Flame-retardant epoxy resin composition, flame-retardant epoxy resin cured product as well as preparation method and application of flame-retardant epoxy resin cured product

The flame retardant epoxy resin composition formed by using reactive phosphorus-containing and nitrogen-containing flame retardant in epoxy resins has solved the problem of reducing performance of traditional flame retardant, and achieved efficient flame retardant performance and Good compatibility, improving thermal and mechanical properties.

CN118994852AActive Publication Date: 2024-11-22CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202310555522.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-17
Publication Date
2024-11-22
Estimated Expiration
2043-05-17

AI Technical Summary

Technical Problem

While improving flame retardant epoxy resins often reduce their mechanical and thermal properties, traditional halogen or phosphorus-containing flame retardants are harmful to the environment and the human body, and have poor compatibility with the matrix.

Method used

The flame retardant epoxy resin composition formed by using a specific reactive phosphorus-containing and nitrogen-containing flame retardant as the component of the epoxy resin and participating in the curing reaction is preferably 5% to 25% of the organic nitrogen-containing flame retardant. and organic phosphorus-containing flame retardant 5% to 25% to improve flame retardant grade and performance.

Benefits of technology

While ensuring the flame retardant level of UL94V0, the thermal and mechanical properties of the flame retardant epoxy resin are greatly improved. This method is non-toxic or low-toxic and has good compatibility.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004232857390000031
    Figure BDA0004232857390000031
  • Figure BDA0004232857390000041
    Figure BDA0004232857390000041
  • Figure BDA0004232857390000071
    Figure BDA0004232857390000071
Patent Text Reader

Abstract

The invention discloses a flame-retardant epoxy resin composition, a flame-retardant epoxy resin cured product as well as a preparation method and application of the flame-retardant epoxy resin cured product. The flame-retardant epoxy resin composition provided by the invention comprises the following substances in parts by weight: 100 parts of epoxy resin; 10 to 100 parts by weight of an organic flame retardant; 0-10 parts by weight of an accelerant; 30-260 parts by weight of a curing agent; 0-50 parts by weight of an epoxy resin diluent; the organic flame retardant is selected from an organic nitrogen-containing flame retardant and an organic phosphorus-containing flame retardant. According to the invention, a specific reactive phosphorus-containing and nitrogen-containing flame retardant is adopted, so that the flame-retardant effect can be achieved, and meanwhile, the flame-retardant epoxy resin can be used as an epoxy resin matrix to participate in a curing reaction; compared with the flame-retardant epoxy resin prepared from the additive flame retardant, the flame-retardant epoxy resin prepared from the flame-retardant epoxy resin and the additive flame retardant has the advantages that the flame-retardant grade reaches UL94V0, and meanwhile, the thermal property and the mechanical property of a product are greatly improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of flame retardant resins, and more particularly to a flame retardant epoxy resin composition, a flame retardant epoxy resin cured product, and a preparation method and application thereof. Background Art

[0002] Epoxy resin (EP) is an important matrix resin in composite materials. It has good physical and chemical properties, especially good bonding strength, stable product size, high hardness, good toughness, tolerance to alkali and most solvents, and good dielectric properties. Therefore, it is widely used in transportation, aerospace, interior decoration, electronic appliances, etc. However, epoxy resin is a flammable material. When burning, it releases heat at a fast rate, spreads flames quickly, and is accompanied by the generation of toxic gases and smoke, which limits its application in composite interior parts. With the increasing requirements for flame retardant properties in daily applications, research on its flame retardant modification has received more and more attention.

[0003] Some flame retardant epoxy resin systems on the market are mainly divided into the following categories:

[0004] 1. Use halogen-containing epoxy resin or epoxy resin with halogen-containing flame retardant added. This type of flame retardant mainly plays a free radical quenching effect in the gas phase during the combustion of the matrix to achieve the purpose of flame retardant modification. However, the combustion of halogen-containing substances will produce acids and dioxins, which will cause great harm to the environment and human body. At present, with increasingly stringent environmental protection requirements, this type of flame-retardant epoxy resin is facing elimination;

[0005] 2. Use phosphorus-containing epoxy resin or epoxy resin with phosphorus-containing flame retardant added. Phosphorus-containing flame retardant mainly decomposes thermally during the combustion process of the matrix to form phosphorus-containing substances such as phosphates and polyphosphates with strong dehydration properties, which promotes the early dehydration and carbonization of the matrix material, forming a continuous and dense covering layer, reducing the release of combustible substances and limiting the transfer of heat and oxygen. At the same time, phosphorus-based flame retardants generate phosphorus-oxygen free radicals through thermal decomposition, quenching the active free radicals generated during the combustion of polymer materials, inhibiting the continuation of chain reactions, and reducing the combustion temperature;

[0006] 3. Epoxy resin with nitrogen-containing flame retardant added. Phosphorus-containing flame retardant mainly exerts flame retardant effect in gas phase. In the process of thermal decomposition, it absorbs a large amount of heat and releases non-combustible gas (such as carbon dioxide, nitrogen, ammonia, water vapor, etc.), thereby reducing the temperature of the material surface and the concentration of combustible gas, so as to achieve the flame retardant effect. However, most of the phosphorus / nitrogen-containing flame retardants are solid powder flame retardants, such as inorganic phosphates, aluminum hydroxide, melamine salts, etc., with particle sizes usually in the micron level, poor compatibility with epoxy resin, and easily cause insufficient thermomechanical and mechanical properties of the resin matrix. As an ideal flame retardant, it should have the characteristics of high flame retardant efficiency, low toxicity or even non-toxicity, good compatibility with the matrix, and good tolerance.

[0007] CN109096472A provides a novel PN-Si synergistic flame retardant epoxy resin curing agent, comprising adding an appropriate amount of the novel PN-Si synergistic flame retardant epoxy resin curing agent to epoxy resin and mixing evenly, and then forming, curing, and post-curing to obtain an epoxy resin system cured product. This novel curing agent can not only cure epoxy resin, but also be used for epoxy resin flame retardancy, and has good curing effect and compatibility.

[0008] CN106633673A provides a flame-retardant epoxy resin based on phosphaphenanthrene derivatives and inorganic flame retardants, by compounding different phosphaphenanthrene derivative flame retardants with different inorganic flame retardants, and melt blending with bisphenol A diglycidyl ether epoxy resin at a certain temperature, adding an organic solvent to obtain a flame-retardant epoxy resin, and then adding a curing agent to the epoxy resin to complete the curing reaction at a certain temperature. The method only needs to mix the flame retardant and the epoxy resin evenly by stirring, and does not require a chemical bonding reaction between the two, which is simple and easy; the epoxy resin modified with the flame retardant has excellent flame retardant properties, the limiting oxygen index can reach 36.9%, and the flame retardant level can reach UL94-V0.

[0009] However, adding flame retardants to epoxy resins in the prior art will still greatly reduce the mechanical and thermal properties of epoxy resins. Therefore, a method is needed to improve the flame retardancy of epoxy resins while maintaining or further improving the mechanical and thermal properties of epoxy resins. Summary of the invention

[0010] In order to solve the problems in the prior art, the present invention proposes a flame retardant epoxy resin composition, a flame retardant epoxy resin cured product, and a preparation method and application thereof. The present invention adopts a specific reactive phosphorus-containing and nitrogen-containing flame retardant, which not only has a flame retardant effect, but also can participate in the curing reaction as an epoxy resin matrix; the flame retardant epoxy resin prepared by the action of the two greatly improves the thermal and mechanical properties of the product while ensuring that the flame retardant grade reaches UL94V0 compared to the flame retardant epoxy resin prepared by the additive flame retardant.

[0011] Without solving the above technical problems, the present invention proposes the following technical solutions:

[0012] One of the objects of the present invention is to provide a flame retardant epoxy resin composition, which comprises the following substances in parts by weight:

[0013]

[0014] The organic flame retardant is selected from organic nitrogen-containing flame retardants and organic phosphorus-containing flame retardants.

[0015] In the flame retardant epoxy resin composition of the present invention, preferably,

[0016] Based on the total weight of epoxy resin and organic flame retardant as 100%,

[0017] The mass proportion of the organic nitrogen-containing flame retardant is 5% to 25%, preferably 5% to 22.5%;

[0018] The mass proportion of the organic phosphorus-containing flame retardant is 5% to 25%, preferably 5% to 22.5%;

[0019] More preferably, based on the total weight of the epoxy resin and the organic flame retardant being 100%, the mass proportion of the organic flame retardant is 25% to 45%.

[0020] In the flame retardant epoxy resin composition of the present invention, preferably,

[0021] 0 to 6 parts by weight of accelerator; and / or,

[0022] 40 to 240 parts by weight of a curing agent; and / or,

[0023] 0 to 40 parts by weight of epoxy resin diluent;

[0024] The organic nitrogen-containing flame retardant is 6-40 parts by weight; for example, 6, 7, 8, 9, 10, 15, 20, 25, 30, 35, 40 parts by weight and any range consisting of any two of the above values;

[0025] The mass of the organic phosphorus-containing flame retardant is 6-40 parts by weight; for example, 6, 7, 8, 9, 10, 15, 20, 25, 30, 35, 40 parts by weight and any range consisting of any two of the above values.

[0026] In the flame retardant epoxy resin composition of the present invention, preferably,

[0027] The epoxy resin is selected from at least one of glycidyl ether epoxy resin, glycidyl ester epoxy resin, and glycidyl amine epoxy resin;

[0028] Preferably,

[0029] The glycidyl ether epoxy resin is selected from at least one of bisphenol A epoxy resin, bisphenol F epoxy resin and novolac epoxy resin; and / or,

[0030] The glycidyl ester epoxy resin is selected from at least one of 4,5-epoxycyclohexane-1,2-dicarboxylic acid diglycidyl ester and methacrylate-2,3-epoxypropyl ester;

[0031] More preferably,

[0032] The epoxy value of the epoxy resin is 0.10 to 1.00 mol / 100g.

[0033] In the flame retardant epoxy resin composition of the present invention, preferably,

[0034] The organic nitrogen-containing flame retardant is selected from triglycidyl isocyanurate; and / or,

[0035] The organic phosphorus-containing flame retardant is selected from triglycidyl phosphate.

[0036]

[0037] The organic flame retardant in the present invention can participate in the curing reaction as an epoxy matrix, greatly improving the flame retardant effect, mechanical and thermal properties; while the general nitrogen-containing and phosphorus-containing flame retardants only play a flame retardant role in the system.

[0038] In the flame retardant epoxy resin composition of the present invention, preferably,

[0039] The accelerator is selected from at least one of quaternary ammonium salts, quaternary phosphonium salts, imidazoles and their derivatives;

[0040] Preferably,

[0041] The quaternary ammonium salt is selected from at least one of benzyltriethylammonium bromide and tetraethylammonium bromide; and / or,

[0042] The quaternary phosphonium salt is selected from at least one of methyl triphenyl phosphonium bromide, ethyl triphenyl phosphonium bromide and butyl triphenyl phosphonium bromide; and / or,

[0043] The imidazole derivative is selected from at least one of dimethylimidazole and diethyltetramethylimidazole.

[0044] In the flame retardant epoxy resin composition of the present invention, preferably,

[0045] The curing agent is selected from at least one of anhydride curing agents and amine curing agents;

[0046] Preferably,

[0047] The acid anhydride curing agent is selected from at least one of methyltetrahydrophthalic anhydride, tetrahydrophthalic anhydride, hexahydrophthalic anhydride, methylhexahydrophthalic anhydride, methylnadic anhydride and maleic anhydride; and / or,

[0048] The amine curing agent is selected from at least one of dicyandiamide, isophoronediamine, triethylenetetramine, polyetheramine, and 3,3′-dimethyl-4,4′-diamino-dicyclohexylmethane.

[0049] In the flame retardant epoxy resin composition of the present invention, preferably,

[0050] The epoxy resin diluent is selected from at least one of glycidyl ether diluents; preferably at least one of ethylene glycol diglycidyl ether, butanediol diglycidyl ether, neopentyl glycol diglycidyl ether, hexanediol diglycidyl ether, trimethylolpropane triglycidyl ether, glycerol triglycidyl ether, and pentaerythritol tetraglycidyl ether.

[0051] A second object of the present invention is to provide a method for preparing the flame retardant epoxy resin composition as described in any one of the first objects of the present invention, comprising the following steps:

[0052] The epoxy resin, the organic flame retardant, the optional accelerator, the curing agent, and the optional epoxy resin diluent are uniformly mixed to prepare a flame retardant epoxy resin composition.

[0053] In the method for preparing the flame retardant epoxy resin composition of the present invention, preferably, the following steps are included:

[0054] (1) heating and melting an epoxy resin and optionally an epoxy resin diluent to obtain a melt;

[0055] (2) adding an organic nitrogen-containing flame retardant to the melt of step (1) and mixing them uniformly to obtain a mixture;

[0056] (3) After heating the curing agent, optionally add an accelerator and mix well;

[0057] (4) The mixture obtained in step (2), the substance obtained in step (3) and the organic phosphorus-containing flame retardant are uniformly mixed to obtain a flame-retardant epoxy resin composition.

[0058] Steps (2) and (3) in the present invention merely represent corresponding steps without any specific order requirement.

[0059] In the method for preparing the flame retardant epoxy resin composition of the present invention, preferably, in step (1), heating to 90-150° C. to melt, preferably keeping the temperature for 15-30 minutes after melting; and / or,

[0060] Step (2), the temperature during the mixing is 90-150°C; preferably, mechanical stirring is used for the mixing, and more preferably, the mixing time is 30-60 minutes; and / or,

[0061] Step (3), the temperature during the mixing is 90-150°C; preferably, mechanical stirring is used for the mixing, and more preferably, the mixing time is 30-60 minutes; and / or,

[0062] In step (4), the temperature during uniform mixing is 20-60° C.; preferably, mechanical stirring is used for uniform mixing, and more preferably, the mixing time is 2-5 min.

[0063] The third object of the present invention is to provide a flame retardant epoxy resin cured product prepared by curing a flame retardant epoxy resin composition comprising any one of the objects of the present invention or a flame retardant epoxy resin composition prepared by the method described in any one of the second objects of the present invention. Preferably, the flame retardant grade of the flame retardant epoxy resin cured product is UL94-V0 or above.

[0064] The fourth object of the present invention is to provide a flame retardant epoxy resin composition as described in any one of the first objects of the present invention, or a flame retardant epoxy resin composition prepared by the method described in any one of the second objects of the present invention, or a flame retardant epoxy resin cured product as described in the third object of the present invention for use in flame retardancy.

[0065] The triglycidyl phosphate of the present invention can be directly purchased or prepared according to an existing method. Preferably, the preparation method of triglycidyl phosphate comprises the following steps: The synthesis route of triglycidyl phosphate (TGP) is as follows:

[0066]

[0067] The method for preparing triglycidyl phosphate (TGP) comprises the following steps:

[0068] (1) Glycidol, phosphorus oxychloride and toluene are placed in a reactor, and an acid-binding agent, triethylamine, is added dropwise at 0 to 4°C;

[0069] (2) After reacting for 16 to 20 hours, the reaction solution is filtered to remove triethylamine hydrochloride;

[0070] (3) The filtrate is passed through a rotary evaporator to remove the solvent and unreacted products, thereby obtaining the product triglycidyl phosphate.

[0071] In some preferred embodiments of the present invention, the molar ratio of glycidol, phosphorus oxychloride and triethylamine is (3.4-4.2): (3.8-4.2): 1

[0072] The endpoints and any values ​​of the scope disclosed in the present invention are not limited to the precise scope or value, and these scopes or values ​​should be understood to include values ​​close to these scopes or values. For numerical ranges, the endpoint values ​​of each scope, the endpoint values ​​of each scope and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be regarded as specifically disclosed in this article. Hereinafter, in principle, each technical solution can be combined with each other to obtain a new technical solution, which should also be regarded as specifically disclosed in this article.

[0073] Compared with the prior art, the present invention has at least the following advantages:

[0074] The present invention adopts a specific reactive phosphorus-containing and nitrogen-containing flame retardant, which not only has a flame retardant effect, but also can act as an epoxy resin matrix to participate in the curing reaction; the flame retardant epoxy resin prepared by the action of the two greatly improves the thermal and mechanical properties of the product while ensuring that the flame retardant grade reaches UL94V0 compared to the flame retardant epoxy resin prepared by the additive flame retardant. DETAILED DESCRIPTION

[0075] The present invention is described in detail below in conjunction with specific embodiments. It is necessary to point out that the following embodiments are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made to the present invention by those skilled in the art based on the contents of the present invention still fall within the scope of protection of the present invention.

[0076] It should also be noted that the various specific technical features described in the following specific embodiments can be combined in any suitable manner without contradiction. To avoid unnecessary repetition, the present invention will not further describe various possible combinations.

[0077] In addition, the various embodiments of the present invention may be arbitrarily combined as long as they do not violate the concept of the present invention. The technical solutions thus formed belong to part of the original disclosure of this specification and also fall within the protection scope of the present invention.

[0078] The raw materials used in the examples and comparative examples, unless otherwise specified, are disclosed in the prior art, for example, they can be directly purchased or prepared according to the preparation methods disclosed in the prior art.

[0079] Test method:

[0080] 1. Tensile strength

[0081] The tensile strength of the cured resin was tested on a universal testing machine of Instron Company of the United States according to the ASTM D638 standard, with a tensile rate of 5 mm / min. The results are shown in Table 1;

[0082] 2. Thermodynamic properties

[0083] The glass transition temperature of the cured resin was measured on a Q800 dynamic mechanical properties analyzer from TA, USA. The test was conducted in single cantilever mode, air environment, heating rate of 3°C / min, temperature measurement range of RT to 250°C, and the peak temperature of tano' was selected as the T g , the results are shown in Table 1.

[0084] 3. Flame retardant effect test

[0085] The flame retardant grade of the flame retardant resin samples was tested according to UL94 standard, and the results are shown in Table 1.

[0086] [Example 1]

[0087] A flame retardant epoxy resin composition, comprising the following components in parts by mass:

[0088]

[0089] The preparation method of the flame retardant epoxy resin composition is:

[0090] (1) Heat 60 g of bisphenol A epoxy resin to 100°C and keep it warm for 15 minutes;

[0091] (2) Add 20 g of triglycidyl isocyanurate, stir mechanically for 60 min, then cool and set aside;

[0092] (3) 120 g of methyltetrahydrophthalic anhydride was heated to 100° C., 3 g of ethyltriphenylphosphonium bromide was added, and the mixture was mechanically stirred for 60 min and then cooled for later use;

[0093] (4) The products obtained in (2) and (3) and 20 g of triglycidylphosphoglycerate were mixed at 20°C for 3 min. The resulting composition was set aside for use.

[0094] [Example 2]

[0095] A flame retardant epoxy resin composition, comprising the following components in parts by mass:

[0096]

[0097] The preparation method of the flame retardant epoxy resin composition is:

[0098] (1) Heat 60 g of bisphenol A epoxy resin to 100°C and keep it warm for 15 minutes;

[0099] (2) Add 20 g of triglycidyl isocyanurate, stir mechanically for 60 min, then cool and set aside;

[0100] (3) 130 g of methyl nadic anhydride was heated to 110° C., 3 g of ethyl triphenylphosphonium bromide was added, and the mixture was mechanically stirred for 60 min and then cooled for later use;

[0101] (4) The products obtained in (2) and (3) and 20 g of triglycidylphosphoglycerate were mixed at 20°C for 4 minutes, and the obtained composition was set aside for use.

[0102] [Example 3]

[0103] A flame retardant epoxy resin composition, comprising the following components in parts by mass:

[0104]

[0105] The preparation method of the flame retardant epoxy resin composition is:

[0106] (1) Heat 50 g of bisphenol A epoxy resin and 10 g of ethylene glycol diglycidyl ether to 100°C and keep warm for 15 min;

[0107] (2) Add 20 g of triglycidyl isocyanurate, stir mechanically for 60 min, then cool and set aside;

[0108] (3) 120 g of methyltetrahydrophthalic anhydride was heated to 100° C., 3 g of ethyltriphenylphosphonium bromide was added, and the mixture was mechanically stirred for 60 min and then cooled for later use;

[0109] (4) The products obtained in (2) and (3) and 20 g of triglycidylphosphoglycerate were mixed at 20°C for 3 min. The resulting composition was set aside for use.

[0110] [Example 4]

[0111] A flame retardant epoxy resin composition, comprising the following components in parts by mass:

[0112]

[0113]

[0114] The preparation method of the flame retardant epoxy resin composition is:

[0115] (1) Heat 75 g of bisphenol A epoxy resin to 100°C and keep it warm for 15 minutes;

[0116] (2) Add 5 g of triglycidyl isocyanurate, stir mechanically for 30 min, then cool and set aside;

[0117] (3) 120 g of methyltetrahydrophthalic anhydride was heated to 100° C., 3 g of ethyltriphenylphosphonium bromide was added, and the mixture was mechanically stirred for 60 min and then cooled for later use;

[0118] (4) The products obtained in (2) and (3) and 20 g of triglycidylphosphoglycerate were mixed at 25°C for 3 minutes, and the obtained composition was set aside for use.

[0119] [Example 5]

[0120] A flame retardant epoxy resin composition, comprising the following components in parts by mass:

[0121]

[0122] The preparation method of the flame retardant epoxy resin composition is:

[0123] (1) Heat 75 g of bisphenol A epoxy resin to 100°C and keep it warm for 15 minutes;

[0124] (2) Add 20 g of triglycidyl isocyanurate, stir mechanically for 30 min, then cool and set aside;

[0125] (3) 120 g of methyltetrahydrophthalic anhydride was heated to 100° C., 3 g of ethyltriphenylphosphonium bromide was added, and the mixture was mechanically stirred for 60 min and then cooled for later use;

[0126] (4) The products obtained in (2) and (3) and 5 g of triglycidylphosphoglycerate were mixed at 25°C for 3 min. The resulting composition was set aside for use.

[0127] [Example 6]

[0128] A flame retardant epoxy resin composition, comprising the following components in parts by mass:

[0129]

[0130] The preparation method of the flame retardant epoxy resin composition is:

[0131] (1) Heat 60 g of phenolic epoxy resin to 120°C and keep warm for 20 minutes;

[0132] (2) Add 20 g of triglycidyl isocyanurate, stir mechanically for 30 min, then cool and set aside;

[0133] (3) 120 g of methyltetrahydrophthalic anhydride was heated to 100° C., 3 g of ethyltriphenylphosphonium bromide was added, and the mixture was mechanically stirred for 60 min and then cooled for later use;

[0134] (4) The products obtained in (2) and (3) and 20 g of triglycidylphosphoglycerate were mixed at 30°C for 3 minutes, and the obtained composition was set aside for use.

[0135] [Example 7]

[0136] A flame retardant epoxy resin composition, comprising the following components in parts by mass:

[0137]

[0138] The preparation method of the flame retardant epoxy resin composition is:

[0139] (1) Heat 60 g of bisphenol F epoxy resin to 110°C and keep warm for 20 minutes;

[0140] (2) Add 20 g of triglycidyl isocyanurate, stir mechanically for 30 min, then cool and set aside;

[0141] (3) 120 g of methyltetrahydrophthalic anhydride was heated to 100° C., 3 g of ethyltriphenylphosphonium bromide was added, and the mixture was mechanically stirred for 60 min and then cooled for later use;

[0142] (4) The products obtained in (2) and (3) and 20 g of triglycidylphosphoglycerate were mixed at 25°C for 3 minutes, and the obtained composition was set aside for use.

[0143] [Example 8]

[0144] A flame retardant epoxy resin composition, comprising the following components in parts by mass:

[0145]

[0146] The preparation method of the flame retardant epoxy resin composition is:

[0147] (1) Heat 50 g of bisphenol A epoxy resin and 10 g of ethylene glycol diglycidyl ether to 100°C and keep warm for 15 min;

[0148] (2) Add 20 g of triglycidyl isocyanurate, stir mechanically for 30 min, then cool and set aside;

[0149] (3) The product obtained in (2), 30 g of isophoronediamine and 20 g of triglycidylphosphoglycerate were mixed at 20° C. for 2 min, and the obtained composition was set aside for use.

[0150] [Example 9]

[0151] A flame retardant epoxy resin composition, comprising the following components in parts by mass:

[0152]

[0153] The preparation method of the flame retardant epoxy resin composition is:

[0154] (1) Heat 50 g of bisphenol A epoxy resin and 20 g of ethylene glycol diglycidyl ether to 100° C. and keep warm for 15 min;

[0155] (2) Add 15 g of triglycidyl isocyanurate, stir mechanically for 30 min, then cool and set aside;

[0156] (3) The product obtained in (2), 20 g of triethylenetetramine and 15 g of triglycidyl phosphate were mixed at 20° C. for 2 min. The obtained composition was ready for use.

[0157] [Example 10]

[0158] A flame retardant epoxy resin composition, comprising the following components in parts by mass:

[0159]

[0160] The preparation method of the flame retardant epoxy resin composition is:

[0161] (1) Heat 75g of TDE-85 epoxy resin to 100°C and keep it warm for 15 minutes;

[0162] (2) Add 5 g of triglycidyl isocyanurate, stir mechanically for 30 min, then cool and set aside;

[0163] (3) 120 g of methyltetrahydrophthalic anhydride was heated to 100° C., 3 g of ethyltriphenylphosphonium bromide was added, and the mixture was mechanically stirred for 60 min and then cooled for later use;

[0164] (4) The products obtained in (2) and (3) and 20 g of triglycidylphosphoglycerate were mixed at 25°C for 3 minutes, and the obtained composition was set aside for use.

[0165] [Example 11]

[0166] A flame retardant epoxy resin composition, comprising the following components in parts by mass:

[0167]

[0168]

[0169] The preparation method of the flame retardant epoxy resin composition is:

[0170] (1) Heat 75 g of bisphenol A epoxy resin to 100°C and keep it warm for 15 minutes;

[0171] (2) Add 5 g of triglycidyl isocyanurate, stir mechanically for 30 min, then cool and set aside;

[0172] (3) Heat 120 g of maleic anhydride to 100° C., add 3 g of ethyltriphenylphosphonium bromide, stir mechanically for 60 min, then cool and set aside;

[0173] (4) The products obtained in (2) and (3) and 20 g of triglycidylphosphoglycerate were mixed at 55°C for 4 minutes, and the obtained composition was ready for use.

[0174] [Example 12]

[0175] A flame retardant epoxy resin composition, comprising the following components in parts by mass:

[0176]

[0177] The preparation method of the flame retardant epoxy resin composition is:

[0178] (1) Heat 75 g of bisphenol A epoxy resin to 100°C and keep it warm for 15 minutes;

[0179] (2) Add 5 g of triglycidyl isocyanurate, stir mechanically for 30 min, then cool and set aside;

[0180] (3) Heat 120 g of methyltetrahydrophthalic anhydride to 100° C., add 3 g of imidazole, stir mechanically for 60 min, then cool and set aside;

[0181] (4) The products obtained in (2) and (3) and 20 g of triglycidylphosphoglycerate were mixed at 25°C for 3 minutes, and the obtained composition was set aside for use.

[0182] [Example 13]

[0183] A flame retardant epoxy resin composition, comprising the following components in parts by mass:

[0184]

[0185] The preparation method of the flame retardant epoxy resin composition is:

[0186] (1) Heat 55 g of bisphenol A epoxy resin and 20 g of propylene glycol triglycidyl ether to 100° C. and keep warm for 15 min;

[0187] (2) Add 5 g of triglycidyl isocyanurate, stir mechanically for 30 min, then cool and set aside;

[0188] (3) 120 g of methyltetrahydrophthalic anhydride was heated to 100° C., 3 g of ethyltriphenylphosphonium bromide was added, and the mixture was mechanically stirred for 60 min and then cooled for later use;

[0189] (4) The products obtained in (2) and (3) and 20 g of triglycidylphosphoglycerate were mixed at 25°C for 3 minutes, and the obtained composition was set aside for use.

[0190] [Example 14]

[0191]

[0192] The preparation method of the flame retardant epoxy resin composition is:

[0193] (1) Heat 80 g of bisphenol A epoxy resin to 100°C and keep it warm for 15 minutes;

[0194] (2) Add 10 g of triglycidyl isocyanurate, stir mechanically for 30 min, then cool and set aside;

[0195] (3) 120 g of methyltetrahydrophthalic anhydride was heated to 100° C., 3 g of ethyltriphenylphosphonium bromide was added, and the mixture was mechanically stirred for 60 min and then cooled for later use;

[0196] (4) The products obtained in (2) and (3) and 10 g of triglycidylphosphoglycerate were mixed at 25°C for 3 minutes, and the resulting composition was set aside for use.

[0197] [Comparative Example 1]

[0198] A flame retardant epoxy resin composition, comprising the following components in parts by mass:

[0199] Bisphenol A epoxy resin (CYD128, Baling Petrochemical) 100 copies

[0200] 3 parts of ethyltriphenylphosphonium bromide

[0201] 120 parts of methyltetrahydrophthalic anhydride

[0202] The preparation method of the flame retardant epoxy resin composition is:

[0203] (1) Heat 120 g of methyltetrahydrophthalic anhydride to 100° C., add 3 g of ethyltriphenylphosphonium bromide, stir mechanically for 60 min, then cool and set aside;

[0204] (2) The product obtained in (1) and 100 g of bisphenol A epoxy resin were mixed at 25° C. for 3 min, and the obtained composition was set aside for use.

[0205] [Comparative Example 2]

[0206] A flame retardant epoxy resin composition, comprising the following components in parts by mass:

[0207]

[0208] The preparation method of the flame retardant epoxy resin composition is:

[0209] (1) Heat 80 g of bisphenol A epoxy resin to 100°C and keep it warm for 15 minutes;

[0210] (2) Add 20 g of triglycidyl isocyanurate, stir mechanically for 60 min, then cool and set aside;

[0211] (3) 120 g of methyltetrahydrophthalic anhydride was heated to 100° C., 3 g of ethyltriphenylphosphonium bromide was added, and the mixture was mechanically stirred for 60 min and then cooled for later use;

[0212] (4) The products obtained in (2) and (3) were mixed at 25°C for 4 minutes, and the obtained composition was set aside for use.

[0213] Embodiment 13

[0214] [Comparative Example 3]

[0215] A flame retardant epoxy resin composition, comprising the following components in parts by mass:

[0216]

[0217] The preparation method of the flame retardant epoxy resin composition is:

[0218] (1) Heat 120 g of methyltetrahydrophthalic anhydride to 100° C., add 3 g of ethyltriphenylphosphonium bromide, stir mechanically for 60 min, then cool and set aside;

[0219] (2) The product of (1), 80 g of bisphenol A epoxy resin and 20 g of triglycidyl phosphate were mixed at 25° C. for 3 min. The resulting composition was set aside for use.

[0220] The 20 parts of TGIC added in Comparative Example 2 or the triglycidyl phosphate added in Comparative Example 3 serve as both a flame retardant and a base resin. Therefore, in Comparative Examples 2 and 3, the total amount of the base resin is actually 100 parts.

[0221] [Comparative Example 4]

[0222] A flame retardant epoxy resin composition, comprising the following components in parts by mass:

[0223]

[0224] Among them, the N and P elements in melamine phosphate have a synergistic flame retardant effect.

[0225] The preparation method of the flame retardant epoxy resin composition is:

[0226] (1) Heat 120 g of methyltetrahydrophthalic anhydride to 100° C., add 3 g of ethyltriphenylphosphonium bromide, stir mechanically for 60 min, then cool and set aside;

[0227] (2) The product of (1), 100 g of bisphenol A epoxy resin and 20 g of melamine phosphate were mixed at 25° C. for 3 min. The resulting composition was set aside for use.

[0228] After curing, the flame retardant epoxy resin compositions prepared in the examples of the present invention and the comparative examples have properties as shown in Table 1.

[0229] Table 1

[0230]

[0231] By comparing the results of Comparative Example 1 and Comparative Example 4, it can be seen that the flame retardant epoxy resin prepared by the existing common flame retardant has greatly reduced thermal and mechanical properties compared to the unmodified epoxy resin. By comparing the results of Comparative Example 1, Comparative Example 2, Comparative Example 3 with Example 14, it can be seen that the present invention uses a specific reactive phosphorus-containing and nitrogen-containing flame retardant, which not only has a flame retardant effect, but also can participate in the curing reaction as an epoxy resin matrix; the flame retardant epoxy resin prepared by the synergistic effect of the two greatly improves the thermal and mechanical properties of the product compared to the flame retardant epoxy resin prepared by the additive flame retardant while ensuring that the flame retardant grade reaches UL94V0.

[0232] The present invention has been described in detail above in conjunction with specific implementations and exemplary examples, but these descriptions cannot be understood as limiting the present invention. Those skilled in the art understand that, without departing from the spirit and scope of the present invention, a variety of equivalent substitutions, modifications or improvements may be made to the technical solution of the present invention and its implementation methods, all of which fall within the scope of the present invention. The scope of protection of the present invention shall be subject to the attached claims.

[0233] All publications, patent applications, patents and other references mentioned in this specification are incorporated herein by reference. Unless otherwise defined, all technical and scientific terms used in this specification have the meanings conventionally understood by those skilled in the art. In the event of a conflict, the definition in this specification shall prevail.

[0234] When this specification uses the prefix "well-known to those skilled in the art", "prior art" or similar terms to introduce materials, substances, methods, steps, devices or components, etc., the objects introduced by the prefix cover those commonly used in the art when this application is filed, but also include those that are not commonly used at present but will become recognized in the art as being suitable for similar purposes.

[0235] In the context of the present specification, any matters or items not mentioned are directly applicable to those known in the art without any changes except those explicitly stated.

Claims

1. A flame retardant epoxy resin composition, comprising the following substances in parts by weight: The organic flame retardant is selected from organic nitrogen-containing flame retardants and organic phosphorus-containing flame retardants.

2. The flame retardant epoxy resin composition according to claim 1, characterized in that: Based on the total weight of epoxy resin and organic flame retardant as 100%, The mass proportion of the organic nitrogen-containing flame retardant is 5% to 25%, preferably 5% to 22.5%; The mass proportion of the organic phosphorus-containing flame retardant is 5% to 25%, preferably 5% to 22.5%; More preferably, based on the total weight of the epoxy resin and the organic flame retardant being 100%, the mass proportion of the organic flame retardant is 25% to 45%.

3. The flame retardant epoxy resin composition according to claim 1, characterized in that: 0 to 6 parts by weight of accelerator; and / or, 40 to 240 parts by weight of a curing agent; and / or, Epoxy resin diluent 0 to 40 parts by weight.

4. The flame retardant epoxy resin composition according to claim 1, characterized in that: The epoxy resin is selected from at least one of glycidyl ether epoxy resin, glycidyl ester epoxy resin, and glycidyl amine epoxy resin; Preferably, The glycidyl ether epoxy resin is selected from at least one of bisphenol A epoxy resin, bisphenol F epoxy resin and novolac epoxy resin; and / or, The glycidyl ester epoxy resin is selected from at least one of 4,5-epoxycyclohexane-1,2-dicarboxylic acid diglycidyl ester and methacrylate-2,3-epoxypropyl ester; More preferably, The epoxy value of the epoxy resin is 0.10 to 1.00 mol / 100g.

5. The flame retardant epoxy resin composition according to claim 1, characterized in that: The organic nitrogen-containing flame retardant is selected from triglycidyl isocyanurate; and / or, The organic phosphorus-containing flame retardant is selected from triglycidyl phosphate.

6. The flame retardant epoxy resin composition according to claim 1, characterized in that: The accelerator is selected from at least one of quaternary ammonium salts, quaternary phosphonium salts, imidazoles and their derivatives; Preferably, The quaternary ammonium salt is selected from at least one of benzyltriethylammonium bromide and tetraethylammonium bromide; and / or, The quaternary phosphonium salt is selected from at least one of methyl triphenyl phosphonium bromide, ethyl triphenyl phosphonium bromide and butyl triphenyl phosphonium bromide; and / or, The imidazole derivative is selected from at least one of dimethylimidazole and diethyltetramethylimidazole.

7. The flame retardant epoxy resin composition according to claim 1, characterized in that: The curing agent is selected from at least one of anhydride curing agents and amine curing agents; Preferably, The acid anhydride curing agent is selected from at least one of methyltetrahydrophthalic anhydride, tetrahydrophthalic anhydride, hexahydrophthalic anhydride, methylhexahydrophthalic anhydride, methylnadic anhydride and maleic anhydride; and / or, The amine curing agent is selected from at least one of dicyandiamide, isophoronediamine, triethylenetetramine, polyetheramine, and 3,3′-dimethyl-4,4′-diamino-dicyclohexylmethane.

8. The flame retardant epoxy resin composition according to claim 1, characterized in that: The epoxy resin diluent is selected from at least one of glycidyl ether diluents; preferably at least one of ethylene glycol diglycidyl ether, butanediol diglycidyl ether, neopentyl glycol diglycidyl ether, hexanediol diglycidyl ether, trimethylolpropane triglycidyl ether, glycerol triglycidyl ether, and pentaerythritol tetraglycidyl ether.

9. A method for preparing the flame retardant epoxy resin composition according to any one of claims 1 to 8, comprising the following steps: The epoxy resin, the organic flame retardant, the optional accelerator, the curing agent, and the optional epoxy resin diluent are uniformly mixed to prepare a flame retardant epoxy resin composition.

10. The method for preparing the flame retardant epoxy resin composition according to claim 9, characterized in that: The following steps are involved: (1) heating and melting an epoxy resin and optionally an epoxy resin diluent to obtain a melt; (2) adding an organic nitrogen-containing flame retardant to the melt of step (1) and mixing them uniformly to obtain a mixture; (3) After heating the curing agent, optionally add an accelerator and mix well; (4) The mixture obtained in step (2), the substance obtained in step (3) and the organic phosphorus-containing flame retardant are uniformly mixed to obtain a flame-retardant epoxy resin composition.

11. The method for preparing the flame retardant epoxy resin composition according to claim 10, characterized in that: Step (1), heating to 90-150°C to melt, preferably keeping warm for 15-30 minutes after melting; and / or, Step (2), the temperature during the mixing is 90-150°C; preferably, mechanical stirring is used for the mixing, and more preferably, the mixing time is 30-60 minutes; and / or, Step (3), the temperature during the mixing is 90-150°C; preferably, mechanical stirring is used for the mixing, and more preferably, the mixing time is 30-60 minutes; and / or, In step (4), the temperature during the mixing is 20-60° C.; preferably, mechanical stirring is used for the mixing, and more preferably, the mixing time is 2-5 min.

12. A flame retardant epoxy resin cured product prepared by curing a flame retardant epoxy resin composition comprising a flame retardant epoxy resin composition according to any one of claims 1 to 8 or a flame retardant epoxy resin composition prepared by the method according to any one of claims 9 to 11, preferably, the flame retardant grade of the flame retardant epoxy resin cured product is UL94-V0 or above.

13. Use of the flame retardant epoxy resin composition according to any one of claims 1 to 8, the flame retardant epoxy resin composition prepared by the method according to any one of claims 9 to 11, or the flame retardant epoxy resin cured product according to claim 12 in flame retardancy.

Citation Information

Patent Citations

  • Halogen-free flame retardant anhydride cured epoxy resin composition

    CN104610704A

  • Novel flame-retardant composite solid material

    CN104893654A

  • Halogen-free flame retardant and flame-retardant resin composition with good flame retardance and processability

    CN112409693A

  • Halogen-free flame-retarding epoxy resin composition containing phosphor and nitrogen and preimpregnated material and laminate containing same

    CN1488672A

  • Halogen free ignition resistant thermoplastic resin compositions

    CN1659217A