Polystyrene composite insulation board and preparation method thereof

By adding multi-component foaming agent and reinforcement to the polystyrene composite insulation board, an efficient bubble cell and three-dimensional network structure is formed, which solves the problem of limited application of polystyrene insulation board in high-end fields, and improves compressive strength and The thermal insulation effect expands the use temperature range and reduces the thermal conductivity.

CN118994805AActive Publication Date: 2024-11-22SHANGHAI EARTHMOTHER ENERGY SAVING TECH
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411299834.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-18
Publication Date
2024-11-22
Estimated Expiration
2044-09-18

AI Technical Summary

Technical Problem

The existing polystyrene insulation boards are limited by the low operating temperature and side compressive strength in high-end fields such as wind power and rail transit, and it is difficult to expand their application areas.

Method used

Using polystyrene composite insulation board, the nucleation agent is optimized by adding multi-component low thermal conductivity foaming agents such as CO2, HFO-1233zd and R-152a, reinforcement materials such as polyamide 6 and straw/hypha composite materials, and the nucleation agent is optimized and The flame retardant ratio combines with a multi-stage extrusion process to form an efficient cell structure and a three-dimensional network structure, improving mechanical properties and thermal insulation effect.

Benefits of technology

The compressive strength, thermal deformation temperature and insulation effect of the polystyrene composite insulation board are significantly improved, the temperature range of its use, the thermal conductivity coefficient is reduced, and the flame retardant performance is enhanced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118994805A_ABST
    Figure CN118994805A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of insulation boards, and particularly discloses a polystyrene composite insulation board and a preparation method thereof. The polystyrene composite insulation board comprises the following raw materials: 75-90 wt% of polystyrene; 5-10 wt% of a reinforcing material; 0.5-3 wt% of a nucleating agent; 1-5 wt% of a flame retardant; 5-10 wt% of a foaming agent; the foaming agent is prepared from any one or more of alcohol, CO2 (carbon dioxide), R-152a, HFO-1233zd and HFO-1234ze. The preparation method comprises the following steps: S1, preparing raw materials; and S2, preparation of the insulation board. The composite insulation board can be used for wall insulation, and has the advantages of low heat conductivity, high strength, stable foam holes and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of thermal insulation boards, and more specifically, to a polystyrene composite thermal insulation board and a preparation method thereof. Background Art

[0002] Extruded polystyrene (XPS) foam is a foam material made from general-grade polystyrene using a continuous extrusion foaming method. Due to its excellent thermal insulation performance, moisture resistance, high compressive strength, chemical corrosion resistance, and easy processing, it is widely used in transportation, refrigeration, construction, interior decoration and other fields.

[0003] Existing XPS sheets are mostly used in the field of thermal insulation, such as cold storage insulation and indoor and outdoor wall insulation. However, in some high-end fields, such as wind power and rail transportation, its low operating temperature (0-75℃) and lateral compressive strength limit the expansion of its application areas. Summary of the invention

[0004] In order to improve the thermal insulation effect and compression resistance of the polystyrene thermal insulation board, the present application provides a polystyrene composite thermal insulation board and a preparation method thereof, which adopts the following technical scheme: In a first aspect, the present application provides a polystyrene composite insulation board, comprising raw materials in the following proportions: Polystyrene 75-90wt%; Reinforcement material 5-10wt%; Nucleating agent 0.5-3wt%; Flame retardant 1-5wt%; 5-10wt% of a foaming agent; the foaming agent comprises any one or more of alcohol, CO2, R-152a, HFO-1233zd and HFO-1234ze.

[0005] By adopting the above technical solution, the present application preferably adopts a multi-component low thermal conductivity foaming agent combination, which is beneficial for reducing the thermal conductivity of the composite insulation board while maintaining the strength.

[0006] R-152a, HFO-1233zd and HFO-1234ze are all foaming agents with low thermal conductivity, which can reduce foam density, increase foam compression strength, and make pore size distribution uniform, thereby improving the thermal insulation effect and mechanical strength of the insulation board.

[0007] Optionally, the blowing agent includes CO2, HFO-1233zd and R-152a in a mass ratio of 3.5:2.1:2.2.

[0008] By adopting the above technical scheme, it is preferred to use multi-component low thermal conductivity foaming agents with appropriate proportions to cooperate with each other, CO2 as the main foaming agent, 1233zd and 152 as auxiliary foaming agents, CO2 can alleviate the problem of high foam brittleness, effectively reduce the insulation coefficient of the composite insulation board, and enable the insulation board to obtain excellent insulation effect.

[0009] Optionally, the reinforcing material includes any one or more of polyamide 6, ABS, and PC.

[0010] By adopting the above technical solution and adding reinforcing materials, the melt strength of the PS matrix can be made higher, which is more conducive to forming a stable pore structure during the pore growth process in the composite insulation board, and enables the composite insulation board to obtain excellent compressive strength and heat deformation temperature.

[0011] Polyamide 6 can significantly enhance the compressive strength of XPS while maintaining the thermal conductivity coefficient unchanged, while improving the side compressive strength. And as the amount of PA6 increases, the compressive strength of the front and side also increases. The introduction of reinforcing materials can also increase the thermal deformation temperature of XPS and increase its use temperature range. Therefore, the introduction of reinforcing materials such as PA6 can significantly increase the mechanical properties of XPS.

[0012] Optionally, the flame retardant includes any one or more of methyl octabromoether, siloxane, and silicone rubber.

[0013] Optionally, the nucleating agent includes any one or more of talc, calcium carbonate, and carbon black.

[0014] Optionally, the reinforcing material further includes straw fibers, and the straw fibers are straw / mycelium composite materials.

[0015] By adopting the above technical solution, the mycelium has a large number of hyphae and hollow tubular structures, and the hyphae can be combined with straw fibers to form an ultra-dense linear network structure, forming a three-dimensional network structure, that is, the composite material has a large number of pore structures. After being added to the composite insulation board, it can effectively improve the pore structure in the insulation board and further reduce the thermal conductivity of the insulation board. In addition, the fiber structure can increase the nucleation sites in the insulation board, so that the insulation board has excellent foaming effect and pore stability.

[0016] Optionally, the straw / mycelium composite material is prepared as follows: the straw fibers are immersed in an alkaline solution, immersed, filtered, washed, and dried to obtain pretreated straw fibers, the pretreated straw fibers, bran, glucose, calcium carbonate, magnesium sulfate, mushroom-enhancing enzyme, and water are mixed to obtain a culture medium, mycelium balls are inoculated into the culture medium, cultured, compacted, demolded, and dried to obtain a straw / mycelium composite material.

[0017] By adopting the above technical solution, preferably using alkali solution to pretreat the straw fiber, the alkali solution can destroy the internal structure of the straw fiber, increase the specific surface area of ​​the straw fiber, provide a good growth interface for the hyphae, promote the growth of the hyphae, make the hyphae and the straw fiber closely combined, so that the composite material has excellent mechanical effect. And after alkali treatment, the hydrophobic protein content in the hyphae can be increased, thereby effectively improving the hydrophobic effect of the composite material.

[0018] Optionally, the straw / mycelium composite material is a straw / mycelium composite material that has been wrapped with oleic acid and magnesium hydroxide.

[0019] By adopting the above technical solution, the composite material is wrapped with oleic acid and magnesium hydroxide, and the oleic acid can combine with the hydroxyl group in the magnesium hydroxide, and then graft long-chain groups on the surface of the composite material, thereby improving the polarity and hydrophobic effect of the composite material, and improving the compatibility and bonding effect between the composite material and polystyrene. In addition, the wrapping of magnesium hydroxide can make the composite material obtain a rough surface and excellent flame retardant effect, which can improve the bonding strength between the composite material and polystyrene, and further improve the flame retardancy and mechanical strength of the composite insulation board.

[0020] In a second aspect, the present application provides a method for preparing a polystyrene composite insulation board, using the following technical solution: A method for preparing a polystyrene composite insulation board comprises the following steps: S1. Raw material preparation: Weigh polystyrene, reinforcing material, nucleating agent, flame retardant and foaming agent respectively by weight; S2. Preparation of thermal insulation board: polystyrene, reinforcing material, nucleating agent and flame retardant are added to the first-stage extruder, mixed, foaming agent is injected from the foaming agent injection port, mixed, extruded, conveyed to the second-stage extruder through the screen changer, stirred, mixed, molded, cut to obtain a composite thermal insulation board.

[0021] Optionally, the screen changer uses a replaceable screen changing system.

[0022] By adopting the above technical solution, due to the use of a replaceable screen changing system, the wire mesh can be replaced and large impurities on the wire mesh can be cleaned after the screen changer has been running for a period of time, thereby reducing the impact of screen changer blockage on the production efficiency of the composite insulation board.

[0023] Optionally, the second-stage extruder is a single-screw extruder.

[0024] By adopting the above technical solution, a single-screw extruder is preferably used as the second-stage extruder. The single-screw extruder can cool the homogeneous melt whose melt strength is greatly reduced after being plasticized by the foaming agent, so as to increase the melt strength and reach the viscosity range required for the molded product.

[0025] In summary, this application has the following beneficial effects: 1. This application uses a blended reinforcing material to reinforce the PS matrix, which is beneficial to improving the compressive strength and heat deformation temperature; 2. This application uses a multi-component low thermal conductivity foaming agent combination, which is beneficial to reduce the thermal conductivity while maintaining strength; 3. The PS matrix modified by blending used in this application has higher melt strength, which is more conducive to stabilizing the cell structure during cell growth; 4. The introduction of a multi-component foaming agent used in this application is beneficial to the nucleation and growth of the bubbles. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 It is a flow chart of the method provided by this application. DETAILED DESCRIPTION

[0027] The present application is further described in detail below with reference to the embodiments. Preparation Example

[0028] Composite material preparation example Preparation Example 1 Preparation of alkali solution: urea, sodium hydroxide and water are mixed to prepare an alkali solution with a urea concentration of 10wt% and a sodium hydroxide concentration of 6wt%.

[0029] The straw fiber is immersed in an alkali solution at 80° C. and a rotation speed of 150 rpm for 30 minutes, filtered, washed, and dried to obtain pretreated straw fiber.

[0030] Preparation of Pleurotus ostreatus culture medium: 20 g corn flour, 2 g peptone, 0.5 g MgSO4·7H2O, 1 g KH2PO4, 0.1 g NaCl and 200 g potato were mixed to prepare Pleurotus ostreatus culture medium.

[0031] Preparation of PDA: 200 g of potato, 20 g of glucose, 5 g of peptone, 2 g of agar, 1.5 g of MgSO4·7H2O and 3 g of KH2PO4 were mixed to prepare PDA.

[0032] Preparation of mycelium culture medium: 60 g straw fiber, 7.5 g bran, 2.8 g glucose, 0.75 g calcium carbonate, 0.1875 g MgSO4·7H2O, 0.2 g mushroom enzyme and distilled water were prepared to obtain mycelium culture medium (water content 70%).

[0033] Place the sterilized PDA in a clean bench, pour it into a plate for packaging, and sterilize it with UV for 15 minutes. Place the mother strain of Pleurotus ostreatus 1103 in a clean bench, punch it into a 0.9 cm diameter cake with a cake puncher, and inoculate it into the PDA plate with an inoculation hook. Place the subcultured Pleurotus ostreatus 1103 in a constant temperature incubator at 28°C and 60% relative humidity for 7 days. Take it out after the mycelium has grown all over the plate and store it in a 4°C refrigerator for later use.

[0034] The sterilized Pleurotus ostreatus culture medium and the subcultured Pleurotus ostreatus 1103 plate were placed in an ultra-clean workbench. The secondary strain was punched into a cake with a diameter of 0.9 cm using a cake puncher. Three cakes were picked out with an inoculation hook and inoculated into 100 mL of Pleurotus ostreatus liquid culture medium.

[0035] The inoculated Pleurotus ostreatus 1103 was placed in a shaking table at 28°C and 160r / min for 7 days to obtain mycelial balls, which were taken out and stored in a refrigerator at 4°C for later use. The mycelial balls of Pleurotus ostreatus 1103 were filtered, 20g of the mycelial balls were weighed from the sterilized mycelial material culture matrix, inoculated with 15% of the mycelial balls by mass, stirred evenly with a glass plate, and placed in a cylindrical glass mold. The mycelial material was placed in an incubator for dark culture, and was taken out and pressed to 5cm every 7 days. After the mycelial material was cultured in a constant temperature incubator for 16 days, it was taken out and demolded. The demolded material was placed in a 60°C oven for drying for 24 hours, and then crushed to obtain a straw / mycelium composite material.

[0036] Preparation Example 2 Add 2g of straw / mycelium composite material and 50mL of 0.5mol / L MgCl2·6H2O solution to the container, turn on the digital display stirrer after uniform dispersion, take 53mL of 1mol / L NaOH solution and add it dropwise to the container, adjust the pH value to about 9, move it into an 85℃ water bath after the addition is complete, and react for 1h. Then add 3.5mL of oleic acid (OA) and continue to react for 2h. After the reaction is completed, cool and filter, wash with water until neutral, wash with anhydrous ethanol, obtain filter cake, freeze-dry, and crush to obtain modified straw / mycelium composite material. Example

[0037] Examples 1-4 On the one hand, the present application provides a polystyrene composite insulation board, including polystyrene, a reinforcing material, a nucleating agent, a flame retardant and a foaming agent, and the specific qualities are shown in the table below.

[0038] Specifically, the polystyrene is general-grade polystyrene, the reinforcing material is PA6, the nucleating agent is talcum powder, the flame retardant is methyl octabromoether, and the foaming agent is carbon dioxide, HFO-1233zd and R-152a.

[0039]

[0040] On the other hand, the present application provides a method for preparing a polystyrene composite insulation board, comprising the following steps: S1. Raw material preparation: Weigh polystyrene, reinforcing material, nucleating agent, flame retardant and foaming agent respectively by weight; S2. Preparation of thermal insulation board: polystyrene, reinforcing material, nucleating agent and flame retardant are added to the first-stage extruder, mixed, foaming agent is injected from the foaming agent injection port, mixed, extruded, conveyed to the second-stage extruder through the screen changer, stirred, mixed, molded, cut to obtain a composite thermal insulation board.

[0041] Specifically, step S2, preparing the insulation board includes: S21, adding polystyrene, reinforcing material, nucleating agent and flame retardant into a first-stage extruder (twin-screw extruder), and setting the temperature of each zone of the twin-screw extruder to 200-230°C; Among them: the section from the feeding port to the foaming agent injection port is mainly a strong shearing section, which is used to fully mix the materials.

[0042] S22, the foaming agent is continuously and stably injected into the twin-screw extruder from the foaming agent injection port through the foaming agent metering pump, and mixed to obtain a mixed melt; Among them: the foaming agent should be injected in liquid state and should be pressurized before injection to prevent gas backflow. The injection position is where the polystyrene, reinforcement material, nucleating agent and flame retardant components are evenly mixed. The screw is designed with multiple protrusions at the injection point to prevent the formation of liquid pools and promote rapid and uniform dispersion of gas in the melt. The plasticization of the melt by the foaming agent leads to a decrease in melt strength. The barrel temperature here is set to 200-210℃.

[0043] S23, the mixed melt is filtered out of large impurities through a screen changer and transported to the second-stage extruder (single screw extruder) through a melt conveying pipeline. Among them: the single screw extruder can cool down the homogeneous melt whose melt strength has been greatly reduced after being plasticized by the foaming agent, so as to improve the melt strength and reach the viscosity range required for the molded product; The screen changer uses a replaceable screen changing system. After a period of operation, large impurities on the wire mesh are replaced and cleaned to reduce the impact on production efficiency. The melt delivery pipeline does not contain a screw, and its barrel temperature is set at 180-200°C; The single screw extruder adopts a step-by-step cooling mode from the front to the head to fully cool the melt. The temperature of each zone is set at 90-140°C. The speed of the single screw should not be too fast to prevent the screw shear heat from heating the melt. The melt cooling rate should be efficient and rapid. Static mixing or melt pump equipment is set in front of the single screw head to control and maintain the pressure of the melt to prevent the melt from being depressurized too early and causing pre-foaming. The static mixing temperature should be appropriately increased, generally set to 110-130°C, to prevent the melt from flowing in a dead zone where it stagnates.

[0044] S24, after cooling, the homogeneous melt passes through the die head and die lip, where the thermodynamic steady state is broken due to rapid pressure relief, and the foaming agent gas quickly escapes from the polymer, causing the melt volume to expand and form a closed cell structure. The XPS is then sized by the shaping template, the whole platform, the traction roller, etc. Among them: the design of the die runner must ensure that the melt flow rate at each part of the die lip is equivalent, because the pressure drop distribution in each area of ​​the mold is calculated under the premise of controlling the total pressure drop of the melt; the pulling roller speed is matched with the melt extrusion amount of the die mouth to ensure that the tensile force on the sheet in the lateral direction is consistent.

[0045] S25. After the XPS board is shaped and flattened, a small amount of edge material on both sides is cut off by a cutter, and after side coding and embossing on the front and back sides, it is sliced ​​by a transverse cutting machine and packaged for storage to obtain a composite insulation board.

[0046] Table 1 Example 1

[0047] Example 5 The difference from Example 4 is that the reinforcing material includes PA6 with a mass ratio of 7:3 and the straw / mycelium composite material prepared in Preparation Example 1.

[0048] Example 6 The difference from Example 3 is that the reinforcing material includes PA6 with a mass ratio of 7:3 and the straw / mycelium composite material prepared in Preparation Example 1. Comparative Example

[0049] Comparative Example 1 The difference between this comparative example and Example 4 is that no reinforcing material is added in this comparative example. Performance testing

[0050] (1) Apparent density test: The test shall be conducted in accordance with the test method of GB / T6343-1996 "Determination of apparent (bulk) density of cellular plastics and rubber".

[0051] (2) Thickness detection: Use a ruler to measure the thickness of the insulation board.

[0052] (3) Compression strength test: Test the 10% compression strength and side compression strength of the insulation board according to GB / T8813-1998 "Compression test method for rigid foam plastics".

[0053] (4) Thermal deformation test: Use a thermal deformation Vicat softening point tester to test the thermal deformation temperature of the insulation board.

[0054] (5) Thermal conductivity test: The thermal conductivity test equipment uses FOX200 produced by TA Instruments of the United States.

[0055] (6) Combustion performance test: The combustion performance level of the insulation board is tested according to GB / T 10801.2-2018 Extruded polystyrene foam for thermal insulation.

[0056] Table 2 Performance test

[0057] Combining the performance test comparison in Table 2, we can find that: 1. By comparing Examples 1-4 with Comparative Example 1, it can be found that the apparent density, compression strength, and heat deformation temperature of the insulation board prepared in Examples 1-4 are all improved, and the thermal conductivity is reduced. This shows that the introduction of PA6 in this application can significantly enhance the compression strength of XPS while maintaining the thermal conductivity unchanged, and at the same time improve the side compressive strength. And as the amount of PA6 feed increases, the compression strength of the front and side also increases. The introduction of reinforcing materials can also increase the heat deformation temperature of XPS and increase its use temperature range. Therefore, the introduction of reinforcing materials such as PA6 can significantly increase the mechanical properties of XPS.

[0058] 2. By comparing Examples 5-6 with Example 4, it can be found that the apparent density, compression strength, and heat deformation temperature of the insulation board prepared in Examples 1-4 are all improved, and the thermal conductivity is reduced. This shows that the mycelium in the present application has a large number of mycelium and hollow tubular structures, and the composite material has a three-dimensional network structure and a large number of pore structures. The hollow insulation structure and fiber structure can be introduced into the insulation board, effectively improving the insulation effect and mechanical strength of the insulation board. By wrapping the composite material with oleic acid and magnesium hydroxide, flame retardant groups and long-chain groups can be introduced on the surface of the composite material, thereby improving the polarity, hydrophobicity, and flame retardant effect of the composite material, and improving the compatibility and bonding effect between the composite material and polystyrene.

[0059] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. A polystyrene composite insulation board, characterized in that: The raw materials include the following proportions: Polystyrene 75-90wt%; Reinforcement material 5-10wt%; Nucleating agent 0.5-3wt%; Flame retardant 1-5wt%; 5-10wt% of a foaming agent; the foaming agent comprises CO2, HFO-1233zd and R-152a in a mass ratio of 3.5:2.1:2.2; The reinforcing material comprises straw fibers, and the straw fibers are straw / mycelium composite materials.

2. A polystyrene composite insulation board according to claim 1, characterized in that: The reinforcing material includes any one or more of polyamide 6, ABS, and PC.

3. The polystyrene composite insulation board according to claim 1, characterized in that: The flame retardant includes any one or more of methyl octabromoether, siloxane, and silicone rubber.

4. The polystyrene composite insulation board according to claim 1, characterized in that: The nucleating agent includes any one or more of talc, calcium carbonate and carbon black.

5. The polystyrene composite insulation board according to claim 1, characterized in that: The straw / mycelium composite material is prepared as follows: immersing straw fibers in alkaline solution, immersing, filtering, washing, and drying to obtain pretreated straw fibers; mixing the pretreated straw fibers, bran, glucose, calcium carbonate, magnesium sulfate, mushroom-enhancing enzymes, and water to obtain a culture medium; inoculating mycelium balls into the culture medium, culturing, compacting, demoulding, and drying to obtain the straw / mycelium composite material.

6. The polystyrene composite insulation board according to claim 1, characterized in that: The straw / mycelium composite material is a straw / mycelium composite material that has been wrapped with oleic acid and magnesium hydroxide.

7. The method for preparing a polystyrene composite thermal insulation board according to any one of claims 1 to 6, characterized in that: The following steps are involved: S1. Raw material preparation: Weigh polystyrene, reinforcing material, nucleating agent, flame retardant and foaming agent respectively by weight; S2. Preparation of thermal insulation board: polystyrene, reinforcing material, nucleating agent and flame retardant are added to the first-stage extruder, mixed, foaming agent is injected from the foaming agent injection port, mixed, extruded, conveyed to the second-stage extruder through the screen changer, stirred, mixed, molded, cut to obtain a composite thermal insulation board.

8. The method for preparing a polystyrene composite thermal insulation board according to claim 7, characterized in that: The screen changer uses a replaceable screen changing system.

9. The method for preparing a polystyrene composite thermal insulation board according to claim 7, characterized in that: The second-stage extruder is a single-screw extruder.

Citation Information

Patent Citations

  • Methods of manufacturing extruded polystyrene foams using carbon dioxide as major blowing agent

    CN106795310A

  • Wear resistant polystyrene expanded composite material resistant to cigarette burning and preparation method thereof

    CN110256720A

  • Initiated chemical vapor deposition apparatus for depositing high quality thin film through buffer chamber