasonically extracting it at 50-60° C. for 0.5-1 h, then adding an equal amount of mixed solvent to extract it for 24 h, and rotary evaporating it at 70-80° C. for 5-6 h to obtain the seaweed extract.

6. The rubber material for automobiles according to claim 5, characterized in that: In the mixed solvent, the volume ratio of methanol, chloroform and water is 4:3:

1.

7. The rubber material for automobiles according to claim 1, wherein: The bamboo leaf extract is prepared by the following method: crushing the bamboo leaves, adding them into 20-50 times the mass of water, stirring evenly, then subjecting them to microwave treatment for 2-4 hours at 0.5-1.5 kW, and filtering; then immersing the filtered residue in anhydrous ethanol, ultrasonically extracting for 0.5-1 hour at 50-60° C., filtering, combining the two filtrates, and drying to obtain the bamboo leaf extract.

8. The rubber material for automobiles according to claim 1, wherein: The epoxidized natural rubber has an epoxidation degree of 20-40.

9. The rubber material for automobiles according to claim 1, wherein: The antioxidant is a p-phenylenediamine antioxidant.

10. The method for preparing the automotive rubber material according to any one of claims 1 to 9, characterized in that: The following steps are involved: (1) mixing ethylene propylene diene monomer rubber, methyl vinyl phenyl silicone rubber, natural rubber, epoxidized natural rubber, seaweed extract, bamboo leaf extract, modified bentonite and carbon black at 50-80° C. for 0.5-1 h to obtain a mixture; (2) adding an anti-aging agent, sulfur, lignin, pretreated plant fiber, nano zinc oxide and activated carbon to the mixture obtained in step (1), mixing at 70-90° C. for 0.2-0.5 h, and sequentially stretching, extruding and hot pressing to obtain a rubber material for automobiles.

Citation Information

Cited By

  • Environment change self-adaptive high-performance vehicle rubber material

    CN119931165A

  • A high-performance automotive rubber material that adapts to environmental changes

    CN119931165B