Polyamide resin composition, molded article, and method for producing polyamide resin composition
By introducing fatty acid metal salts of alkali metal and/or alkaline earth metal into the polyamide resin composition, combining aliphatic and semiaromatic polyamides, the lack of surface appearance and mechanical characteristics of the polyamide resin in high-period molding is solved. The problem is that the water absorption rigidity, surface appearance and permeability of the molded product have been improved.
Patent Information
- Application Number
- CN202410616332.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-05-19
- Filing Date
- 2024-05-17
- Publication Date
- 2024-11-22
AI Technical Summary
The existing polyamide resin compositions have both surface appearance and mechanical characteristics under high-period molding conditions, especially the crystallization speed of polyhexamide resin and semi-aromatic amorphous polyamide resin 6T/6I is slow and the suitability is poor. It is difficult to take into account the surface appearance and high-period molding requirements of molded products.
Using a polyamide resin composition containing a fatty acid metal salt of alkali metal and/or alkaline earth metal, the metal ion distribution with a gamma distribution of metal ion is 1.0 or more, combined with aliphatic polyamide, semi-aromatic polyamide and inorganic filling Material to improve the water absorption rigidity, surface appearance and leakage resistance of molded products.
The molded products under high-period molding conditions have excellent water absorption rigidity, surface appearance and leakage resistance, and are suitable for use in a variety of industrial and electronic components.
Smart Images

Figure BDA0004845371330000031 
Figure BDA0004845371330000081 
Figure BDA0004845371330000441
Abstract
Description
Technical Field
[0001] The present invention relates to a polyamide resin composition, a molded product and a method for producing the polyamide resin composition. Background Art
[0002] Generally, polyamide resins have excellent mechanical properties as well as heat resistance, impact resistance, and chemical resistance, and are therefore widely used in automobile parts, electrical parts, electronic parts, household goods, and the like.
[0003] In recent years, from the viewpoint of economical efficiency and environmental issues, there is a strong demand for polyamide resins with wider moldability and wider use environment, especially polyamide resin materials with improved rigidity after water absorption (water absorption rigidity) and rigidity under high temperature use (thermal rigidity) and small changes in physical properties when used in all environments.
[0004] In addition, in order to improve productivity, molded products using polyamide resins are sometimes molded under high-cycle molding conditions by increasing the molding temperature and lowering the mold temperature. On the other hand, when molding is performed under high-temperature conditions, sometimes the polyamide resin decomposes or changes in fluidity and cannot stably obtain molded products. Therefore, polyamide resins that are excellent in the stability of the surface appearance of molded products even under the above-mentioned harsh molding conditions and are suitable for high-cycle molding are particularly required.
[0005] In order to meet such requirements, as materials capable of improving the surface appearance and mechanical properties of molded products, the following are disclosed: polyamide comprising polyamide 66 / 6I into which an isophthalic acid component is introduced (for example, refer to Patent Document 1); and a polyamide resin composition comprising a polycaproamide resin, a semi-aromatic amorphous polyamide resin 6T / 6I and an inorganic reinforcing material (for example, refer to Patent Document 2).
[0006] In addition, as a material capable of improving mechanical properties, fluidity, surface appearance, etc., a polyamide resin composition including polyamide 6T / 6I introduced with a terephthalic acid component and an isophthalic acid component is disclosed (for example, see Patent Document 3).
[0007] In addition, a material obtained by combining a polyamide resin composition and a release agent for the purpose of improving demolding properties is disclosed (for example, refer to Patent Documents 4 and 5), and it is reported that by combining aliphatic metal salts of stearic acid and ester compounds, amide compounds, etc. as release agents, the adhesion between the molded product and the mold wall surface is reduced.
[0008] Prior art literature
[0009] Patent Literature
[0010] Patent Document 1: Japanese Patent Application Laid-Open No. 6-032980
[0011] Patent Document 2: Japanese Patent Application Publication No. 2000-154316
[0012] Patent Document 3: Japanese Patent Application Laid-Open No. 11-349806
[0013] Patent Document 4: Japanese Patent Application Laid-Open No. 11-42666
[0014] Patent Document 5: Japanese Patent Application Publication No. 2013-147641 Summary of the invention
[0015] Problems to be solved by the invention
[0016] However, the techniques disclosed in Patent Documents 1 to 5 are insufficient to achieve both suitability for high-cycle molding in terms of productivity and surface appearance of molded products. In particular, the polyamide resin composition comprising polycaproamide resin and semi-aromatic amorphous polyamide resin 6T / 6I described in Patent Document 2 has a slow crystallization rate, poor suitability for high-cycle molding, and room for improvement in production processability. Therefore, it is difficult to achieve both surface appearance of molded products and suitability for high-cycle molding.
[0017] The present invention is made in view of the above situation, and provides a polyamide resin composition which has excellent rigidity, surface appearance and oozing resistance when formed into a molded article and is suitable for high-cycle molding, a molded article containing the polyamide resin composition, and a method for producing the polyamide resin composition.
[0018] Means used to solve problems
[0019] That is, the present invention is as follows. (1)
[0021] A polyamide resin composition, characterized in that the polyamide resin composition contains a polyamide resin (A) and a fatty acid metal salt (B) of a metal including an alkali metal and / or an alkaline earth metal,
[0022] The polyamide resin composition contains 0.05 parts by mass or more and 5.00 parts by mass or less of the fatty acid metal salt (B) relative to 100 parts by mass of the polyamide resin (A),
[0023] In the area distribution related to the spatial area per metal ion of the fatty acid metal salt (B) calculated by subjecting the surface of the polyamide resin composition to the following measurement, a shape parameter k of the gamma distribution is 1.0 or more.
[0024] [Measurement]
[0025] In order to calculate the spatial area of each metal ion on the surface of the polyamide resin composition, in a distribution image or an intensity information image of a metal ion image obtained by mapping the metal ions of the fatty acid metal salt (B) on the surface of the polyamide resin composition, Voronoi segmentation is performed with the center of the metal ion as the parent point. The spatial area of each region obtained by the Voronoi segmentation is calculated, each spatial area is classified, and a shape parameter k is calculated based on a gamma distribution represented by the following formula.
[0026]
[0027] (where k: shape parameter, θ: scale parameter, x: spatial area) (2)
[0029] The polyamide resin composition as described in (1), wherein the fatty acid metal salt (B) is a fatty acid metal salt having a terminal hydrocarbon group with 19 or more carbon atoms. (3)
[0031] The polyamide resin composition as described in (1) or (2), wherein the polyamide resin (A) is an aliphatic polyamide (Aa), a semi-aromatic polyamide (Ab) containing a diamine unit and a dicarboxylic acid unit, or a mixture of an aliphatic polyamide (Aa) and a semi-aromatic polyamide (Ab). (4)
[0033] The polyamide resin composition as described in (3), wherein
[0034] When the polyamide resin (A) is set to 100 parts by mass, the polyamide resin composition contains:
[0035] 50 parts by mass or more and 99 parts by mass or less of the aliphatic polyamide (Aa),
[0036] 1 part by mass or more and 50 parts by mass or less of the semi-aromatic polyamide (Ab),
[0037] 0.05 parts by mass or more and 5.00 parts by mass or less of the fatty acid metal salt (B), and
[0038] 0.01 parts by mass or more and 3.00 parts by mass or less of the fatty acid amide compound (C). (5)
[0040] The polyamide resin composition according to (4), wherein a ratio Bw / Cw of a mass Bw of the fatty acid metal salt (B) to a mass Cw of the fatty acid amide compound (C) is 0.6 or more and 4.0 or less. (6)
[0042] The polyamide resin composition as described in (4) or (5), wherein the ratio Bn / Cn of the number of carbon atoms Bn of the terminal hydrocarbon group of the fatty acid metal salt (B) to the number of carbon atoms Cn of the terminal hydrocarbon group of the fatty acid amide compound (C) is greater than 1.00 and less than or equal to 2.00. (7)
[0044] The polyamide resin composition according to any one of (3) to (6), wherein the aliphatic polyamide (Aa) is polyamide 6 or polyamide 66. (8)
[0046] The polyamide resin composition as described in any one of (3) to (7), wherein the semi-aromatic polyamide (Ab) contains 50 mol% or more of isophthalic acid units based on all dicarboxylic acid units constituting the semi-aromatic polyamide (Ab), and the semi-aromatic polyamide (Ab) contains a diamine unit having 4 to 10 carbon atoms as the diamine unit. (9)
[0048] A polyamide resin composition as described in any one of (3) to (7), wherein the semi-aromatic polyamide (Ab) contains 75 mol% or more of isophthalic acid units relative to all dicarboxylic acid units constituting the semi-aromatic polyamide (Ab), and the semi-aromatic polyamide (Ab) contains a diamine unit having 4 to 10 carbon atoms as the diamine unit. (10)
[0050] The polyamide resin composition according to any one of (1) to (9), wherein the weight average molecular weight Mw of the polyamide resin (A) is 10,000 or more and 50,000 or less. (11)
[0052] The polyamide resin composition according to any one of (1) to (10), wherein the molecular weight distribution Mw / Mn of the polyamide resin (A) is 2.4 or less. (12)
[0054] The polyamide resin composition according to any one of (1) to (11), wherein the fatty acid metal salt (B) is at least one selected from the group consisting of sodium montanate and calcium montanate. (13)
[0056] The polyamide resin composition as described in any one of (4) to (12), wherein the fatty acid amide compound (C) is one or more selected from the group consisting of fatty acid amide compounds having a hydrocarbon group having 9 to 30 carbon atoms and fatty acid bisamide compounds having a hydrocarbon group having 9 to 30 carbon atoms. (14)
[0058] The polyamide resin composition according to any one of (4) to (13), wherein the fatty acid amide compound (C) is at least one selected from the group consisting of N,N′-ethylenebisstearylamide and N-stearyl erucamide. (15)
[0060] The polyamide resin composition according to any one of (1) to (14), further comprising an inorganic filler (D).
[0061] The content of the inorganic filler (D) is 5 parts by mass or more and 200 parts by mass or less relative to 100 parts by mass of the polyamide resin (A). (16)
[0063] The polyamide resin composition according to any one of (1) to (15), further comprising aniline black (E),
[0064] The content of the aniline black (E) is greater than 0 parts by mass and less than or equal to 0.5 parts by mass relative to 100 parts by mass of the polyamide resin (A). (17)
[0066] The polyamide resin composition according to any one of (1) to (16), wherein the chloride ion content is 5 ppm or less on a mass basis. (18)
[0068] A molded article, characterized in that the molded article comprises the polyamide resin composition according to any one of (1) to (17). (19)
[0070] A production method, which is the production method of the polyamide resin composition according to any one of (1) to (17), characterized in that:
[0071] The production method includes the step of melt-kneading the polyamide resin (A) and the fatty acid metal salt (B).
[0072] Effects of the Invention
[0073] According to the present invention, a polyamide resin composition which is excellent in rigidity, surface appearance and oozing resistance when a molded product is made and is suitable for high-cycle molding, and a method for producing the same, as well as a molded product comprising the polyamide resin composition and having excellent rigidity, surface appearance and oozing resistance when a molded product is made and has excellent rigidity, surface appearance and oozing resistance when a molded product is absorbed can be provided. DETAILED DESCRIPTION
[0074] Hereinafter, a method for implementing the present invention (hereinafter referred to as "this embodiment") is described in detail. The following this embodiment is an example for illustrating the present invention and is not intended to limit the present invention to the following contents. The present invention can be implemented after being appropriately deformed within the scope of its purpose.
[0075] In addition, in this specification, "polyamide" means a polymer having an amide group (-NHCO-) in the main chain.
[0076] 《Polyamide resin composition》
[0077] The polyamide resin composition of the present embodiment is a polyamide resin composition containing a polyamide resin (A) and a fatty acid metal salt (B) of a metal including an alkali metal and / or an alkaline earth metal, characterized in that, in the area distribution related to the spatial area of each metal ion of the fatty acid metal salt (B) calculated by using the surface of the polyamide resin composition for the following measurement, the shape parameter k of the gamma distribution is greater than 1.0.
[0078] [Measurement]
[0079] In order to calculate the spatial area of each metal ion on the surface of the polyamide resin composition, in a distribution image or an intensity information image of a metal ion image obtained by mapping the metal ions of the fatty acid metal salt (B) on the surface of the polyamide resin composition, Voronoi segmentation is performed with the center of the metal ion as the parent point. The spatial area of each region obtained by the Voronoi segmentation is calculated, each spatial area is classified, and a shape parameter k is calculated based on a gamma distribution represented by the following formula.
[0080]
[0081] (where k: shape parameter, θ: scale parameter, x: spatial area)
[0082] The polyamide resin composition of the present embodiment has the above-mentioned structure, and can provide a molded article having excellent rigidity, surface appearance, and bleed-out resistance when absorbing water, and can be suitable for high-cycle molding.
[0083] Hereinafter, the details of each constituent component of the polyamide resin composition according to the present embodiment will be described.
[0084] <Polyamide resin (A)>
[0085] The polyamide resin (A) is not particularly limited, and examples thereof include aliphatic polyamide (Aa), semi-aromatic polyamide (Ab) containing a diamine unit and a dicarboxylic acid unit, and a mixture of an aliphatic polyamide (Aa) and a semi-aromatic polyamide (Ab).
[0086] The polyamide resin (A) may be one kind alone or a combination of two or more kinds.
[0087] <Aliphatic polyamide (Aa)>
[0088] The aliphatic polyamide (Aa) preferably contains one or more units (Aa-1) selected from the group consisting of lactam units and aminocarboxylic acid units, or contains an aliphatic dicarboxylic acid unit (Aa-2) and an aliphatic diamine unit (Aa-3).
[0089] [One or more units selected from the group consisting of lactam units and aminocarboxylic acid units (Aa-1)]
[0090] The aliphatic polyamide (Aa) may contain one or more units (Aa-1) selected from the group consisting of lactam units and aminocarboxylic acid units. By containing such units, there is a tendency to obtain a polyamide having excellent toughness.
[0091] It should be noted that the "lactam unit and aminocarboxylic acid unit" referred to herein refers to polymerized (polycondensed) lactam and aminocarboxylic acid.
[0092] The lactam constituting the lactam unit is not particularly limited, but is preferably a lactam having 4 to 14 carbon atoms, and more preferably a lactam having 6 to 12 carbon atoms.
[0093] Specific examples of the lactam include butyrolactam, pivalolactam, ε-caprolactam, capryllactam, enantholactam, undecanolactam, and laurolactam (lauryllactam), but the lactam is not limited thereto.
[0094] Among them, as the lactam, ε-caprolactam or laurolactam is preferred, and ε-caprolactam is more preferred. The inclusion of a lactam unit derived from such a lactam tends to provide a polyamide resin composition having further excellent toughness.
[0095] It should be noted that the "lactam constituting the lactam unit" referred to herein refers to a lactam that can be polymerized (polycondensed).
[0096] The aminocarboxylic acid constituting the aminocarboxylic acid unit is not particularly limited, but an aminocarboxylic acid having 4 to 14 carbon atoms is preferred, and an aminocarboxylic acid having 6 to 12 carbon atoms is more preferred.
[0097] Specific examples of the aminocarboxylic acid include ω-aminocarboxylic acid and α,ω-amino acid, which are compounds obtained by ring-opening of lactam, but are not limited thereto.
[0098] In addition, as the aminocarboxylic acid, a linear or branched saturated aliphatic carboxylic acid having 4 to 14 carbon atoms substituted with an amino group at the ω position is preferred. Examples of such aminocarboxylic acids include, but are not limited to, 6-aminocaproic acid, 11-aminoundecanoic acid, and 12-aminododecanoic acid. In addition, as the aminocarboxylic acid, p-aminomethylbenzoic acid and the like can also be mentioned.
[0099] In addition, the "aminocarboxylic acid constituting the aminocarboxylic acid unit" mentioned here refers to an aminocarboxylic acid that can be polymerized (polycondensed).
[0100] The lactam and the aminocarboxylic acid constituting the lactam unit and the aminocarboxylic acid unit may be used alone or in combination of two or more.
[0101] [Aliphatic dicarboxylic acid unit (Aa-2)]
[0102] Examples of the aliphatic dicarboxylic acid constituting the aliphatic dicarboxylic acid unit (Aa-2) include, but are not limited to, linear or branched saturated aliphatic dicarboxylic acids having 3 to 20 carbon atoms, such as malonic acid, dimethylmalonic acid, succinic acid, 2,2-dimethylsuccinic acid, 2,3-dimethylglutaric acid, 2,2-diethylsuccinic acid, 2,3-diethylglutaric acid, glutaric acid, 2,2-dimethylglutaric acid, adipic acid, 2-methyladipic acid, trimethyladipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, dodecanedioic acid, tetradecanedioic acid, hexadecanedioic acid, octadecanedioic acid, eicosanedioic acid, and diglycolic acid.
[0103] From the viewpoint of having a tendency to be more excellent in heat resistance, fluidity, toughness, low water absorption and rigidity of the polyamide resin composition, the aliphatic dicarboxylic acid preferably contains an aliphatic dicarboxylic acid having 6 or more carbon atoms. The aliphatic dicarboxylic acid having 6 or more carbon atoms is not particularly limited, and examples thereof include adipic acid, sebacic acid, dodecanedioic acid, tetradecanedioic acid, hexadecanedioic acid, octadecanedioic acid, eicosanedioic acid, etc. Among them, from the viewpoint of heat resistance of the polyamide resin composition, adipic acid, sebacic acid or dodecanedioic acid is more preferred.
[0104] The aliphatic dicarboxylic acid constituting the aliphatic dicarboxylic acid unit (Aa-2) may be used alone or in combination of two or more.
[0105] The aliphatic polyamide (Aa) may further contain a unit derived from a trivalent or higher polycarboxylic acid such as trimellitic acid, trimesic acid, or pyromellitic acid as necessary within a range not impairing the effects exerted by the polyamide resin composition of the present embodiment.
[0106] The trivalent or higher polyvalent carboxylic acid may be used alone or in combination of two or more.
[0107] [Aliphatic diamine unit (Aa-3)]
[0108] The aliphatic diamine constituting the aliphatic diamine unit (Aa-3) may be linear or branched.
[0109] Examples of the linear aliphatic diamine constituting the aliphatic diamine unit (Aa-3) include, but are not limited to, linear saturated aliphatic diamines having 2 to 20 carbon atoms, such as ethylenediamine, propylenediamine, tetramethylenediamine, pentamethylenediamine, hexamethylenediamine, heptamethylenediamine, octamethylenediamine, nonamethylenediamine, decamethylenediamine, undecamethylenediamine, dodecamethylenediamine, and tridecamethylenediamine.
[0110] Examples of the branched aliphatic diamine (a diamine constituting a diamine unit having a substituent branching from a main chain) constituting the aliphatic diamine unit (Aa-3) include, but are not limited to, branched saturated aliphatic diamines having a carbon number of 3 or more and 20 or less, such as 2-methylpentamethylenediamine (also called 2-methyl-1,5-diaminopentane), 2,2,4-trimethylhexamethylenediamine, 2,4,4-trimethylhexamethylenediamine, 2-methyl-1,8-octanediamine (also called 2-methyloctamethylenediamine), and 2,4-dimethyloctamethylenediamine.
[0111] Among them, 2-methylpentamethylenediamine or 2-methyl-1,8-octanediamine is preferred, and 2-methylpentamethylenediamine is more preferred. The inclusion of the aliphatic diamine unit (Aa-3) derived from such an aliphatic diamine tends to provide a polyamide resin composition having better heat resistance, rigidity, and the like.
[0112] The number of carbon atoms in the aliphatic diamine unit (Aa-3) is more preferably 6 or more and 12 or less, and further preferably 6 or more and 10 or less. When the number of carbon atoms is at least the above lower limit, the heat resistance tends to be more excellent, while when the number of carbon atoms is at most the above upper limit, the crystallinity and the mold release property tend to be more excellent.
[0113] The aliphatic diamine constituting the aliphatic diamine unit may be used alone or in combination of two or more.
[0114] The aliphatic polyamide (Aa) may further contain a unit derived from a trivalent or higher-valent aliphatic amine such as bis-hexamethylenetriamine as necessary within a range not impairing the effects exerted by the polyamide resin composition of the present embodiment.
[0115] The trivalent or higher polyvalent aliphatic amines may be used alone or in combination of two or more.
[0116] As the aliphatic polyamide (Aa), specifically, polyamide 6 (PA6), polyamide 66 (PA66), etc. can be cited. PA6 is excellent in terms of mechanical properties, appearance, moldability and toughness, and is therefore considered to be a material suitable for automotive parts. PA66 is excellent in heat resistance, especially in mechanical properties at high temperatures.
[0117] [Content of Aliphatic Polyamide (Aa)]
[0118] In the case where the polyamide resin (A) is a mixture of an aliphatic polyamide (Aa) and a semi-aromatic polyamide (Ab), the content of the aliphatic polyamide (Aa) is preferably 50 parts by mass or more and 99 parts by mass or less, more preferably 50 parts by mass or more and 90 parts by mass or less, further preferably 60 parts by mass or more and 85 parts by mass or less, further preferably 65 parts by mass or more and 82 parts by mass or less, particularly preferably 70 parts by mass or more and 80 parts by mass or less, and most preferably 75 parts by mass or more and 80 parts by mass or less. When the content of the aliphatic polyamide (Aa) is within the above range, there is a tendency to obtain a polyamide resin composition having excellent mechanical properties, molding processability, anti-bleeding, and laser printing properties and suitable for high-cycle molding. In addition, for a polyamide resin composition also containing an inorganic filler (D) represented by glass fiber described later, there is a tendency to have a more excellent surface appearance.
[0119] <Semi-aromatic polyamide (Ab)>
[0120] The semi-aromatic polyamide (Ab) is a polyamide containing a diamine unit (Abb) and a dicarboxylic acid unit (Aba). When the aliphatic polyamide (Aa) and the semi-aromatic polyamide (Ab) are combined in the polyamide resin (A) of the present embodiment, the fatty acid metal salt (B) tends to be well dispersed on the surface of the molded product during molding.
[0121] The semi-aromatic polyamide (Ab) preferably contains 20 mol% to 80 mol% of aromatic structural units relative to all structural units of the semi-aromatic polyamide (Ab), more preferably contains 30 mol% to 70 mol% of aromatic structural units, and further preferably contains 40 mol% to 60 mol% of aromatic structural units.
[0122] It should be noted that the "aromatic structural unit" referred to herein refers to an aromatic diamine unit and an aromatic dicarboxylic acid unit.
[0123] [Dicarboxylic acid unit (Aba)]
[0124] The dicarboxylic acid unit (Aba) may include, for example, an aromatic dicarboxylic acid unit, an aliphatic dicarboxylic acid unit, an alicyclic dicarboxylic acid unit, etc., without particular limitation. Among them, it is preferred to include an isophthalic acid unit.
[0125] The content of the isophthalic acid unit relative to 100 mol % of all dicarboxylic acid units (Aba) constituting the semi-aromatic polyamide (Ab) is preferably 50 mol % or more, more preferably 65 mol % or more, further preferably 70 mol % or more, further preferably 75 mol % or more, particularly preferably 80 mol % or more and 100 mol % or less, and most preferably 100 mol %.
[0126] When the ratio of the isophthalic acid unit in the dicarboxylic acid unit (Aba) is not less than the above lower limit, there is a tendency to obtain a polyamide resin composition having all of mechanical properties, particularly water absorption rigidity, thermal rigidity, fluidity, surface appearance, etc., further improved.
[0127] In addition, the ratio of the predetermined monomer unit which comprises a semi-aromatic polyamide (Ab) can be measured by nuclear magnetic resonance spectroscopy (NMR) etc.
[0128] (Aromatic dicarboxylic acid unit)
[0129] Examples of the aromatic dicarboxylic acid constituting the aromatic dicarboxylic acid unit include, but are not limited to, dicarboxylic acids having a phenyl group, a naphthyl group, and the like in addition to the above-mentioned isophthalic acid. The aromatic group of the aromatic dicarboxylic acid may be unsubstituted or may have a substituent.
[0130] There are no particular restrictions on the substituent, and examples thereof include: alkyl groups having 1 to 4 carbon atoms, aryl groups having 6 to 10 carbon atoms, aralkyl groups having 7 to 10 carbon atoms, halogen groups such as chloro and bromo groups, silyl groups having 1 to 6 carbon atoms, sulfonic acid groups and salts thereof (sodium salts, etc.), and the like.
[0131] Examples of the aromatic dicarboxylic acid include, in addition to the above-mentioned isophthalic acid, terephthalic acid, naphthalene dicarboxylic acid, 2-chloroterephthalic acid, 2-methylterephthalic acid, 5-methylisophthalic acid, sodium 5-sulfonate of isophthalic acid, and the like, but are not limited thereto, to aromatic dicarboxylic acids having 8 to 20 carbon atoms which are unsubstituted or substituted with a prescribed substituent.
[0132] The aromatic dicarboxylic acid constituting the aromatic dicarboxylic acid unit may be used alone or in combination of two or more.
[0133] (Aliphatic dicarboxylic acid unit)
[0134] Examples of the aliphatic dicarboxylic acid constituting the aliphatic dicarboxylic acid unit include, but are not limited to, linear or branched saturated aliphatic dicarboxylic acids having 3 to 20 carbon atoms, such as malonic acid, dimethylmalonic acid, succinic acid, 2,2-dimethylsuccinic acid, 2,3-dimethylglutaric acid, 2,2-diethylsuccinic acid, 2,3-diethylglutaric acid, glutaric acid, 2,2-dimethylglutaric acid, adipic acid, 2-methyladipic acid, trimethyladipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, dodecanedioic acid, tetradecanedioic acid, hexadecanedioic acid, octadecanedioic acid, eicosanedioic acid, and diglycolic acid.
[0135] (alicyclic dicarboxylic acid unit)
[0136] Examples of the alicyclic dicarboxylic acid constituting the alicyclic dicarboxylic acid unit (hereinafter also referred to as "alicyclic dicarboxylic acid unit") include, but are not limited to, alicyclic dicarboxylic acids having an alicyclic structure with carbon atoms of 3 or more and 10 or less, preferably alicyclic dicarboxylic acids having carbon atoms of 5 or more and 10 or less.
[0137] Examples of such alicyclic dicarboxylic acids include, but are not limited to, 1,4-cyclohexanedicarboxylic acid, 1,3-cyclohexanedicarboxylic acid, and 1,3-cyclopentanedicarboxylic acid. Among them, 1,4-cyclohexanedicarboxylic acid is preferred.
[0138] In addition, the alicyclic dicarboxylic acid which comprises an alicyclic dicarboxylic acid unit may be used individually by 1 type, or may use 2 or more types together.
[0139] The alicyclic group of the alicyclic dicarboxylic acid may be unsubstituted or may have a substituent. Examples of the substituent include, but are not limited to, alkyl groups having 1 to 4 carbon atoms, such as methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, and tert-butyl.
[0140] In the semi-aromatic polyamide (Ab), preferred dicarboxylic acid units (Aba) other than isophthalic acid units include aromatic dicarboxylic acid units other than isophthalic acid units, and more preferably aromatic dicarboxylic acid units other than isophthalic acid units having 8 or more carbon atoms.
[0141] When such a dicarboxylic acid unit (Aba) is contained, the polyamide resin composition tends to have more excellent mechanical properties, particularly water absorption rigidity, thermal rigidity, fluidity, surface appearance, and the like.
[0142] In the present specification, the dicarboxylic acid constituting the dicarboxylic acid unit (Aba) is not limited to the compounds described as the above-mentioned dicarboxylic acids, and may be a compound equivalent to the above-mentioned dicarboxylic acids.
[0143] It should be noted that the "compound equivalent to a dicarboxylic acid" referred to herein refers to a compound that can form a dicarboxylic acid structure similar to the dicarboxylic acid structure derived from the above dicarboxylic acid. Examples of such compounds include, but are not limited to, anhydrides and acyl halides of dicarboxylic acids.
[0144] The semi-aromatic polyamide (Ab) may further contain a unit derived from a trivalent or higher polyvalent carboxylic acid such as trimellitic acid, trimesic acid, or pyromellitic acid as necessary within a range not impairing the effects exerted by the polyamide resin composition of the present embodiment.
[0145] The trivalent or higher polyvalent carboxylic acid may be used alone or in combination of two or more.
[0146] [Diamine unit (Abb)]
[0147] The diamine unit (Abb) constituting the semi-aromatic polyamide (Ab) may include, for example, an aromatic diamine unit, an aliphatic diamine unit, an alicyclic diamine unit, etc., without particular limitation, and preferably includes a diamine unit having 4 to 10 carbon atoms.
[0148] The content of the diamine units having 4 to 10 carbon atoms is preferably 50 mol% or more, more preferably 80 mol% or more and 100 mol% or less, further preferably 90 mol% or more and 100 mol% or less, and particularly preferably 100 mol% based on 100 mol% of all diamine units (Abb) constituting the semi-aromatic polyamide (Ab).
[0149] When the content of the diamine unit having 4 to 10 carbon atoms in the diamine unit (Abb) is equal to or more than the above lower limit, a polyamide resin composition tends to be obtained in which all mechanical properties, particularly water absorption rigidity, thermal rigidity, fluidity, surface appearance, and bleed resistance, are further improved.
[0150] (Aliphatic diamine unit)
[0151] Examples of the aliphatic diamine constituting the aliphatic diamine unit include, but are not limited to, linear saturated aliphatic diamines having 4 to 20 carbon atoms, such as ethylenediamine, propylenediamine, tetramethylenediamine, pentamethylenediamine, hexamethylenediamine, heptamethylenediamine, octamethylenediamine, nonamethylenediamine, decamethylenediamine, undecamethylenediamine, dodecamethylenediamine, and tridecamethylenediamine.
[0152] (Alicyclic diamine unit)
[0153] Examples of the alicyclic diamine (hereinafter also referred to as “alicyclic diamine”) constituting the alicyclic diamine unit include, but are not limited to, 1,4-cyclohexanediamine, 1,3-cyclohexanediamine, and 1,3-cyclopentanediamine.
[0154] (Aromatic diamine unit)
[0155] The aromatic diamine constituting the aromatic diamine unit may be any diamine containing an aromatic group, and is not limited to the following, but examples thereof include meta-xylylenediamine.
[0156] These diamines constituting the diamine unit (Abb) may be used alone or in combination of two or more.
[0157] Among the diamine units (Abb), aliphatic diamine units are preferred, diamine units having a linear saturated aliphatic group having 4 to 10 carbon atoms are more preferred, diamine units having a linear saturated aliphatic group having 6 to 10 carbon atoms are further preferred, and hexamethylenediamine units are particularly preferred.
[0158] By including such a diamine unit, there is a tendency for the polyamide resin composition to have more excellent mechanical properties, particularly water absorption rigidity, thermal rigidity, fluidity, surface appearance, and the like.
[0159] The semi-aromatic polyamide (Ab) may further contain a unit derived from a trivalent or higher polyvalent aliphatic amine such as bis-hexamethylenetriamine as necessary within a range not impairing the effects exerted by the polyamide resin composition of the present embodiment.
[0160] The trivalent or higher polyvalent aliphatic amines may be used alone or in combination of two or more.
[0161] As the semi-aromatic polyamide (Ab), polyamide 6I (polyhexamethylene isophthalamide), polyamide 6I / 6T, polyamide MXD6, polyamide 9I or polyamide 10I is preferred, and polyamide 6I is more preferred. Polyamide 6I is excellent in heat resistance, molding processability and flame retardancy, and is therefore considered to be a material suitable for automotive parts.
[0162] [Content of semi-aromatic polyamide (Ab)]
[0163] In the case where the polyamide resin (A) is a mixture of an aliphatic polyamide (Aa) and a semi-aromatic polyamide (Ab), the content of the semi-aromatic polyamide (Ab) is preferably 1 part by mass or more and 50 parts by mass or less, more preferably 10 parts by mass or more and 50 parts by mass or less, further preferably 15 parts by mass or more and 40 parts by mass or less, further preferably 18 parts by mass or more and 35 parts by mass or less, particularly preferably 20 parts by mass or more and 30 parts by mass or less, and most preferably 20 parts by mass or more and 25 parts by mass or less. When the content of the semi-aromatic polyamide (Ab) is within the above range, there is a tendency to obtain a polyamide resin composition having excellent mechanical properties, molding processability, anti-bleeding, and laser printability and suitable for high-cycle molding. In addition, for a polyamide resin composition further containing an inorganic filler (D) represented by glass fiber described later, there is a tendency to have a more excellent surface appearance.
[0164] <Capping agent>
[0165] The ends of the polyamide resin (A) may be blocked with a known terminal blocking agent.
[0166] When the polyamide resin (A) is produced from the above-mentioned dicarboxylic acid and diamine and, if necessary, at least one selected from the group consisting of lactam and aminocarboxylic acid, such a terminal blocking agent can also be added as a molecular weight modifier.
[0167] Examples of the terminal blocking agent include monocarboxylic acids, monoamines, acid anhydrides such as phthalic anhydride, monoisocyanates, monoacyl halides, monoesters, and monoalcohols, but are not limited thereto.
[0168] Among them, monocarboxylic acid or monoamine is preferred. When the terminal of the polyamide resin (A) is capped with an end-capping agent, a polyamide resin composition tends to have better thermal stability.
[0169] The terminal blocking agent may be used alone or in combination of two or more.
[0170] The monocarboxylic acid that can be used as the end-capping agent is any monocarboxylic acid that is reactive with the amino group that may be present at the end of the polyamide resin (A). Examples thereof include, but are not limited to, aliphatic monocarboxylic acids such as formic acid, acetic acid, propionic acid, butyric acid, valeric acid, caproic acid, caprylic acid, lauric acid, tridecanoic acid, myristic acid, palmitic acid, stearic acid, pivalic acid, and isobutyric acid; alicyclic monocarboxylic acids such as cyclohexanecarboxylic acid; and aromatic monocarboxylic acids such as benzoic acid, methyl benzoic acid, α-naphthoic acid, β-naphthoic acid, methyl naphthoic acid, and phenylacetic acid.
[0171] In particular, from the viewpoint of fluidity and mechanical strength, the terminal of the semi-aromatic polyamide (Ab) is preferably capped with acetic acid.
[0172] The monocarboxylic acid may be used alone or in combination of two or more.
[0173] The monoamine that can be used as the end-capping agent is any monoamine that is reactive with the carboxyl group that may be present at the end of the polyamide resin (A). Examples thereof include, but are not limited to, aliphatic monoamines such as methylamine, ethylamine, propylamine, butylamine, hexylamine, octylamine, decylamine, stearylamine, dimethylamine, diethylamine, dipropylamine, and dibutylamine; alicyclic monoamines such as cyclohexylamine and dicyclohexylamine; and aromatic monoamines such as aniline, toluidine, diphenylamine, and naphthylamine.
[0174] The monoamines may be used alone or in combination of two or more.
[0175] The polyamide resin composition containing the polyamide resin (A) end-capped with an end-capping agent tends to be more excellent in heat resistance, fluidity, toughness, low water absorption and rigidity.
[0176] <Method for producing polyamide resin (A)>
[0177] The method for producing the polyamide resin (A) will be described.
[0178] When the polyamide resin (A) is produced, the amount of the dicarboxylic acid added and the amount of the diamine added are preferably about the same molar amount. Regarding the molar ratio, taking into account the amount of the diamine dissipated to the outside of the reaction system during the polymerization reaction, the molar amount of the diamine as a whole relative to the molar amount of the dicarboxylic acid as a whole is preferably 0.9 to 1.2, more preferably 0.95 to 1.1, and even more preferably 0.98 to 1.05.
[0179] The method for producing the polyamide resin (A) may include, for example, the following polymerization step (1) or (2), but is not limited thereto.
[0180] (1) A step of polymerizing one or more selected from the group consisting of lactam constituting a lactam unit and aminocarboxylic acid constituting an aminocarboxylic acid unit to obtain a polymer.
[0181] (2) A step of polymerizing a combination of a dicarboxylic acid constituting a dicarboxylic acid unit and a diamine constituting a diamine unit to obtain a polymer.
[0182] In addition, as the method for producing the polyamide resin (A), it is preferred that the polymerization step is followed by a step of increasing the degree of polymerization of the polyamide. In addition, if necessary, the polymerization step and the step of increasing the degree of polymerization of the polyamide may be followed by a step of capping the ends of the obtained polymer using a capping agent.
[0183] As a specific method for producing the polyamide resin (A), for example, various methods as exemplified in the following 1) to 4) can be mentioned.
[0184] 1) A method in which an aqueous solution or aqueous suspension of one or more selected from the group consisting of lactams, aminocarboxylic acids, dicarboxylic acid-diamine salts, and mixtures of dicarboxylic acids and diamines is heated and polymerized while being kept in a molten state (hereinafter sometimes referred to as "hot melt polymerization method").
[0185] 2) A method in which the degree of polymerization of a polyamide obtained by hot melt polymerization is increased while the polyamide is kept in a solid state at a temperature below the melting point (hereinafter, sometimes referred to as "hot melt polymerization / solid phase polymerization method").
[0186] 3) A method of polymerizing one or more selected from the group consisting of dicarboxylic acid-diamine salts, mixtures of dicarboxylic acids and diamines, lactams, and aminocarboxylic acids while maintaining a solid state (hereinafter sometimes referred to as "solid phase polymerization").
[0187] 4) A method of polymerizing using a dicarboxylic acid halide component equivalent to a dicarboxylic acid and a diamine component (hereinafter, sometimes referred to as a "solution method").
[0188] Among them, as a specific method for producing polyamide resin (A), a method for producing polyamide resin (A) by hot melt polymerization is preferably used. In addition, when producing polyamide resin (A) by hot melt polymerization, it is preferably kept in a molten state until the polymerization is completed. In order to keep the molten state, it is necessary to produce under polymerization conditions suitable for polyamide resin. As polymerization conditions, for example, the conditions shown below can be cited. First, the polymerization pressure in the hot melt polymerization is controlled at 14 kg / cm 2 Above and 25kg / cm 2 Next, the pressure in the tank was reduced over 30 minutes until it reached atmospheric pressure (gauge pressure: 0 kg / cm2 ).
[0189] In the method for producing the polyamide resin (A), the polymerization form is not particularly limited, and may be a batch type or a continuous type.
[0190] The polymerization apparatus used for producing the polyamide resin (A) is not particularly limited, and a known apparatus can be used. Specific examples of the polymerization apparatus include autoclave reactors, drum reactors, extruder reactors (kneaders, etc.), and the like.
[0191] Hereinafter, as a method for producing the polyamide resin (A), a method for producing the polyamide resin (A) by a batch hot melt polymerization method will be specifically described, but the method for producing the polyamide resin (A) is not limited thereto.
[0192] First, an aqueous solution containing about 40% by mass or more and about 60% by mass or less of a raw material component of a polyamide resin (A) (a mixture of a lactam, an aminocarboxylic acid or a dicarboxylic acid and a diamine) is prepared. Next, the aqueous solution is concentrated to about 65% by mass or more and about 90% by mass or less in a concentration tank operated at a temperature of 110° C. to 180° C. and a pressure of about 0.035 MPa to about 0.6 MPa (gauge pressure) to obtain a concentrated solution.
[0193] Next, the obtained concentrated solution was transferred to an autoclave, and heating was continued until the pressure in the autoclave reached about 1.2 MPa or more and about 2.2 MPa or less (gauge pressure).
[0194] Next, in the autoclave, the pressure is maintained at about 1.2 MPa or more and about 2.2 MPa or less (gauge pressure) while extracting at least one of the water and gas components. Next, when the temperature reaches about 220°C or more and about 260°C or less, the pressure is reduced to atmospheric pressure (gauge pressure is 0 MPa). After the pressure in the autoclave is reduced to atmospheric pressure, the pressure is reduced as needed, thereby effectively removing the by-product water.
[0195] Next, the autoclave is pressurized with an inert gas such as nitrogen, and the polyamide melt is extruded from the autoclave in the form of strands. The extruded strands are cooled and cut to obtain pellets of the polyamide resin (A).
[0196] <Polymer terminal of polyamide resin (A)>
[0197] The polymer terminal of the polyamide resin (A) is not particularly limited, but can be classified and defined as the following 1) to 4).
[0198] That is, 1) amino terminal, 2) carboxyl terminal, 3) terminal formed by a blocking agent, and 4) other terminal.
[0199] 1) The amino terminal is a polymer terminal having an amino group (-NH2 group) and is derived from a raw material diamine.
[0200] 2) The carboxyl terminal is a polymer terminal having a carboxyl group (-COOH group), and is derived from a raw material dicarboxylic acid.
[0201] 3) The terminal formed by the terminal blocking agent is a terminal formed when the terminal blocking agent is added during polymerization. Examples of the terminal blocking agent include the above-mentioned terminal blocking agents.
[0202] 4) Other terminals are polymer terminals not classified into the above 1) to 3), and examples thereof include terminals generated by deamination reaction of an amino terminal and terminals generated by decarboxylation reaction from a carboxyl terminal.
[0203] <Characteristics of polyamide resin (A)>
[0204] [Weight average molecular weight Mw]
[0205] As an index of the molecular weight of polyamide resin (A), weight average molecular weight Mw can be utilized.The weight average molecular weight Mw of polyamide resin (A) is preferably more than 10000 and less than 50000, more preferably more than 17000 and less than 40000, further preferably more than 20000 and less than 34000, more preferably more than 23000 and less than 33500, particularly preferably more than 25000 and less than 33000, most preferably more than 26000 and less than 32000.When weight average molecular weight Mw is within the above range, mechanical properties, especially water absorption rigidity, thermal rigidity, fluidity, demoulding properties etc. can be obtained.In addition, for the polyamide resin composition also containing the inorganic filler (D) represented by glass fiber described later, there is a tendency that surface appearance is more excellent.
[0206] Examples of a method for controlling the Mw of the polyamide resin (A) to fall within the above range include using an aliphatic polyamide (Aa) and a semi-aromatic polyamide (Ab) each having a Mw within the above range.
[0207] In addition, the measurement of Mw (weight average molecular weight) can be measured using GPC (gel permeation chromatography) as described in Examples mentioned later.
[0208] [Molecular weight distribution Mw / Mn]
[0209] The molecular weight distribution of the polyamide resin (A) is determined by weight average molecular weight Mw / number average molecular weight Mn as an index.
[0210] The Mw / Mn of the polyamide resin (A) is 1.0 or more, preferably 2.4 or less, preferably 1.7 or more and 2.3 or less, preferably 1.8 or more and 2.2 or less, preferably 1.9 or more and 2.1 or less. When Mw / Mn is within the above range, there is a tendency to obtain a polyamide resin composition having better fluidity, etc. In addition, for a polyamide resin composition also containing an inorganic filler (D) represented by glass fiber described later, there is a tendency to have a better surface appearance.
[0211] As a method for controlling the Mw / Mn of the polyamide resin (A) to be within the above range, when the semi-aromatic polyamide (Ab) is included, the molecular weight distribution Mw of the semi-aromatic polyamide (Ab) is adjusted to (A-b) / Mn (A-b) It is important to control Mw / Mn within the above range.
[0212] When a large number of aromatic compound units are contained in the molecular structure of the polyamide resin (A), the molecular weight distribution (Mw / Mn) tends to increase as the molecular weight increases. A high molecular weight distribution means that the ratio of polyamide molecules with a three-dimensional molecular structure is high, and the three-dimensional structuralization of the molecules is easier to proceed during high-temperature processing, and the fluidity is reduced. Therefore, for a polyamide resin composition that also contains an inorganic filler (D) represented by glass fiber described later, the surface appearance may deteriorate. Therefore, by increasing the molecular weight distribution Mw of the semi-aromatic polyamide (Ab), the molecular weight distribution Mw of the semi-aromatic polyamide (Ab) is increased. (A-b) / Mn (A-b) By controlling the content to be below the above upper limit, the surface appearance can be further improved.
[0213] In addition, the measurement of Mw / Mn of the polyamide resin (A) can be calculated using the weight average molecular weight Mw and the number average molecular weight Mn obtained by GPC as described in Examples described later.
[0214] <Characteristics of Aliphatic Polyamide (Aa)>
[0215] [Weight average molecular weight Mw (A-a) ]
[0216] As an indicator of the molecular weight of the aliphatic polyamide (Aa), the weight average molecular weight Mw can be used. (A-a) . Mw of aliphatic polyamide (Aa) (A-a) It is preferably 10,000 to 50,000, more preferably 15,000 to 45,000, further preferably 20,000 to 40,000, and particularly preferably 25,000 to 37,000.
[0217] When Mw (A-a)When the molecular weight is within the above range, there is a tendency to obtain a polyamide resin composition having better mechanical properties, especially water absorption rigidity, thermal rigidity, fluidity, etc. In addition, for a polyamide resin composition further containing an inorganic filler (D) represented by glass fiber described later, there is a tendency to have a better surface appearance. It should be noted that the measurement of the weight average molecular weight Mw (Aa) can be measured using GPC.
[0218] [Molecular weight distribution Mw (A-a) / Mn (A-a) ]
[0219] The molecular weight distribution of aliphatic polyamide (Aa) is the weight average molecular weight Mw (A-a) / Number average molecular weight Mn (A-a) As an indicator.
[0220] Molecular weight distribution Mw of aliphatic polyamide (Aa) (A-a) / Mn (A-a) It can be 1.0 or more, preferably 1.8 or more and 2.5 or less, and more preferably 1.9 or more and 2.4 or less. (A-a) / Mn (A-a) When the content is within the above range, a polyamide resin composition having better fluidity etc. tends to be obtained. In addition, a polyamide resin composition further containing an inorganic filler (D) represented by glass fiber described later tends to have better surface appearance.
[0221] As the molecular weight distribution Mw (A-a) / Mn (A-a) The method of controlling within the above range includes, for example, adding a known polycondensation catalyst such as phosphoric acid or sodium hypophosphite as an additive during the hot melt polymerization of the aliphatic polyamide (Aa); and controlling the polymerization conditions such as heating conditions and reduced pressure conditions.
[0222] Molecular weight distribution Mw (A-a) / Mn (A-a ) can be measured using the weight average molecular weight Mw obtained by GPC (A-a) , number average molecular weight Mn (A-a) calculate.
[0223] <Characteristics of semi-aromatic polyamide (Ab)>
[0224] [Weight average molecular weight Mw (A-b) ]
[0225] As an indicator of the molecular weight of the semi-aromatic polyamide (Ab), the weight average molecular weight Mw can be used. (A-b) . Weight average molecular weight Mw (A-b)It is preferably 10,000 to 50,000, more preferably 13,000 to 40,000, further preferably 15,000 to 35,000, particularly preferably 18,000 to 30,000, and most preferably 19,000 to 29,000.
[0226] When the weight average molecular weight Mw (A-b) When the content is within the above range, a polyamide resin composition having more excellent mechanical properties, particularly water absorption rigidity, thermal rigidity, fluidity, etc., tends to be obtained. In addition, a polyamide resin composition further containing an inorganic filler (D) represented by glass fiber described later tends to have more excellent surface appearance.
[0227] It should be noted that the weight average molecular weight Mw (A-b ) can be measured using GPC.
[0228] [Molecular weight distribution Mw (A-b) / Mn (A-b) ]
[0229] The molecular weight distribution of semi-aromatic polyamide (Ab) is the weight average molecular weight Mw (A-b) / Number average molecular weight Mn (A-b) As an indicator.
[0230] Molecular weight distribution Mw of semi-aromatic polyamide (Ab) (A-b) / Mn (A-b) It can be 1.0 or more, preferably 2.4 or less, more preferably 1.7 or more and 2.4 or less, further preferably 1.8 or more and 2.3 or less, particularly preferably 1.9 or more and 2.2 or less, and most preferably 1.9 or more and 2.1 or less.
[0231] When the molecular weight distribution Mw (A-b) / Mn (A-b) When the content is within the above range, a polyamide resin composition having better fluidity etc. tends to be obtained. In addition, a polyamide resin composition further containing an inorganic filler (D) represented by glass fiber described later tends to have better surface appearance.
[0232] As the molecular weight distribution Mw (A-b) / Mn (A-b)The method of controlling the temperature within the above range includes, for example, a method of adding a known polycondensation catalyst such as phosphoric acid and sodium hypophosphite as an additive during the hot melt polymerization of the semi-aromatic polyamide (Ab). In addition, a method of controlling the polymerization conditions such as heating conditions and reduced pressure conditions can be mentioned. It is important to complete the polycondensation reaction at a low temperature and in a short time. In particular, when the semi-aromatic polyamide (Ab) is an amorphous polyamide, since it has no melting point, the reaction temperature can be lowered.
[0233] When a large number of aromatic compound units are contained in the molecular structure of polyamide (A), the molecular weight distribution Mw (A-b) / Mn (A-b) The tendency of the molecular weight distribution to increase with the molecular weight. A high molecular weight distribution means that the ratio of polyamide molecules with a three-dimensional molecular structure is high, and the three-dimensional structuralization of the molecules is easier to proceed during high-temperature processing, and the fluidity is reduced. Therefore, for a polyamide resin composition that also contains an inorganic filler (D) represented by glass fiber described later, the surface appearance may deteriorate. Therefore, by adjusting the molecular weight distribution Mw (A-b) / Mn (A-b) By controlling the content to be below the above upper limit, the surface appearance can be further improved.
[0234] It should be noted that the molecular weight distribution Mw (A-b) / Mn (A-b ) can be measured using the weight average molecular weight Mw obtained by GPC (A-b) , number average molecular weight Mn (A-b) Perform calculations.
[0235] <Metal salt of fatty acid (B)>
[0236] The fatty acid metal salt (B) is a fatty acid metal salt of a metal containing an alkali metal ion and / or an alkaline earth metal ion. That is, the metal element constituting the fatty acid metal salt (B) is not particularly limited as long as it contains an alkali metal and / or an alkaline earth metal, and may contain zinc, aluminum, etc., for example.
[0237] Examples of the alkali metal include sodium and potassium.
[0238] Examples of the alkaline earth metal include calcium and magnesium.
[0239] Among them, sodium, potassium, calcium, magnesium or aluminum is more preferred.
[0240] The fatty acid constituting the fatty acid metal salt (B) may be chain-shaped or cyclic, but is preferably chain-shaped. In addition, when the fatty acid constituting the fatty acid metal salt (B) is chain-shaped, it may be straight-chain or branched, but is preferably straight-chain. Examples of straight-chain fatty acids include lauric acid, myristic acid, pentadecanoic acid, palmitic acid, heptadecanoic acid, stearic acid, eicosanoic acid, behenic acid, lignoceric acid, cerotic acid, montanic acid, and melissic acid.
[0241] The fatty acid metal salt (B) is not particularly limited as long as it is a combination of a metal element including an alkali metal and / or an alkaline earth metal and a fatty acid. However, from the viewpoint of nucleation effect and fluidity, a metal salt of a higher fatty acid having a terminal hydrocarbon group with 12 or more carbon atoms is preferred, and a metal salt of a higher fatty acid having a terminal hydrocarbon group with 19 or more carbon atoms is more preferred.
[0242] In addition, as such a fatty acid metal salt (B), a montanic acid salt is preferred, and sodium montanic acid or calcium montanic acid is more preferred.
[0243] These fatty acid metal salts (B) may be used alone or in combination of two or more.
[0244] [Content of fatty acid metal salt (B)]
[0245] The content of the fatty acid metal salt (B) is 0.05 to 5.00 parts by mass, preferably 0.05 to 1.00 parts by mass, and more preferably 0.10 to 0.50 parts by mass, relative to 100 parts by mass of the polyamide resin (A).
[0246] When the content of the fatty acid metal salt (B) is above the above lower limit, a polyamide resin composition more suitable for high cycle molding can be obtained. On the other hand, when the content of the fatty acid metal salt (B) is below the above upper limit, a polyamide resin composition having better mechanical properties such as toughness and rigidity, especially water absorption properties, can be obtained without impairing the properties of the polyamide resin (A).
[0247] <Fatty acid amide compound (C)>
[0248] The polyamide resin composition of the present embodiment can contain a fatty acid amide compound (C).
[0249] When the polyamide resin composition of the present embodiment contains the fatty acid amide compound (C), the dispersibility of the fatty acid metal salt (B) can be improved, and a polyamide resin composition having better molding cycle, and better anti-bleeding and laser printability when a molded product is obtained can be obtained.
[0250] The fatty acid amide compound (C) is preferably one or more selected from the group consisting of an amide compound of an aliphatic carboxylic acid (fatty acid) having a terminal hydrocarbon group with a carbon number of 9 or more and 30 or less and a bisamide compound of an aliphatic carboxylic acid (fatty acid) having a terminal hydrocarbon group with a carbon number of 9 or more and 30 or less. That is, the fatty acid amide compound (C) is preferably one or more selected from the group consisting of a fatty acid amide compound having a hydrocarbon group with a carbon number of 9 or more and 30 or less at the terminal and a fatty acid bisamide compound having a hydrocarbon group with a carbon number of 9 or more and 30 or less at one or both terminals. The above-mentioned terminal hydrocarbon group of the fatty acid amide compound (C) more preferably has a carbon number of 12 or more and 27 or less, and further preferably has a carbon number of 17 or more and 21 or less.
[0251] As fatty acid amide compound (C), for example, capric amide, lauryl amide, palmitamide, stearic amide, oleic amide, erucic amide, N-stearyl stearic amide, N-stearyl oleic amide, N-oleyl stearic amide, N-stearyl erucic amide, N-oleyl oleic amide, N-hydroxymethyl stearic amide, N,N'-methylene bis stearic amide, N,N'-ethylene bis capric amide, N,N'-ethylene bis lauryl amide, N,N'-ethylene bis stearic amide, N,N'-ethylene bis behenic amide, N,N'-hexamethylene bis stearic amide, N,N'-hexamethylene bis behenic amide, N,N'-ethylene bis oleic amide, N,N'-ethylene bis erucic amide, N,N'-hexamethylene bis oleic amide, etc. can be cited, but it is not limited thereto. Among them, bisamide compounds are preferred, and N,N'-ethylene bis stearic amide or N-stearyl erucic amide is more preferred.
[0252] These fatty acid amide compounds (C) may be used alone or in combination of two or more.
[0253] [Content of fatty acid amide compound (C)]
[0254] The content of the fatty acid amide compound (C) is preferably 0.01 to 3.00 parts by mass, more preferably 0.05 to 2.00 parts by mass, and further preferably 0.10 to 1.00 parts by mass, relative to 100 parts by mass of the polyamide resin (A).
[0255] When the content of the fatty acid amide compound (C) is above the above lower limit, a polyamide resin composition having better processability can be obtained. On the other hand, when the content of the fatty acid amide compound (C) is below the above upper limit, a polyamide resin composition having better mechanical properties such as toughness and rigidity, especially water absorption properties, can be obtained without damaging the properties of the polyamide resin (A).
[0256] In the polyamide resin composition, the ratio Bw / Cw of the mass Bw of the fatty acid metal salt (B) to the mass Cw of the fatty acid amide compound (C) is preferably 0.6 or more and 4.0 or less, more preferably 0.8 or more and 3.8 or less, further preferably 1.0 or more and 3.5 or less, further preferably 1.5 or more and 3.4 or less, and particularly preferably 2.0 or more and 3.0 or less. When the mass ratio Bw / Cw is above the above lower limit, a polyamide resin composition more suitable for high cycle molding can be prepared. In addition, when the mass ratio Bw / Cw is below the above upper limit, a polyamide resin composition having better surface appearance and mechanical properties can be prepared.
[0257] The ratio Bn / Cn of the carbon number Bn of the terminal hydrocarbon group of the fatty acid metal salt (B) and the carbon number Cn of the terminal hydrocarbon group of the fatty acid amide compound (C) is preferably greater than 1.00 and less than or equal to 2.00, more preferably 1.01 or more and 2.00 or less, more preferably 1.10 or more and 1.80 or less, and more preferably 1.35 or more and 1.60 or less. By the carbon number ratio Bn / Cn being greater than the above lower limit or being above the above lower limit, a polyamide resin composition that is more suitable for high cycle molding, exudation resistance after molding, and laser printability can be made. In addition, when the carbon number ratio Bn / Cn is below the upper limit, a polyamide resin composition that is more excellent in surface appearance and mechanical properties can be made.
[0258] When carbon number ratio Bn / Cn is within the above range, fatty acid amide compound (C) works as the emulsifier of polyamide matrix and fatty acid metal salt (B), therefore the dispersibility of fatty acid metal salt (B) in polyamide resin composition can be improved dramatically.When carbon number ratio Bn / Cn is greater than the above upper limit, the compatibility of fatty acid amide compound (C) and fatty acid metal salt (B) is low, therefore interaction is small, there is the tendency that the dispersion diameter of fatty acid metal salt (B) is constant.In addition, when carbon number ratio Bn / Cn is below the above lower limit or less than the above lower limit, the compatibility of fatty acid amide compound (C) and fatty acid metal salt (B) becomes high, therefore fatty acid metal salt (B) is encapsulated in the micelle of fatty acid amide compound (C), there is the tendency that the seepage of fatty acid metal salt (B) is prevented when molding. Therefore, when the carbon atom ratio Bn / Cn is controlled within the above range, the fatty acid metal salt (B) on the surface of the molded product will not be unevenly distributed during molding but will be more evenly dispersed. Therefore, a polyamide resin composition can be made that is more suitable for high-cycle molding without damaging the appearance, and has better anti-bleeding properties after molding and laser printing properties.
[0259] <Inorganic filler (D)>
[0260] The polyamide resin composition of the present embodiment preferably further contains an inorganic filler (D). By containing the inorganic filler (D), a polyamide resin composition having more excellent mechanical properties such as toughness and rigidity and more suitable for high-cycle molding can be obtained.
[0261] The inorganic filler (D) is not particularly limited, and examples thereof include glass fiber, carbon fiber, calcium silicate fiber, potassium titanate fiber, aluminum borate fiber, flaky glass, talc, kaolin, mica, hydrotalcite, zinc carbonate, calcium hydrogen phosphate, wollastonite, zeolite, boehmite, magnesium oxide, calcium silicate, sodium aluminosilicate, magnesium silicate, Ketjen black, acetylene black, furnace black, carbon nanotubes, graphite, brass, copper, silver, aluminum, nickel, iron, calcium fluoride, montmorillonite, swelling fluorine mica, apatite, and the like.
[0262] These inorganic fillers (D) may be used alone or in combination of two or more.
[0263] Among them, as the inorganic filler (D), glass fiber, carbon fiber, flaky glass, talc, kaolin, mica, calcium hydrogen phosphate, wollastonite, carbon nanotubes, graphite, calcium fluoride, montmorillonite, swelling fluorine mica or apatite are preferred from the viewpoints of rigidity and strength. In addition, as the inorganic filler (D), glass fiber or carbon fiber is more preferred, and glass fiber is further preferred.
[0264] In the case where the inorganic filler (D) is glass fiber or carbon fiber, the number average fiber diameter (d) is preferably 3 μm or more and 30 μm or less, more preferably 5 μm or more and 17 μm or less. In addition, the weight average fiber length (L) is preferably 100 μm or more and 750 μm or less. In addition, the aspect ratio ((L) / (d)) of the weight average fiber length (L) relative to the number average fiber diameter (d) is preferably 3 or more and 100 or less, more preferably 10 or more and 100 or less. By using the glass fiber or carbon fiber of the above-mentioned structure, higher characteristics can be exhibited.
[0265] In addition, especially when the inorganic filler (D) is glass fiber, the number average fiber diameter (d) is preferably 3 μm or more and 30 μm or less, more preferably 5 μm or more and 17 μm or less, and particularly preferably 7 μm or more and 13 μm or less. In addition, the weight average fiber length (L) is more preferably 103 μm or more and 500 μm or less. In addition, the aspect ratio ((L) / (d)) is preferably 3 or more and 100 or less.
[0266] The number average fiber diameter (d) and the weight average fiber length (L) of the inorganic filler (D) can be measured by the following method.
[0267] First, polyamide resin composition is put into electric furnace, and contained organic matter is incinerated. From the residue component after this treatment, arbitrarily select more than 100 inorganic fillers (D), utilize scanning electron microscope (SEM) to observe, and measure the fiber diameter (major diameter) of these inorganic fillers (D), thus number average fiber diameter (d) can be obtained. In addition, use the SEM photo measurement fiber length of the above-mentioned more than 100 inorganic fillers (D) taken with 1000 times of multiple, thus weight average fiber length (L) can be obtained.
[0268] The content of the inorganic filler (D) in the polyamide resin composition is preferably 5 parts by mass or more and 200 parts by mass or less, more preferably 10 parts by mass or more and 200 parts by mass or less, further preferably 20 parts by mass or more and 150 parts by mass or less, particularly preferably 30 parts by mass or more and 120 parts by mass or less, and most preferably 40 parts by mass or more and 100 parts by mass or less, relative to 100 parts by mass of the polyamide resin (A).
[0269] When the content of the inorganic filler (D) is above the above lower limit, the mechanical properties such as strength and rigidity of the polyamide resin composition are further improved, and a polyamide resin composition more suitable for high-cycle molding can be prepared. On the other hand, when the content of the inorganic filler (D) is below the above upper limit, a polyamide resin composition with better surface appearance can be obtained.
[0270] <Aniline Black (E)>
[0271] The polyamide resin composition of the present embodiment can contain aniline black (E). The polyamide resin composition of the present embodiment contains aniline black (E), and the interaction between aniline black (E) and the fatty acid metal salt (B) is used to improve the dispersibility of the fatty acid metal salt (B), so that a polyamide resin composition with better molding periodicity, surface glossiness when a molded product is made, and laser printability can be prepared.
[0272] The content of aniline black (E) in the polyamide resin composition is preferably greater than 0 part by mass and less than or equal to 0.5 part by mass, more preferably greater than 0.01 part by mass and less than 0.3 part by mass, and further preferably greater than 0.05 part by mass and less than 0.1 part by mass, relative to 100 parts by mass of the polyamide resin (A).
[0273] When the content of aniline black (E) is above the above lower limit, a polyamide resin composition having better molding periodicity, surface glossiness when a molded product is made, and laser printability can be obtained. On the other hand, when the content of aniline black (E) is below the above upper limit, a polyamide resin composition having better laser printability can be obtained.
[0274] The aniline black (E) contained in the polyamide resin composition of the present embodiment may contain chloride ions (Cl - ). In aniline black (E), the content of chloride ions is preferably 5000 ppm or less, more preferably 2500 ppm or less, and further preferably 1000 ppm or less, based on mass. By setting the content of chloride ions to 5000 ppm or less, based on mass, the interaction with the fatty acid metal salt (B) is appropriately adjusted, the dispersibility of the fatty acid metal salt (B) becomes good, and there is a tendency for the shape parameter k to increase.
[0275] The chloride ion content in the polyamide resin composition of the present embodiment is not particularly limited. In the polyamide resin composition, the chloride ion content is preferably 5 ppm or less, more preferably 2.5 ppm or less, and further preferably 1 ppm or less, based on the mass basis. When the chloride ion content is 5 ppm or less based on the mass basis, the interaction with the fatty acid metal salt (B) is appropriately adjusted, the dispersibility of the fatty acid metal salt (B) becomes good, and there is a tendency for the shape parameter k to increase.
[0276] The chloride ion content in the polyamide resin composition can be adjusted by adjusting the chloride ion content of each component constituting the polyamide resin composition or the content ratio of each component.
[0277] <Other ingredients (F)>
[0278] The polyamide resin composition of the present embodiment may contain other components (F) within the range that does not impair the effects of the polyamide resin composition of the present embodiment. Examples of other components (F) include heat stabilizers, other polymers, metal phosphites, metal hypophosphites, phosphite compounds, and other additives.
[0279] The other components (F) may be used alone or in combination of two or more.
[0280] [Heat stabilizer]
[0281] Examples of the heat stabilizer include phenolic heat stabilizers, phosphorus-containing heat stabilizers, amine heat stabilizers, metal salts of elements of Group 3, Group 4, and Groups 11 to 14 of the periodic table, and halides of alkali metals or alkaline earth metals, but are not limited thereto.
[0282] Examples of phenolic heat stabilizers include, but are not limited to, hindered phenol compounds, etc. Hindered phenol compounds have the property of imparting excellent heat resistance and light resistance to resins such as polyamide and fibers.
[0283] Examples of the hindered phenol compound include N,N'-hexane-1,6-diylbis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionamide], pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], N,N'-hexamethylenebis(3,5-di-tert-butyl-4-hydroxyhydrocinnamic acid amide), triethylene glycol bis[3-(3-tert-butyl-5-methyl-4-hydroxyphenyl)propionate], 3,9-bis{2- [3-(3-tert-butyl-4-hydroxy-5-methylphenyl)propionyloxy]-1,1-dimethylethyl}-2,4,8,10-tetraoxaspiro[5.5]undecane, diethyl 3,5-di-tert-butyl-4-hydroxybenzylphosphonate, 1,3,5-trimethyl-2,4,6-tris(3,5-di-tert-butyl-4-hydroxybenzyl)benzene and 1,3,5-tris(4-tert-butyl-3-hydroxy-2,6-dimethylbenzyl)isocyanuric acid, etc., but are not limited thereto.
[0284] These hindered phenol compounds may be used alone or in combination of two or more.
[0285] In particular, from the viewpoint of improving heat aging resistance, as the hindered phenol compound, N,N′-hexane-1,6-diylbis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionamide] is preferred.
[0286] When a phenolic heat stabilizer is used, the content of the phenolic heat stabilizer in the polyamide resin composition is preferably 0.01% by mass to 1% by mass, more preferably 0.1% by mass to 1% by mass, relative to the total mass of the polyamide resin composition. When the content of the phenolic heat stabilizer is within the above range, the extrusion processability and molding stability of the polyamide resin composition can be further improved, and the gas generation can be further reduced.
[0287] Examples of the phosphorus-containing heat stabilizer include pentaerythritol-type phosphite compounds, trioctyl phosphite, trilauryl phosphite, tridecyl phosphite, diphenyl octyl phosphite, triisodecyl phosphite, diisodecyl phenyl phosphite, ditridecyl phenyl phosphite, isooctyl diphenyl phosphite, isodecyl diphenyl phosphite, tridecyl diphenyl phosphite, triphenyl phosphite, tris(nonylphenyl) phosphite, tris(2,4-di-tert-butylphenyl) phosphite, tris(2,4-di-tert-butyl-5-methylphenyl) phosphite, tris(butyloxy)phosphite Phosphite, 4,4'-butylidene bis(3-methyl-6-tert-butylphenyl) ester-tetra(tridecyl) ester, diphosphite, 4,4'-isopropylidene diphenyl ester-tetra(C12-C15 mixed alkyl) ester, phosphite, 4,4'-isopropylidene bis(2-tert-butylphenyl) ester-di(nonylphenyl) ester, tris(biphenyl) phosphite, 1,1,3-tris(2-methyl-5-tert-butyl-4-hydroxyphenyl) butane diphosphite tetra(tridecyl) ester, diphosphite, 4,4'-butylidene bis(3-methyl-6-tert-butylphenyl) ester-tetra(tridecyl) ester, diphosphite, 4,4 '-Isopropylidene diphenyl ester-tetra(C1~C15 mixed alkyl) ester, tris(mono- and di-mixed nonylphenyl) phosphite, 4,4'-isopropylidene bis(2-tert-butylphenyl) phosphite-di(nonylphenyl) ester, 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide, tris(3,5-di-tert-butyl-4-hydroxyphenyl) phosphite, 4,4'-isopropylidene diphenyl polyphosphite hydrogenated, bis(4,4'-butylidene bis(3-methyl-6-tert-butylphenyl))-1,6-hexanediol diphosphite di(octylphenyl) ester, 1,1,3-tris(2-methyl-4- Hydroxy-5-tert-butylphenyl) butane triphosphite hexa(tridecyl) ester, tris(4,4'-isopropylidenebis(2-tert-butylphenyl)) phosphite, tris(1,3-distearoyloxyisopropyl) phosphite, 2,2'-methylenebis(4,6-di-tert-butylphenyl) octyl phosphite, 2,2'-methylenebis(3-methyl-4,6-di-tert-butylphenyl) phosphite-2-ethylhexyl ester, 4,4'-biphenylene diphosphite tetra(2,4-di-tert-butyl-5-methylphenyl) ester and 4,4'-biphenylene diphosphite tetra(2,4-di-tert-butylphenyl) ester, etc., but are not limited thereto.
[0288] These phosphorus-containing heat stabilizers may be used alone or in combination of two or more.
[0289] Among them, the phosphorus-containing heat stabilizer is preferably one or more selected from the group consisting of pentaerythritol-type phosphite compounds and tris(2,4-di-tert-butylphenyl) phosphite from the viewpoint of further improving the extrusion processability and molding stability of the polyamide resin composition and reducing the amount of gas generated.
[0290] Examples of the pentaerythritol type phosphite compounds include pentaerythritol diphosphite 2,6-di-tert-butyl-4-methylphenyl ester-phenyl ester, pentaerythritol diphosphite 2,6-di-tert-butyl-4-methylphenyl ester-methyl ester, pentaerythritol diphosphite 2,6-di-tert-butyl-4-methylphenyl ester-2-ethylhexyl ester, pentaerythritol diphosphite 2,6-di-tert-butyl-4-methylphenyl ester-isodecyl ester, pentaerythritol diphosphite 2,6-di-tert-butyl-4-methylphenyl ester-lauryl ... Phosphite 2,6-di-tert-butyl-4-methylphenyl ester-isotridecyl ester, Pentaerythritol diphosphite 2,6-di-tert-butyl-4-methylphenyl ester-stearyl ester, Pentaerythritol diphosphite 2,6-di-tert-butyl-4-methylphenyl ester-cyclohexyl ester, Pentaerythritol diphosphite 2,6-di-tert-butyl-4-methylphenyl ester-benzyl ester, Pentaerythritol diphosphite 2,6-di-tert-butyl-4-methylphenyl ester-ethyl cellosolve ester, Pentaerythritol diphosphite 2,6-di-tert-butyl-4-methylphenyl ester-butyl carbitol Ester, pentaerythritol diphosphite 2,6-di-tert-butyl-4-methylphenyl ester-octylphenyl ester, pentaerythritol diphosphite 2,6-di-tert-butyl-4-methylphenyl ester-nonylphenyl ester, pentaerythritol diphosphite bis (2,6-di-tert-butyl-4-methylphenyl) ester, pentaerythritol diphosphite bis (2,6-di-tert-butyl-4-ethylphenyl) ester, pentaerythritol diphosphite 2,6-di-tert-butyl-4-methylphenyl ester-2,6-di-tert-butylphenyl ester, pentaerythritol diphosphite 2,6-di-tert-butyl-4-methyl Phenyl ester-2,4-di-tert-butylphenyl ester, pentaerythritol diphosphite 2,6-di-tert-butyl-4-methylphenyl ester-2,4-di-tert-octylphenyl ester, pentaerythritol diphosphite 2,6-di-tert-butyl-4-methylphenyl ester-2-cyclohexylphenyl ester, pentaerythritol diphosphite 2,6-di-tert-pentyl-4-methylphenyl ester-phenyl ester, pentaerythritol diphosphite di(2,6-di-tert-pentyl-4-methylphenyl) ester and pentaerythritol diphosphite di(2,6-di-tert-octyl-4-methylphenyl) ester, etc., but are not limited thereto.
[0291] These pentaerythritol-type phosphite compounds may be used alone or in combination of two or more.
[0292] Among them, as the pentaerythritol type phosphite compound, from the viewpoint of reducing the amount of gas generated by the polyamide resin composition, preferably, at least one selected from the group consisting of pentaerythritol diphosphite di(2,6-di-tert-butyl-4-methylphenyl) ester, pentaerythritol diphosphite di(2,6-di-tert-butyl-4-ethylphenyl) ester, pentaerythritol diphosphite di(2,6-di-tert-amyl-4-methylphenyl) ester and pentaerythritol diphosphite di(2,6-di-tert-octyl-4-methylphenyl) ester is used, and pentaerythritol diphosphite di(2,6-di-tert-butyl-4-methylphenyl) ester is more preferred.
[0293] When a phosphorus-containing heat stabilizer is used, the content of the phosphorus-containing heat stabilizer in the polyamide resin composition is preferably 0.01% by mass or more and 1% by mass or less, and more preferably 0.1% by mass or more and 1% by mass or less, relative to the total mass of the polyamide resin composition. When the content of the phosphorus-containing heat stabilizer is within the above range, the extrusion processability and molding stability of the polyamide resin composition can be further improved, and the gas generation can be further reduced.
[0294] Examples of the amine heat stabilizer include 4-acetoxy-2,2,6,6-tetramethylpiperidine, 4-stearoyloxy-2,2,6,6-tetramethylpiperidine, 4-acryloyloxy-2,2,6,6-tetramethylpiperidine, 4-(phenylacetoxy)-2,2,6,6-tetramethylpiperidine, 4-benzoyloxy-2,2,6,6-tetramethylpiperidine, 4-methoxy-2,2,6,6-tetramethylpiperidine, 4-stearoyloxy-2,2,6,6-tetramethylpiperidine, 4-cyclohexyloxy-2,2,6,6-tetramethylpiperidine, 4-benzyloxy-2,2,6,6-tetramethylpiperidine. Methylpiperidine, 4-phenoxy-2,2,6,6-tetramethylpiperidine, 4-(ethylcarbamoyloxy)-2,2,6,6-tetramethylpiperidine, 4-(cyclohexylcarbamoyloxy)-2,2,6,6-tetramethylpiperidine, 4-(phenylcarbamoyloxy)-2,2,6,6-tetramethylpiperidine, di(2,2,6,6-tetramethyl-4-piperidinyl) carbonate, di(2,2,6,6-tetramethyl-4-piperidinyl) oxalate, di(2,2,6,6-tetramethyl-4-piperidinyl) malonate, di(2,2,6,6-tetramethyl-4-piperidinyl) sebacate, hexane Bis(2,2,6,6-tetramethyl-4-piperidinyl) terephthalate, 1,2-bis(2,2,6,6-tetramethyl-4-piperidinyl) ethane, α,α'-bis(2,2,6,6-tetramethyl-4-piperidinyl) p-xylene, bis(2,2,6,6-tetramethyl-4-piperidinyl) toluene-2,4-dicarbamate, bis(2,2,6,6-tetramethyl-4-piperidinyl) hexamethylene-1,6-dicarbamate, tris(2,2,6,6-tetramethyl-4 Benzene-1,3,4-tricarboxylic acid tris(2,2,6,6-tetramethyl-4-piperidinyl) ester, 1-[2-{3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionyloxy}butyl]-4-[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionyloxy]-2,2,6,6-tetramethylpiperidine, 1,2,3,4-butanetetracarboxylic acid, 1,2,2,6,6-pentamethyl-4-piperidinol and β,β,β',β'-tetramethyl-3,9-[2,4,8,10-tetraoxaspiro(5.5)undecane]diethanol condensate, etc., but are not limited thereto.
[0295] These amine heat stabilizers may be used alone or in combination of two or more.
[0296] When an amine heat stabilizer is used, the content of the amine heat stabilizer in the polyamide resin composition is preferably 0.01% by mass or more and 1% by mass or less, and more preferably 0.1% by mass or more and 1% by mass or less, relative to the total mass of the polyamide resin composition. When the content of the amine heat stabilizer is within the above range, the extrusion processability and molding stability of the polyamide resin composition can be further improved, and the gas generation can be further reduced.
[0297] The metal salt of an element of Group 3, Group 4, and Groups 11 to 14 of the periodic table is not particularly limited as long as it is a salt of a metal belonging to these groups.
[0298] Among them, copper salts are preferred from the viewpoint of further improving the extrusion processability and molding stability of the polyamide resin composition. Examples of the copper salts include copper halides, copper acetate, copper propionate, copper benzoate, copper adipate, copper terephthalate, copper isophthalate, copper salicylate, copper nicotinate, copper stearate, and copper complex salts formed by coordination of copper and a chelating agent, but are not limited thereto.
[0299] Examples of the copper halide include cuprous iodide, cuprous bromide, cupric bromide, and cuprous chloride.
[0300] Examples of the chelating agent include ethylenediamine and ethylenediaminetetraacetic acid.
[0301] These copper salts may be used alone or in combination of two or more.
[0302] Among them, as the copper salt, at least one selected from the group consisting of cuprous iodide, cuprous bromide, cupric bromide, cuprous chloride and cupric acetate is preferred, and at least one selected from the group consisting of cuprous iodide and cupric acetate is more preferred. When the preferred copper salts listed above are used, a polyamide resin composition having better heat aging resistance and capable of more effectively suppressing metal corrosion of the screw and barrel during extrusion (hereinafter, sometimes referred to as "metal corrosion") can be obtained.
[0303] When copper salt is used as a heat stabilizer, the content of copper salt in the polyamide resin composition is preferably 0.01 to 0.60 parts by mass, more preferably 0.02 to 0.40 parts by mass, relative to 100 parts by mass of the polyamide resin (A). When the content of copper salt is within the above range, the extrusion processability and molding stability of the polyamide resin composition can be further improved, and the precipitation of copper and metal corrosion can be more effectively suppressed.
[0304] In addition, from the viewpoint of improving the heat aging resistance of the polyamide resin composition, 6The content concentration of the copper element derived from the copper salt in parts by mass (1,000,000 parts by mass) of the polyamide resin (A) is preferably 10 parts by mass or more and 2,000 parts by mass or less, more preferably 30 parts by mass or more and 1,500 parts by mass or less, and even more preferably 50 parts by mass or more and 500 parts by mass or less.
[0305] Examples of the alkali metal or alkaline earth metal halide include potassium iodide, potassium bromide, potassium chloride, sodium iodide, sodium chloride, and the like, but are not limited thereto.
[0306] These alkali metal or alkaline earth metal halides may be used alone or in combination of two or more.
[0307] Among them, as the halide of an alkali metal or an alkaline earth metal, from the viewpoint of improving heat aging resistance and suppressing metal corrosion, at least one selected from the group consisting of potassium iodide and potassium bromide is preferred, and potassium iodide is more preferred.
[0308] When an alkali metal or alkaline earth metal halide is used, the content of the alkali metal or alkaline earth metal halide in the polyamide resin composition is preferably 0.05 parts by mass or more and 20 parts by mass or less, and more preferably 0.2 parts by mass or more and 10 parts by mass or less, relative to 100 parts by mass of the polyamide resin (A). When the content of the alkali metal or alkaline earth metal halide is within the above range, the extrusion processability and molding stability of the polyamide resin composition can be further improved, and copper precipitation and metal corrosion can be more effectively suppressed.
[0309] The heat stabilizer components described above may be used alone or in combination of two or more.
[0310] Among them, as the heat stabilizer, a mixture of a copper salt and a halide of an alkali metal or an alkaline earth metal is preferred from the viewpoint of being able to further improve the extrusion processability and molding stability of the polyamide resin composition.
[0311] The content ratio of the copper salt to the halide of the alkali metal or alkaline earth metal is preferably 2 / 1 or more and 40 / 1 or less, more preferably 5 / 1 or more and 30 / 1 or less, based on the molar ratio of the halogen to the copper (halogen / copper). When the molar ratio of the halogen to the copper (halogen / copper) is within the above range, the extrusion processability and molding stability of the polyamide resin composition can be further improved.
[0312] In addition, when the molar ratio of halogen to copper (halogen / copper) is above the above lower limit, copper precipitation and metal corrosion can be more effectively suppressed. On the other hand, when the molar ratio of halogen to copper (halogen / copper) is below the above upper limit, corrosion of the screw of the molding machine can be more effectively prevented without almost impairing the mechanical properties (toughness, etc.).
[0313] [Other polymers]
[0314] Other polymers may be added within the range that the effect of the polyamide resin composition of the present embodiment is not impaired. As other polymers, there is no particular limitation as long as they are polymers other than polyamide, and examples thereof include polyesters, liquid crystal polyesters, polyphenylene sulfide, polyphenylene ether, polycarbonate, polyarylate, phenolic resin, epoxy resin, acrylic resin, styrene resin, etc. As polyesters, for example, polybutylene terephthalate, polytrimethylene terephthalate, polyethylene terephthalate, polyethylene naphthalate, etc. may be mentioned, but are not limited thereto.
[0315] The content of other polymers is preferably 1 to 200 parts by mass, more preferably 5 to 100 parts by mass, and further preferably 5 to 50 parts by mass, relative to 100 parts by mass of the polyamide resin (A). When the content of other polymers is within the above range, a polyamide resin composition having better heat resistance and demoulding properties can be prepared.
[0316] [Phosphite metal salt, hypophosphite metal salt]
[0317] The polyamide resin composition of the present embodiment may contain at least one metal salt selected from the group consisting of metal phosphites and metal hypophosphites. Examples of the metal phosphites and metal hypophosphites include salts of phosphorous acid, hypophosphorous acid, pyrophosphorous acid or diphosphorous acid with elements of Group 1 and Group 2 of the periodic table, manganese, zinc, aluminum, ammonia, alkylamines, cycloalkylamines or diamines.
[0318] Among them, as the phosphorous acid metal salt and the hypophosphite metal salt, sodium hypophosphite, calcium hypophosphite or magnesium hypophosphite is preferred.
[0319] When at least one metal salt selected from the group consisting of these phosphorous acid metal salts and hypophosphite metal salts is contained, a polyamide resin composition having further excellent extrusion processability and molding process stability can be obtained.
[0320] The content of at least one metal salt selected from the group consisting of metal phosphites and metal hypophosphites is preferably 0.001 to 1.0 parts by mass, more preferably 0.01 to 0.5 parts by mass, based on 100 parts by mass of the polyamide resin (A).
[0321] [Phosphite compounds]
[0322] Specific examples of the phosphite compound include trioctyl phosphite, trilauryl phosphite, tridecyl phosphite, dioctyl diphenyl phosphite, triisodecyl phosphite, diisodecyl phenyl phosphite, ditridecyl phenyl phosphite, isooctyl diphenyl phosphite, isodecyl diphenyl phosphite, tridecyl diphenyl phosphite, triphenyl phosphite, tributyl phosphite, tris(nonylphenyl) phosphite, tris(2,4-di-tert-butylphenyl) phosphite, ethyl di[2,4-bis(1,1-dimethylethyl)-6-methylphenyl] phosphite, and pentaerythritol diphosphite di(2,4-di-tert-butylphenyl) phosphite. Ester, pentaerythritol diphosphite di(2,6-di-tert-butyl-4-methylphenyl) ester, 2,2-methylenebis(4,6-di-tert-butylphenyl) phosphite octyl ester, 4,4'-butylidene bis(phosphite 3-methyl-6-tert-butylphenyl ester-di(tridecyl) ester), 1,1,3-tris(2-methyl-4-di(tridecyl)phosphite-5-tert-butylphenyl)butane, 4,4'-isopropylidene bis(phosphite phenyl ester-dialkyl ester), tris(2,4-di-tert-butylphenyl) phosphite, 2,2-methylenebis(4,6-di-tert-butylphenyl) phosphite octyl ester, pentaerythritol diphosphite di(2,6-di-tert-butyl-4-methylphenyl) ester, etc.
[0323] These phosphite compounds may be used alone or in combination of two or more.
[0324] When the phosphite compound is added, a polyamide resin composition having more excellent extrusion processability and molding process stability can be obtained.
[0325] The content of the phosphite compound is preferably 0.01 part by mass or more and 1.0 part by mass or less, and more preferably 0.05 part by mass or more and 0.5 part by mass or less, relative to 100 parts by mass of the polyamide resin (A).
[0326] [Other additives]
[0327] The polyamide resin composition of the present embodiment may contain other additives commonly used in polyamide resin compositions within the range that does not impair the effects of the polyamide resin composition of the present embodiment. Other additives include, for example, colorants such as pigments and dyes (including coloring masterbatches), flame retardants, fibrillating agents, fluorescent whitening agents, plasticizers, antioxidants, ultraviolet absorbers, antistatic agents, flowability improvers, extenders, elastomers, and the like.
[0328] When the polyamide resin composition of the present embodiment contains other additives, the content of other additives varies depending on the type of the other additives, the purpose of the polyamide resin composition, etc., and therefore, there is no particular limitation as long as it is within a range that does not impair the effects of the polyamide resin composition of the present embodiment. For example, relative to 100 mass % of the polyamide resin composition, the content of other additives can be greater than 0 mass % and less than 5 mass %, or can be greater than 0.01 mass % and less than 1.5 mass %.
[0329] <Method for producing polyamide resin composition>
[0330] The method for producing the polyamide resin composition is not particularly limited as long as it includes a step of melt-kneading the polyamide resin (A) and the fatty acid metal salt (B), the fatty acid amide compound (C) added as needed, the inorganic filler (D), aniline black (E) and other components (F).
[0331] Examples of a method for mixing the components (A) and (B) and, if necessary, the components (C) to (F) include the following method (1) or (2).
[0332] (1) A method in which the components (A) and (B) and, if necessary, (C) to (F) are mixed using a Henschel mixer or the like, and the mixture is supplied to a melt kneader and kneaded.
[0333] (2) A method in which the components (A) and (B) and the components (C), (E) and (F) added as needed are mixed in advance using a Henschel mixer or the like to prepare a mixture containing these components, the mixture is supplied to a melt-kneader and kneaded, and then the component (D) is added from a side feeder as needed and kneaded.
[0334] Regarding the method of supplying the components constituting the polyamide resin composition to the melt-kneader, all the components may be supplied at once from the same supply port, or the components may be supplied from different supply ports.
[0335] The melt kneading temperature is preferably about 1° C. or higher and about 100° C. or lower than the melting point of the polyamide resin (A), and more preferably about 10° C. or higher and about 60° C. or lower than the melting point of the polyamide resin (A).
[0336] The shear rate in the mixer is preferably about 100 seconds -1 In addition, the average residence time during kneading is preferably about 0.5 minutes or more and about 5 minutes or less.
[0337] The melt kneading machine may be any known device, and for example, a single-screw or twin-screw extruder, a Banbury mixer, a mixing roll, etc. are preferably used.
[0338] The amount of each component blended when producing the polyamide resin composition of the present embodiment is the same as the content of each component in the above-mentioned polyamide resin composition.
[0339] <Characteristics of polyamide resin composition>
[0340] [Dispersibility of Metal Ions of Fatty Acid Metal Salt (B) (Shape Parameter k)]
[0341] In the area distribution related to the spatial area of each metal ion of the fatty acid metal salt (B) calculated by subjecting the surface of the above-mentioned polyamide resin composition to the following measurement, the shape parameter k of the gamma distribution is greater than 1.0, preferably greater than 1.3, more preferably greater than 1.5, and even more preferably greater than 2.0.
[0342] When the dispersibility (shape parameter k) of the metal ions of the fatty acid metal salt (B) is equal to or greater than the above lower limit, a polyamide resin composition excellent in bleed resistance and suitable for high-cycle molding can be obtained.
[0343] [Measurement]
[0344] In order to calculate the spatial area of each metal ion on the surface of the polyamide resin composition, Voronoi segmentation is performed with the center of the metal ion as the parent point in a distribution image or an intensity information image of a metal ion image obtained by mapping the metal ions of the fatty acid metal salt (B) on the surface of the polyamide resin composition. The spatial area of each region obtained by the Voronoi segmentation is calculated, and each spatial area is classified to prepare a histogram, and the shape parameter k of the gamma distribution represented by the following formula is calculated from the distribution state of the histogram.
[0345]
[0346] (where k: shape parameter, θ: scale parameter, x: spatial area)
[0347] As a method for controlling the dispersibility (shape parameter k) of metal ions, there can be cited: a method of adjusting the outlet resin temperature of a melt kneader when manufacturing a polyamide resin composition; a method of adjusting the mass ratio Bw / Cw of a fatty acid metal salt (B) to a fatty acid amide compound (C), and the carbon atom number ratio Bn / Cn of a fatty acid metal salt (B) to a terminal hydrocarbon group of a fatty acid amide compound (C) when the polyamide resin composition contains a fatty acid amide compound (C); a method of adjusting the chloride ion content in the polyamide resin composition when the polyamide resin composition contains chloride ions due to the presence of aniline black (E) and the like. In order to keep the dispersibility (shape parameter k) of metal ions within the above range, it is preferred to adjust the outlet resin temperature in a melt kneader to 290° C. or more during the manufacture of the polyamide resin composition. In addition, it is preferred that the mass ratio Bw / Cw of a fatty acid metal salt (B) to a fatty acid amide compound (C) and the carbon atom number ratio Bn / Cn of a fatty acid metal salt (B) to a terminal hydrocarbon group of a fatty acid amide compound (C) satisfy the above range. In addition, it is preferred that the chloride ion content in the polyamide resin composition satisfy the above range.
[0348] The method for calculating the shape parameter k is not particularly limited as long as it is the following method: the spatial area of each metal ion is calculated by Voronoi segmentation from the distribution image obtained by mapping the metal ions of the fatty acid metal salt (B) on the surface of the polyamide resin composition or the intensity information image of the metal ion image, each spatial area is classified to produce a histogram, and the shape parameter k is calculated using a density function from the distribution state of the produced histogram.
[0349] As the analytical method used in the calculation of shape parameter k, as long as the method that the metal ion of the fatty acid metal salt (B) on the surface of polyamide resin composition can be mapped, there is no particular restriction, and known observation methods can be used. As known observation methods, for example, the molecules and element analysis methods of the surfaces commonly known such as scanning electron microscope-energy dispersive X-ray spectrometry (SEM-EDX), time-of-flight secondary ion mass spectrometry (TOF-SIMS) can be listed, but it is not limited thereto. It is also possible to measure the molded product as required, preferably on the smooth surface of the molded product of plate shape, etc.
[0350] The distribution image obtained by the above observation method tends to accurately obtain the ion distribution by binarizing the image using the Otsu method. Alternatively, when using the intensity information image of the metal ion image, it is possible to analyze the data by plotting without binarization.
[0351] 《Molding products》
[0352] The molded article of the present embodiment includes the polyamide resin composition of the present embodiment described above, and is obtained by molding the polyamide resin composition of the present embodiment described above.
[0353] There are no particular restrictions on the method for producing the molded article, and a known molding method can be used.
[0354] Examples of known molding methods include, but are not limited to, press molding, injection molding, gas-assisted injection molding, welding molding, extrusion molding, blow molding, film molding, hollow molding, multilayer molding, melt spinning and other commonly known plastic molding methods.
[0355] Furthermore, since the polyamide resin composition is suitable for high-cycle molding, the molded article of the present embodiment can be suitably produced by high-cycle molding.
[0356] The surface gloss value of the molded article of the present embodiment is high. The surface gloss value of the molded article of the present embodiment is preferably 50 or more, more preferably 70 or more, and further preferably 80 or more. When the surface gloss value of the molded article is greater than the above lower limit, the obtained molded article can be appropriately used as various parts such as automobile parts, electrical and electronic parts, industrial material parts, industrial material parts, and daily necessities and household products.
[0357] The molded product of the present embodiment is obtained by the above-mentioned polyamide resin composition, so the mechanical properties, especially the water absorption rigidity, thermal rigidity, fluidity, surface appearance and corrosion resistance are excellent. Therefore, the molded product can be suitable for various parts such as automobile parts, electrical and electronic parts, household appliance parts, OA (office automation) equipment parts, portable device parts, industrial equipment parts, daily necessities and household goods, and can be suitable for extrusion purposes, etc. Among them, the molded product is suitable for use as automobile parts, electrical and electronic parts, household appliance parts, OA equipment parts or portable device parts.
[0358] The automobile parts are not particularly limited, and examples thereof include intake system parts, cooling system parts, fuel system parts, interior parts, exterior parts, and electrical parts.
[0359] Example
[0360] Hereinafter, the present invention will be described in detail with reference to specific examples and comparative examples, but the present invention is not limited to the following examples.
[0361] Each constituent component of the polyamide resin composition used in Examples and Comparative Examples will be described.
[0362] <Composition>
[0363] [Aliphatic polyamide (Aa)]
[0364] Aa-1: Polyamide 6 (manufactured by Ube Industries, Ltd., trade name: "SF1013A", Mw (A-a) :31500,Mw (A-a) / Mn (A-a) :2.2)
[0365] Aa-2: Polyamide 66 (synthesized by the method described below)
[0366] [Semi-aromatic polyamide (Ab)]
[0367] Ab-1: Polyamide 6I (synthesized by the method described below)
[0368] Ab-2: Polyamide 6I / 6T (manufactured by EMS, trade name: "G21", Mw (A-b) :27000,Mw (A-b) / Mn (A-b) :2.4)
[0369] Ab-3: polyamide MXD6 (manufactured by Toyobo Co., Ltd., Toyobo Nylon, trade name "T-600", Mw (A-b) :45000,Mw (A-b) / Mw (A-b) :2.2)
[0370] [Metal salt of fatty acid (B)]
[0371] B-1: Sodium montanate (manufactured by Clariant, trade name: "LICOMONT NAV101")
[0372] B-2: Calcium montanate (manufactured by Clariant, trade name: "LICOMONT CAV102")
[0373] B-3: Calcium stearate (manufactured by NOF Corporation, trade name: "Calcium Stearate G")
[0374] [Fatty acid amide compound (C)]
[0375] C-1: N,N'-ethylenebisstearamide (manufactured by Kao Corporation, trade name: "KAO WAX EB-P")
[0376] C-2: N-stearyl erucamide (manufactured by Nippon Seika Co., Ltd., trade name: "SNT-P")
[0377] [Inorganic filler (D)]
[0378] D-1: Glass fiber (GF) (manufactured by Nippon Electric Glass Co., Ltd., trade name: "ECS03T275H", number average fiber diameter 10 μm, cut length (weight average fiber length) 3 mm)
[0379] [(E) Nigrosine]
[0380] E-1: Aniline black (manufactured by Orient Chemical Co., Ltd., TH807) (chloride ion concentration: 0.06 mass %)
[0381] E-2: Nigrosine (manufactured by Orient Chemical Co., Ltd., TH870) (chloride ion concentration: 1.6 mass %)
[0382] [(F) Other ingredients]
[0383] F-1: Carbon black (CB) (manufactured by Mitsubishi Chemical Corporation, trade name: "#45")
[0384] <Manufacturing of polyamide>
[0385] Hereinafter, each method for producing aliphatic polyamide (Aa-2) and semi-aromatic polyamide (Ab-1) will be described in detail. It should be noted that aliphatic polyamide (Aa-2) and semi-aromatic polyamide (Ab-1) obtained by the following production method were dried in a nitrogen gas stream to adjust the water content to about 0.2% by mass, and then used as a raw material for the polyamide resin composition in the examples and comparative examples described below.
[0386] [Synthesis of Aliphatic Polyamide (Aa-2) (Polyamide 66)]
[0387] The polymerization reaction of polyamide was carried out by the "hot melt polymerization method" as follows.
[0388] 1500g of equimolar salt of adipic acid and hexamethylenediamine was dissolved in 1500g of distilled water to prepare an equimolar 50% uniform aqueous solution of the raw monomer. The aqueous solution was put into an autoclave with an internal volume of 5.4L and replaced with nitrogen. While stirring at a temperature of 110°C or more and 150°C or less, water vapor was slowly extracted and concentrated to a solution concentration of 70% by mass. Then, the internal temperature was raised to 220°C. At this time, the autoclave was pressurized to 1.8MPa. In this state, it was maintained for 1 hour until the internal temperature reached 245°C, and the pressure was maintained at 1.8MPa while slowly extracting water vapor and reacting for 1 hour. Then, the pressure was reduced for 1 hour. Then, the autoclave was maintained at a reduced pressure of 650 Torr (86.66kPa) for 10 minutes using a vacuum device. At this time, the final internal temperature of the polymerization was 265°C.
[0389] Then, the product was pressurized with nitrogen and made into a strand from the lower spinneret (nozzle), water-cooled, cut, discharged in a pellet form, and dried at 100°C in a nitrogen atmosphere for 12 hours to obtain a crystalline aliphatic polyamide (Aa-2) (polyamide 66).
[0390] The Mw of the obtained crystalline aliphatic polyamide (Aa-2) (polyamide 66) is (A-a) 35000, Mw (A-a) / Mn (A-a) is 2.0.
[0391] [Synthesis of semi-aromatic polyamide (Ab-1) (polyamide 6I)]
[0392] The polymerization reaction of polyamide was carried out by the "hot melt polymerization method" as follows.
[0393] First, 1500g of an equimolar salt of isophthalic acid and hexamethylenediamine and 1.5 mol% of adipic acid and 0.5 mol% of acetic acid in excess of all equimolar salt components were dissolved in 1500g of distilled water to prepare a uniform aqueous solution of 50% by mass of the raw monomers. Then, while stirring at a temperature of 110°C or more and 150°C or less, water vapor was slowly extracted and concentrated to a solution concentration of 70% by mass. Then, the internal temperature was raised to 220°C. At this time, the autoclave was pressurized to 1.8MPa. In this state, it was maintained for 1 hour until the internal temperature reached 245°C, and the pressure was maintained at 1.8MPa while slowly extracting water vapor and reacting for 1 hour. Then, the pressure was reduced for 30 minutes. Then, the autoclave was maintained at a reduced pressure of 650 Torr (86.66kPa) for 10 minutes using a vacuum device. At this time, the final internal temperature of the polymerization was 265°C.
[0394] Next, the pellets were dried at 100° C. in a nitrogen atmosphere for 12 hours to obtain a semi-aromatic polyamide (Ab-1) (polyamide 6I).
[0395] The content of the isophthalic acid unit in the dicarboxylic acid unit of the obtained semi-aromatic polyamide (Ab-1) (polyamide 6I) was 100 mol%. Mw (A-b) 20000, Mw (A-b) / Mn (A-b) is 2.0.
[0396] <Measurement and evaluation methods of physical properties>
[0397] The pellets of the polyamide resin compositions obtained in the examples and comparative examples were dried in a nitrogen stream to adjust the water content in the polyamide resin compositions to 500 mass ppm or less. Then, various physical properties were measured and evaluated using the pellets of each polyamide resin composition after adjusting the water content by the following methods.
[0398] [Molecular weight (Mw) and molecular weight distribution (Mw / Mn) of polyamide resin composition]
[0399] The weight average molecular weight Mw and number average molecular weight Mn of each polyamide resin composition were measured by GPC (manufactured by Tosoh Corporation, HLC-8020, hexafluoroisopropanol solvent, PMMA (polymethyl methacrylate) standard sample (manufactured by Polymer Laboratories) conversion). Then, the molecular weight distribution (Mw / Mn) was calculated using the obtained Mw and Mn. It should be noted that TSK-GEL GMHHR-M and G1000HHR were used as GPC columns.
[0400] [Measurement of Dispersibility (Shape Parameter k) of Metal Ions of Fatty Acid Metal Salt (B)]
[0401] For each polyamide resin composition, a flat sheet (6 cm×9 cm×3 mm thick) was produced using an injection molding machine (NEX50III-5EG, manufactured by Nissei Plastic Industry Co., Ltd.). The cooling time was set to 25 seconds, the screw speed was set to 200 rpm, the mold temperature was set to 90° C., the barrel temperature was set to 280° C., and the injection pressure and injection speed were appropriately adjusted so that the filling time was within the range of 1.6 seconds ± 0.1 seconds.
[0402] Use TOF-SIMS to observe and measure the surface at any position of the molded sheet under the following observation conditions, thus obtain the intensity information image of the metal ion image. The spatial area of each metal ion is calculated by the intensity information image of the obtained metal ion image. About calculation, in the intensity information image, the plotting points of the metal ion are more than 200 and the mode of less than 2000 is selected from the metal ion with high intensity, in order to obtain the spatial area of each metal ion, the center of each metal ion is taken as the mother point and Voronoi segmentation is carried out. It should be noted that the polygon exposed to the outside is removed.
[0403] The spatial area of each region obtained by Voronoi segmentation is classified by area, and then a histogram is prepared. From the distribution state of the obtained histogram, a shape parameter k of the gamma distribution represented by the following equation is calculated.
[0404]
[0405] (where k: shape parameter, θ: scale parameter, x: spatial area)
[0406] (Observation conditions)
[0407] Equipment used: nanoTOF (manufactured by ULVAC-PHI)
[0408] Primary ion: Bi3++
[0409] Accelerating voltage: 30 kV
[0410] Ion current: 0.1nA (DC)
[0411] Analysis area: 600μm×600μm
[0412] Analysis time: 15 minutes
[0413] Detection ion: positive ion
[0414] Neutralization: Electron Gun
[0415] Oxygen introduction: Yes, 5.0×10 -5 Pa
[0416] [Chloride ion content]
[0417] The chloride ions (Cl ) contained in the pellets of the polyamide resin composition were analyzed by combustion ion chromatography. - ) content was quantified. Specifically, the sample was prepared by a combustion tube combustion method using ultrapure water (hydrogen peroxide, containing hydrazine hydrate) as an absorbent using an automatic sample combustion device AQF-2100H manufactured by Mitsubishi Chemical Analytical Technology Co., Ltd. An Integrion RFIC manufactured by Thermo Fisher Scientific was used as an ion chromatography (IC) device, an IonPac AS18-4μm (4mmφ×150mm) manufactured by Thermo Fisher Scientific was used as a column, a KOH aqueous solution was used as an eluent, and a UV detector was used as a detector.
[0418] The chloride ion (Cl - ) content.
[0419] “Cl - Content (ppm by mass)"
[0420] =[(IC measurement value (mg / L))×(dilution rate)-(blank IC measurement value (mg / L))]×[(absorption liquid volume (mL)) / 1000]×[1000000 / (mass of sample (mg))]
[0421] [Retention rate of flexural modulus after water absorption]
[0422] For each polyamide resin composition, an ISO dumbbell with a thickness of 4 mm was prepared and used as a test piece. Using the obtained test piece, the bending modulus before water absorption was measured according to ISO178. Next, the ISO dumbbell was placed in a constant temperature and humidity atmosphere (temperature: 23°C, relative humidity: 50%), and after reaching water absorption equilibrium, the bending modulus after water absorption was measured according to ISO178. The bending modulus retention rate (%) after water absorption was calculated using the following formula.
[0423] "Flexural modulus retention rate after water absorption (%)" = (flexural modulus after water absorption) / (flexural modulus before water absorption) × 100
[0424] The case where the flexural modulus retention rate after water absorption was 90% or more was evaluated as A (excellent), the case where the flexural modulus retention rate after water absorption was greater than or equal to 80% and less than 90% was evaluated as B (good), the case where the flexural modulus retention rate after water absorption was greater than or equal to 70% and less than 80% was evaluated as C (acceptable), and the case where the flexural modulus retention rate after water absorption was less than 70% was evaluated as D (poor), thereby evaluating the rigidity during water absorption.
[0425] [Low speed appearance]
[0426] For each polyamide resin composition, a flat molded sheet (6 cm×9 cm×3 mm thick) was produced using an injection molding machine (NEX50III-5EG, manufactured by Nissei Plastic Industry Co., Ltd.). The cooling time was set to 25 seconds, the screw speed was set to 200 rpm, the mold temperature was set to 90° C., the barrel temperature was set to 280° C., and the injection pressure and injection speed were appropriately adjusted so that the filling time was within the range of 4.5 seconds±0.1 seconds.
[0427] The surface appearance of the flat molded sheet produced in this manner was evaluated according to the following criteria.
[0428] (Evaluation Criteria)
[0429] A (good): Glass fibers are not visible on the flat molded piece.
[0430] B (acceptable): Glass fibers were seen in a part of the flat molded piece.
[0431] C (poor): Glass fibers were seen throughout the entire flat molded sheet.
[0432] [Surface gloss]
[0433] For each polyamide resin composition, a flat molded sheet (6 cm×9 cm×3 mm thick) was produced using an injection molding machine (NEX50III-5EG, manufactured by Nissei Plastic Industry Co., Ltd.). The cooling time was set to 25 seconds, the screw speed was set to 200 rpm, the mold temperature was set to 90° C., the barrel temperature was set to 280° C., and the injection pressure and injection speed were appropriately adjusted so that the filling time was within the range of 1.6 seconds ± 0.1 seconds.
[0434] The 60-degree glossiness of the center portion of the main surface of the flat molded sheet produced in this manner was measured using a gloss meter (IG320 manufactured by HORIBA) in accordance with JIS-K7150. The larger the measured value, the better the surface appearance.
[0435] [Demolding time]
[0436] For each polyamide resin composition, a flat molded sheet (6 cm × 9 cm × thickness 3 mm) was manufactured using an injection molding machine (NEX50III-5EG, manufactured by Nissei Resin Industry Co., Ltd.). The injection time was set to 15 seconds, the screw speed was set to 200 rpm, the mold temperature was set to 90°C, and the barrel temperature was set to 280°C. The injection pressure and injection speed were appropriately adjusted so that the filling time was within the range of 1.6 seconds ± 0.1 seconds. At this time, the shortest cooling time for the molded sheet to fall naturally (automatically) from the mold 10 times in a row was taken as the demolding time (seconds). The shorter the demolding time, the better the demolding property is judged to be.
[0437] [Exudation test]
[0438] For each polyamide resin composition, a flat molded sheet (6 cm×9 cm×3 mm thick) was produced using an injection molding machine (NEX50III-5EG, manufactured by Nissei Plastic Industry Co., Ltd.). The cooling time was set to 25 seconds, the screw speed was set to 200 rpm, the mold temperature was set to 90° C., the barrel temperature was set to 280° C., and the injection pressure and injection speed were appropriately adjusted so that the filling time was within the range of 1.6 seconds ± 0.1 seconds.
[0439] The flat sheet thus prepared was placed in a constant temperature and humidity chamber (temperature: 80°C, relative humidity: 95%) for 500 hours. The flat sheet was taken out, the oozing out on the surface was observed, and the difficulty of oozing out (oozing out resistance) was evaluated according to the following criteria.
[0440] (Evaluation Criteria)
[0441] A (good): No oozing out is observed on the flat molded piece.
[0442] B (acceptable): Bleeding was seen on a part of the flat molded piece.
[0443] C (poor): Bleeding was observed on the entire flat molded sheet.
[0444] [Laser printability]
[0445] For each polyamide resin composition, a flat molded sheet (6 cm×9 cm×3 mm thick) was produced using an injection molding machine (NEX50III-5EG, manufactured by Nissei Plastic Industry Co., Ltd.). The cooling time was set to 25 seconds, the screw speed was set to 200 rpm, the mold temperature was set to 90° C., the barrel temperature was set to 280° C., and the injection pressure and injection speed were appropriately adjusted so that the filling time was within the range of 1.6 seconds ± 0.1 seconds.
[0446] A laser marking machine manufactured by Keyence Corporation, trade name "MD-V9920", was used to mark the surface of the molded sheet with a square of 3 mm × 3 mm by laser marking, thereby obtaining a molded product. The laser marking conditions were set to a wavelength of 1064 nm, a scanning speed of 2000 mm / sec, an output power of 5.2 W or 9.1 W, a processing frequency of 20 kHz, and a processing pitch of 50 μm.
[0447] The visual evaluation criteria for laser printability are as follows.
[0448] (Evaluation Criteria)
[0449] A (good): The contrast between the laser-marked portion and the non-laser-marked portion is very clear, and there is no deformation of the characters.
[0450] B (acceptable): The contrast between the laser-marked portion and the non-laser-marked portion is clear, and some characters are deformed.
[0451] C (poor): The contrast between the laser-marked portion and the non-laser-marked portion is unclear, and the characters are deformed as a whole.
[0452] [Examples 1 to 12 and Comparative Examples 1 to 9]
[0453] A TEM58SX twin-screw extruder manufactured by Toshiba Machine Co., Ltd. (set temperature: 280°C, discharge volume 400 kg / hour, screw speed 300 rpm, resin temperature 300°C to 340°C) was used to supply a blend obtained by pre-blending components (A) to (C) and (F) from the top feed port set at the upstreammost part of the extruder, and component (D) was supplied from the side feed port on the downstream side of the extruder (the resin supplied from the top feed port was fully molten). The molten kneaded product extruded from the die was cooled in the form of strands and granulated to obtain polyamide resin composition pellets. The blending amount of each polyamide resin composition is shown in Tables 1 and 2.
[0454] Tables 1 to 3 show the measurement and evaluation results of various physical properties.
[0455] [Comparative Example 10]
[0456] A ZSK-26Mc twin-screw extruder manufactured by Coperion (set temperature: 280°C, discharge volume 25kg / hour, screw speed 300rpm, outlet resin temperature 280°C) was used, and a blend obtained by pre-blending components (A) to (C) and (F) was supplied from the top feed port set at the uppermost upstream portion of the extruder, and component (D) was supplied from the side feed port on the downstream side of the extruder (the resin supplied from the top feed port was fully molten). The molten kneaded product extruded from the die was cooled in the form of strands and granulated to obtain polyamide resin composition pellets. The amount of the polyamide resin composition is shown in Table 2.
[0457] Table 2 shows the measurement and evaluation results of various physical properties.
[0458] [Examples 13, 14 and Comparative Examples 11, 12]
[0459] A TEM58SX twin-screw extruder manufactured by Toshiba Machine Co., Ltd. (set temperature: 280°C, discharge volume 400 kg / hour, screw speed 300 rpm, resin temperature 300°C to 340°C) was used to supply a blend obtained by pre-blending components (A) to (C), component (E) and component (F) from the top feed port set at the upstreammost part of the extruder, and component (D) was supplied from the side feed port on the downstream side of the extruder (the resin supplied from the top feed port was fully molten). The molten kneaded product extruded from the die was cooled in the form of strands and granulated to obtain polyamide resin composition pellets. The blending amount of each polyamide resin composition is shown in Table 3.
[0460] Table 3 shows the measurement and evaluation results of various physical properties.
[0461]
[0462]
[0463] [Table 3]
[0464]
[0465] As shown in Table 1, the molded articles obtained from the polyamide resin compositions of Examples 1 to 12, which contain the components (A) and (B) and have a shape parameter k of 1.0 or more, have mold release properties suitable for high-cycle molding, and are excellent in rigidity, surface appearance, and anti-bleeding when the molded articles are water-absorbed. In addition, the laser printability is also excellent.
[0466] In comparison between Example 1 and Example 2, which differ in the presence or absence of the component (D), a tendency was observed that the mold release property and the anti-bleeding property were more excellent by blending the component (D).
[0467] In addition, in Examples 2, 6 and 7 where the carbon atom number ratio Bn / Cn is the same but the mass ratio Bw / Cw is different, a tendency is observed that the mold releasability is better as the mass ratio Bw / Cw increases, and a tendency is observed that the surface appearance is better as the mass ratio Bw / Cw decreases.
[0468] In Examples 2, 3 and 4 in which the ratio of the component (Ab) in the component (A) was different, the higher the ratio of the component (Ab), the better the rigidity and surface appearance during water absorption. On the other hand, when the ratio of the component (Ab) in the component (A) was small, the mold release property was better.
[0469] In comparison of Examples 2 and 12 in which the types of component (C) and carbon atom ratios Bn / Cn differ, a tendency is observed that the mold release properties and surface appearance are improved as the fatty acid amide compound (C-1) is added and the carbon atom ratio Bn / Cn increases.
[0470] In comparison between Examples 2 and 10 in which the types of the component (Aa) are different, a tendency is observed that the surface appearance is more excellent by blending the aliphatic polyamide (Aa-1) (PA6).
[0471] The molded article obtained from the polyamide resin composition of Comparative Example 4 not containing the component (B) had good rigidity and surface appearance when absorbing water, but poor releasability.
[0472] In addition, the shape parameter k of the molded article using the polyamide resin composition of Comparative Example 10 in which the extrusion conditions were changed was lower than that of the Examples, and the rigidity and surface appearance when absorbing water were good, but the mold releasability was poor.
[0473] As can be seen from Table 3, the polyamide resin compositions of Examples 13 and 14 containing the component (E) have higher shape parameters k than those of Example 2, and tend to have better releasability and surface appearance.
[0474] In addition, although the (E) component was contained, Comparative Examples 11 and 12, which had a high chloride ion content, had a shape parameter k lower than that of the examples and poor releasability. In addition, the laser printability was inferior to that of Examples 13 and 14.
[0475] Industrial Applicability
[0476] The polyamide resin composition of the present invention has excellent rigidity, surface appearance, and anti-bleeding property when it is made into a molded article, and is suitable for high-cycle molding. In addition, the molded article obtained by molding the polyamide resin composition of the present invention has excellent rigidity, surface appearance, and anti-bleeding property when it is water-absorbed. Therefore, the molded article of the present invention can be suitably used as various parts such as automobile parts, electrical and electronic parts, industrial material parts, industrial material parts, and daily necessities and household products.
Claims
1. A polyamide resin composition, characterized in that The polyamide resin composition comprises a polyamide resin (A) and a fatty acid metal salt (B) of a metal including an alkali metal and / or an alkaline earth metal, The polyamide resin composition contains 0.05 parts by mass or more and 5.00 parts by mass or less of the fatty acid metal salt (B) relative to 100 parts by mass of the polyamide resin (A), In the area distribution related to the spatial area per metal ion of the fatty acid metal salt (B) calculated by subjecting the surface of the polyamide resin composition to the following measurement, a shape parameter k of the gamma distribution is 1.0 or more, [Measurement] In order to calculate the spatial area of each metal ion on the surface of the polyamide resin composition in a distribution image or an intensity information image of a metal ion image obtained by mapping the metal ions of the fatty acid metal salt (B), Voronoi segmentation is performed with the center of the metal ion as a parent point, and the spatial area of each region obtained by the Voronoi segmentation is calculated, and each spatial area is classified, and a shape parameter k is calculated according to the gamma distribution represented by the following formula: Where k: shape parameter, θ: scale parameter, x: spatial area.
2. The polyamide resin composition according to claim 1, wherein The fatty acid metal salt (B) is a fatty acid metal salt having a terminal hydrocarbon group with 19 or more carbon atoms.
3. The polyamide resin composition according to claim 1 or 2, wherein The polyamide resin (A) is an aliphatic polyamide (Aa), a semi-aromatic polyamide (Ab) containing a diamine unit and a dicarboxylic acid unit, or a mixture of an aliphatic polyamide (Aa) and a semi-aromatic polyamide (Ab).
4. The polyamide resin composition according to claim 3, wherein When the polyamide resin (A) is set to 100 parts by mass, the polyamide resin composition contains: 50 parts by mass or more and 99 parts by mass or less of the aliphatic polyamide (Aa), 1 part by mass or more and 50 parts by mass or less of the semi-aromatic polyamide (Ab), 0.05 parts by mass or more and 5.00 parts by mass or less of the fatty acid metal salt (B), and 0.01 parts by mass or more and 3.00 parts by mass or less of the fatty acid amide compound (C).
5. The polyamide resin composition according to claim 4, wherein The ratio Bw / Cw of the mass Bw of the fatty acid metal salt (B) to the mass Cw of the fatty acid amide compound (C) is 0.6 or more and 4.0 or less.
6. The polyamide resin composition according to claim 4, wherein The ratio Bn / Cn of the number of carbon atoms Bn of the terminal hydrocarbon group of the fatty acid metal salt (B) to the number of carbon atoms Cn of the terminal hydrocarbon group of the fatty acid amide compound (C) is greater than 1.00 and less than or equal to 2.
00.
7. The polyamide resin composition according to claim 3, wherein The aliphatic polyamide (Aa) is polyamide 6 or polyamide 66.
8. The polyamide resin composition according to claim 3, wherein The semi-aromatic polyamide (Ab) contains 50 mol % or more of isophthalic acid units based on all dicarboxylic acid units constituting the semi-aromatic polyamide (Ab), and contains a diamine unit having 4 to 10 carbon atoms as the diamine unit.
9. The polyamide resin composition according to claim 3, wherein The semi-aromatic polyamide (Ab) contains 75 mol % or more of isophthalic acid units based on all dicarboxylic acid units constituting the semi-aromatic polyamide (Ab), and contains a diamine unit having 4 to 10 carbon atoms as the diamine unit.
10. The polyamide resin composition according to claim 1 or 2, wherein The weight average molecular weight Mw of the polyamide resin (A) is 10,000 or more and 50,000 or less.
11. The polyamide resin composition according to claim 1 or 2, wherein The molecular weight distribution Mw / Mn of the polyamide resin (A) is 2.4 or less.
12. The polyamide resin composition according to claim 1 or 2, wherein The fatty acid metal salt (B) is at least one selected from the group consisting of sodium montanate and calcium montanate.
13. The polyamide resin composition according to claim 4, wherein The fatty acid amide compound (C) is one or more selected from the group consisting of fatty acid amide compounds having a hydrocarbon group having 9 to 30 carbon atoms and fatty acid bisamide compounds having a hydrocarbon group having 9 to 30 carbon atoms.
14. The polyamide resin composition according to claim 4, wherein The fatty acid amide compound (C) is at least one selected from the group consisting of N,N′-ethylenebisstearylamide and N-stearyl erucamide.
15. The polyamide resin composition according to claim 1 or 2, wherein The polyamide resin composition further contains an inorganic filler (D), The content of the inorganic filler (D) is 5 parts by mass or more and 200 parts by mass or less relative to 100 parts by mass of the polyamide resin (A).
16. The polyamide resin composition according to claim 1 or 2, wherein The polyamide resin composition further contains aniline black (E), The content of the aniline black (E) is greater than 0 parts by mass and less than or equal to 0.5 parts by mass relative to 100 parts by mass of the polyamide resin (A).
17. The polyamide resin composition according to claim 1 or 2, wherein The content of chloride ions is 5 ppm or less on a mass basis.
18. A molded article, characterized in that: The molded article comprises the polyamide resin composition according to claim 1 or 2.
19. A production method, which is the production method of the polyamide resin composition according to claim 1 or 2, characterized in that: The production method includes the step of melt-kneading the polyamide resin (A) and the fatty acid metal salt (B).