Toughened polyamide composite material as well as preparation method and application thereof
By using high-temperature melt-kneading of fluoridazoline quaternary ammonium salt and polyamide resin in polyamide materials, a cross-linking network structure is formed, which solves the problem of insufficient impact resistance of polyamide materials under low temperature conditions and improves the material Low temperature toughness and impact resistance.
Patent Information
- Application Number
- CN202411142145.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-20
- Publication Date
- 2024-11-22
AI Technical Summary
The prior art is difficult to toughen and enhance polyamide materials at the same time, and the materials are prone to become brittle under low temperature conditions, and have insufficient resistance to low temperature embrittlement and toughening properties.
The fluorinated imidazoline quaternary ammonium salt and polyamide resin are used for high-temperature melt-kneading to form a crosslinking network structure, reducing the water absorption of the material and improving the low-temperature impact resistance.
The low-temperature impact resistance and uniform toughness of polyamide composite materials are improved, reducing the possibility of the material becoming brittle under low temperature conditions, and meeting the application needs in high-altitude environments.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention belongs to the field of polymer materials and relates to a toughened polyamide composite material and a preparation method and application thereof. Background Art
[0002] Polyamide, commonly known as nylon, is a general term for a class of polymers containing amide groups (-CONH-) in the repeating units on the main chain of the molecule. Polyamide can be obtained by ring-opening polymerization of lactam or by condensation polymerization of diamine and dibasic acid. Polyamide materials have developed rapidly due to their excellent performance and wide application. So far, polyamide has become the most used variety among the five major engineering plastics. Whether in the basic research of polyamide or its application development, polyamide materials have always occupied an important position in the large family of polymer materials.
[0003] Toughening and strengthening of polymers have always been a hot area in polymer research. By toughening and strengthening polyamide materials, a series of polyamides with better performance can be obtained, which continuously expands its application areas. At the same time, compared with synthesizing new high-performance polymers, toughening and strengthening traditional materials is a relatively low-cost and direct method. There are three main methods for toughening and strengthening polyamides: 1. Add small molecules to polyamide to toughen and strengthen it through physical and mechanical methods. Chinese patent No. CN106221204 discloses a method for preparing glass fiber reinforced polyamide. Through a unique formula design and a two-step extrusion process, a glass fiber reinforced polyamide blend with low melting point, good rigidity and toughness balance and good dimensional stability is prepared. It can be widely used in the fields of automobiles, engineering structural parts, and electronic and electrical products with high rigidity and toughness balance, wear resistance and dimensional stability.
[0004] 2. Blending different polymers with polyamide to toughen and strengthen the polyamide. Chinese patent No. CN101235196 discloses a toughening agent for polyamide and toughened polyamide, wherein the toughening agent is prepared by the following method: pre-irradiated or peroxide-added polyolefin is mixed with functionalized low-molecular polybutadiene, and the mixture is put into an extruder for grafting reaction of polyolefin to obtain a modified polyolefin toughening agent, which is then dispersed in polyamide by extrusion blending. The core-shell structure formed by the toughening agent can maintain the rigidity and toughness balance of the polyamide system, and the functional groups in the toughening agent can form a good interface bond with the polyamide. Chinese patent publication number CN1480489 discloses a method for preparing a toughened polyamide blend obtained by blending polyamide and mixed rubber components. The morphology and particle size distribution of the rubber phase contained in the toughened polyamide composition can be controlled by changing the particle size of the powdered rubber with a cross-linked structure mixed in and selecting an appropriate unvulcanized rubber or thermoplastic elastomer. The toughened polyamide composition has good toughness and processing performance, while maintaining good strength and rigidity.
[0005] 3. Copolymerization with polyamide by chemical methods to toughen and strengthen polyamide. The patent with publication number CN109705342A uses monofunctional isocyanate end-capping to reduce the content of terminal carboxyl and terminal amino groups in polyamide resin. However, since isocyanate is prone to self-polymerization to form dimers or high molecular weight polymers, it is easy to introduce impurities into polyamide resin, thereby affecting the mechanical properties of polyamide.
[0006] In summary, the current methods for toughening and strengthening polyamides are mainly concentrated on the above three methods. However, these three methods all have some shortcomings: for example, these methods are difficult to achieve the purpose of both toughening and strengthening the material at the same time, often at the expense of one of the properties. In addition, the key factor that determines the performance of polymer composites is the compatibility issue. The method of adding small molecule fillers or second polymers often faces poor interactions between fillers or second polymers and matrix polymers, resulting in agglomeration or phase separation in the matrix.
[0007] At present, the development of polyamide resins with good resistance to low-temperature embrittlement and toughening properties is still a problem to be solved urgently in the existing technical field. Summary of the invention
[0008] In order to solve the deficiencies of the prior art and products, the present invention provides a toughened polyamide composite material and a preparation method and application thereof.
[0009] A toughened polyamide composite material contains at least polyamide resin and fluorine-containing imidazoline quaternary ammonium salt; the production raw materials of the polyamide resin include at least hexamethylenediamine and dibasic acid; the mass ratio of the polyamide resin to the fluorine-containing imidazoline quaternary ammonium salt is 100:(10-30).
[0010] In some embodiments of the present invention, the polyamide resin is any one of polyamide resin PA66 and polyamide resin PA610.
[0011] In some embodiments of the present invention, the preparation process of the fluorine-containing imidazoline quaternary ammonium salt comprises the following steps: S1: Add diethylenetriamine and fluorinated alkyl acid in a molar ratio of 1:(1-1.2) into a reaction vessel, then add a water-carrying agent and a catalyst, and heat to reflux for dehydration reaction for 8-10 hours; S2: removing the water-carrying agent and water from the reaction system in S1 by vacuum distillation, adding benzyl chloride thereto, reacting at 100-110° C. for 5-7 hours, and recrystallizing the obtained reaction system with a mixed solution of acetone and toluene to obtain the fluorine-containing imidazoline quaternary ammonium salt.
[0012] Furthermore, the fluorinated alkyl acid in S1 is at least one of 2H,2H,3H,3H-perfluorodecanoic acid, 2H,2H,3H,3H-perfluorononanoic acid, 2H,2H,3H,3H-perfluorooctanoic acid, 2H,2H,3H,3H-perfluoroheptanoic acid, 4,4,5,5,6,6-hexafluorohexanoic acid, 4-fluorocyclohexylcarboxylic acid, and 4,4-difluorocyclohexylcarboxylic acid.
[0013] Because the fluorine-containing imidazoline quaternary ammonium salt in the polyurethane resin not only reduces the water absorption of the material, but also controls the dehydration of the obtained material at low temperatures. Therefore, the fluorine-containing alkyl acid used to prepare the fluorine-containing imidazoline quaternary ammonium salt is preferably at least one of the above-mentioned compounds, otherwise it will affect the migration of the fluorine-containing imidazoline quaternary ammonium salt in the polyamide resin and the chemical combination with its terminal amino group, resulting in insufficient low-temperature impact resistance and uniform toughness of the obtained toughened polyamide composite material.
[0014] Furthermore, the water-carrying agent in S1 is any one of toluene and xylene, and its usage mass accounts for 20-30% of the total mass of the diethylenetriamine and the fluorinated alkyl acid.
[0015] Furthermore, the catalyst in S1 is any one of Lewis acid catalysts, specifically, aluminum oxide, zinc oxide, magnesium oxide, iron oxide, etc.
[0016] Furthermore, the temperature of the heating reflux in S1 is 120-150°C.
[0017] Furthermore, the molar amount of the benzyl chloride in S2 is 1-1.05 times the molar amount of the diethylenetriamine in S1.
[0018] The preparation method of the toughened polyamide composite material comprises the following steps: drying the polyamide resin in a vacuum environment, and melt-mixing the polyamide resin with the fluorine-containing imidazoline quaternary ammonium salt, wherein the melt-mixing temperature is 20-30°C higher than the melting point of the polyurethane resin, and the melt-mixing time is 0.5-5min, so that the fluorine-containing imidazoline quaternary ammonium salt can be infiltrated into the polyamide resin; after the mixing is completed, a strand is extruded from a nozzle, the strand is cooled in water, and cut into granules in a granulator to obtain the toughened polyamide composite material.
[0019] The melting and mixing temperature is set at a level 20-30°C higher than the melting point of the polyurethane resin, in view of the fact that under the action of high temperature, the terminal amino groups of some linear polyamide molecular chains will be dehydrogenated, and the adjacent terminal amino groups will react with each other to remove an amino group and generate a secondary amino group at the same time. The hydrogen atoms on the secondary amino group are relatively active and can react with the amino groups in the fluorinated imidazoline quaternary ammonium salt. The crosslinking points formed between the chains through the fluorinated imidazoline quaternary ammonium salt increase as the high temperature treatment time increases, thereby forming a three-dimensional crosslinked network structure. Moreover, at this temperature level, it can be ensured that the polyamide resin will not decompose even if it is bent and melted.
[0020] The present invention also provides the use of the toughened polyamide composite material in preparing molded parts.
[0021] Beneficial effects: Compared with the prior art, the present invention creatively melt-mixes the homemade fluorinated imidazoline quaternary ammonium salt and the polyamide resin at a certain high temperature, so that cross-linking is achieved between them through chemical reaction, which neither destroys the main molecular chain structure of the polyamide resin nor can utilize the special structure of the fluorinated imidazoline quaternary ammonium salt to moderately reduce the water absorption of the polyamide resin. At the same time, the low-temperature dehydration of the obtained toughened polyamide composite material is also alleviated, reducing the possibility of the material becoming brittle under low temperature conditions after expansion, thereby achieving excellent low-temperature impact resistance. DETAILED DESCRIPTION
[0022] The present invention will be described below in conjunction with specific embodiments. It should be noted that the following embodiments are examples of the present invention and are only used to illustrate the present invention, but not to limit the present invention. Other combinations and various modifications within the concept of the present invention may be performed without departing from the spirit or scope of the present invention.
[0023] The preparation of the fluorine-containing imidazoline quaternary ammonium salt used in the embodiment is exemplified below: Fluorinated imidazoline quaternary ammonium salt #1 S1: 103.2 g (1.0 mol) of diethylenetriamine and 442 g (1.0 mol) of 2H,2H,3H,3H-perfluorodecanoic acid were added to a reaction vessel, and then 109 g of toluene and 10.9 g of alumina were added, and the mixture was heated to 150°C to reflux for dehydration reaction for 8 hours; S2: The water-carrying agent and water in the reaction system in S1 are removed by vacuum distillation, 126.6 g (1.0 mol) of benzyl chloride is added thereto, and the reaction is carried out at 100° C. for 7 hours. The obtained reaction system is recrystallized with a mixed solution of acetone and toluene to obtain the fluorinated imidazoline quaternary ammonium salt #1.
[0024] Fluorinated imidazoline quaternary ammonium salt #2 S1: 103.2 g (1.0 mol) of diethylenetriamine and 266.2 g (1.1 mol) of 4,4,5,5,6,6-hexafluorohexanoic acid were added to a reaction vessel, followed by 92.35 g of xylene and 9.24 g of zinc oxide, and heated to 130°C to reflux for dehydration reaction for 9 hours; S2: The water-carrying agent and water in the reaction system in S1 are removed by vacuum distillation, 127.9 g (1.02 mol) of benzyl chloride is added thereto, and the reaction is carried out at 100° C. for 6 hours. The obtained reaction system is recrystallized with a mixed solution of acetone and toluene to obtain the fluorinated imidazoline quaternary ammonium salt #2.
[0025] Fluorinated imidazoline quaternary ammonium salt #3 S1: 103.2 g (1.0 mol) of diethylenetriamine and 175.4 g (1.2 mol) of 4-fluorocyclohexylcarboxylic acid were added to a reaction vessel, followed by 83.58 g of xylene and 8.36 g of magnesium oxide, and heated to 120°C to reflux for dehydration reaction for 10 h; S2: The water-carrying agent and water in the reaction system in S1 are removed by vacuum distillation, 132.9 g (1.05 mol) of benzyl chloride is added thereto, and the reaction is carried out at 110° C. for 5 hours. The obtained reaction system is recrystallized with a mixed solution of acetone and toluene to obtain the fluorinated imidazoline quaternary ammonium salt #3.
[0026] Fluorinated imidazoline quaternary ammonium salt #4 Similar to fluorinated imidazoline quaternary ammonium salt #1, except that the 2H,2H,3H,3H-perfluorodecanoic acid is replaced by nonadecafluorodecanoic acid.
[0027] Example 1 100 parts of polyamide resin PA66 (melting point 252° C.) are placed in a vacuum environment for drying, and melt-kneading with 10 parts of the fluorine-containing imidazoline quaternary ammonium salt #1. The melt-kneading temperature is 20° C. higher than the melting point of the polyurethane resin, and the melt-kneading time is 5 minutes, so that the fluorine-containing imidazoline quaternary ammonium salt #1 can penetrate into the polyamide resin. After the mixing is completed, a strand is extruded from a nozzle, the strand is cooled in water, and cut into pellets in a pelletizer to obtain the toughened polyamide composite material.
[0028] Example 2 100 parts of polyamide resin PA66 (melting point 252° C.) are placed in a vacuum environment for drying, and melt-kneading with 20 parts of the fluorine-containing imidazoline quaternary ammonium salt #2. The melt-kneading temperature is 25° C. higher than the melting point of the polyurethane resin, and the melt-kneading time is 3 minutes, so that the fluorine-containing imidazoline quaternary ammonium salt #2 can penetrate into the polyamide resin. After the mixing is completed, a strand is extruded from a nozzle, the strand is cooled in water, and cut into pellets in a pelletizer to obtain the toughened polyamide composite material.
[0029] Example 3 100 parts of polyamide resin PA610 (melting point 218° C.) are placed in a vacuum environment for drying, and melt-kneading with 30 parts of the fluorine-containing imidazoline quaternary ammonium salt #3. The melt-kneading temperature is 30° C. higher than the melting point of the polyurethane resin, and the melt-kneading time is 0.5 min, so that the fluorine-containing imidazoline quaternary ammonium salt #3 can penetrate into the polyamide resin. After the mixing is completed, a strand is extruded from a nozzle, the strand is cooled in water, and cut into pellets in a pelletizer to obtain the toughened polyamide composite material.
[0030] Example 4 Same as Example 1, except that the fluorine-containing imidazoline quaternary ammonium salt #1 is replaced by the fluorine-containing imidazoline quaternary ammonium salt #4.
[0031] Comparative Example 1 Same as Example 1, except that the amount of fluorine-containing imidazoline quaternary ammonium salt #1 is reduced to 8 parts.
[0032] Comparative Example 2 Same as Example 3, except that the amount of fluorine-containing imidazoline quaternary ammonium salt #3 is increased to 32 parts.
[0033] Comparative Example 3 Same as Example 3, except that the fluorine-containing imidazoline quaternary ammonium salt #3 is not added.
[0034] Performance Testing Low-temperature impact resistance: Place the sample in a GT-7005 high and low temperature alternating testing machine, freeze it at -30°C for 1 hour, take it out, and test its bending performance in accordance with GB / T9341-2008, and its impact performance in accordance with GB / T1043.1-2008.
[0035] The test results are detailed in Table 1:
[0036] It can be seen from the data in Table 1 that the flexural strength and impact strength of the polyamide composite materials obtained in Examples 1-4 decreased after low-temperature freezing, but the indicators after the decrease were better than the test results obtained in Comparative Examples 1-3. It can be seen that the homemade fluorinated imidazoline quaternary ammonium salt has a significant promoting effect on improving the toughness of polyamide resin at low temperatures.
[0037] In addition, although the impact strength of the polyamide composite material obtained in Example 4 is not much different from that of Example 1 at room temperature, after low-temperature treatment, its impact strength is significantly lower than that of Example 1. It can be inferred that the fluorine content in the fluorinated alkyl acid used will affect the water absorption of the polyamide. When the material is impacted by the outside world, the molecular chains cannot move or slip with each other through the intervention of water molecules, and cannot absorb the energy brought by the impact, and its impact resistance is also reduced.
[0038] The results of Comparative Examples 1-3 indicate that adding too much or too little of the fluorine-containing imidazoline quaternary ammonium salt is detrimental to the toughness and low-temperature impact resistance of the polyamide resin.
[0039] In summary, the fluorine-containing imidazoline quaternary ammonium salt is added to the polyamide resin to effectively absorb the impact load, so that the low-temperature toughness of the finally obtained polyamide composite material is good and can meet the requirements of the product being used in a high-cold environment.
Claims
1. A toughened polyamide composite material, characterized in that: It contains at least polyamide resin and fluorine-containing imidazoline quaternary ammonium salt; the production raw materials of the polyamide resin include at least hexamethylenediamine and dibasic acid; the mass ratio of the polyamide resin to the fluorine-containing imidazoline quaternary ammonium salt is 100: (10-30).
2. The toughened polyamide composite material according to claim 1, characterized in that: The polyamide resin is any one of polyamide resin PA66 and polyamide resin PA610.
3. The toughened polyamide composite material according to claim 1, characterized in that: The preparation process of the fluorine-containing imidazoline quaternary ammonium salt comprises the following steps: S1: Add diethylenetriamine and fluorinated alkyl acid in a molar ratio of 1:(1-1.2) into a reaction vessel, then add a water-carrying agent and a catalyst, and heat to reflux for dehydration reaction for 8-10 hours; S2: removing the water-carrying agent and water from the reaction system in S1 by vacuum distillation, adding benzyl chloride thereto, reacting at 100-110° C. for 5-7 hours, and recrystallizing the obtained reaction system with a mixed solution of acetone and toluene to obtain the fluorine-containing imidazoline quaternary ammonium salt.
4. The toughened polyamide composite material according to claim 3, characterized in that: The fluorinated alkyl acid in S1 is at least one of 2H,2H,3H,3H-perfluorodecanoic acid, 2H,2H,3H,3H-perfluorononanoic acid, 2H,2H,3H,3H-perfluorooctanoic acid, 2H,2H,3H,3H-perfluoroheptanoic acid, 4,4,5,5,6,6-hexafluorohexanoic acid, 4-fluorocyclohexylcarboxylic acid, and 4,4-difluorocyclohexylcarboxylic acid.
5. The toughened polyamide composite material according to claim 3, characterized in that: The water-carrying agent in S1 is any one of toluene and xylene, and its usage mass accounts for 20-30% of the total mass of the diethylenetriamine and the fluorinated alkyl acid.
6. The toughened polyamide composite material according to claim 3, characterized in that: The catalyst in S1 is any one of Lewis acid catalysts.
7. The toughened polyamide composite material according to claim 3, characterized in that: The heating reflux temperature in S1 is 120-150°C.
8. The toughened polyamide composite material according to claim 3, characterized in that: The molar amount of the benzyl chloride in S2 is 1-1.05 times the molar amount of the diethylenetriamine in S1.
9. The method for preparing the toughened polyamide composite material according to any one of claims 1 to 8, characterized in that: The method comprises the following steps: drying the polyamide resin in a vacuum environment, and melt-mixing the polyamide resin with the fluorine-containing imidazoline quaternary ammonium salt, wherein the melt-mixing temperature is 20-30° C. higher than the melting point of the polyurethane resin, and the melt-mixing time is 0.5-5 minutes, so that the fluorine-containing imidazoline quaternary ammonium salt can be infiltrated into the polyamide resin; After the mixing is completed, a strand is extruded from a nozzle, cooled in water, and cut into pellets in a pelletizer to obtain the toughened polyamide composite material.
10. Use of the toughened polyamide composite material according to any one of claims 1 to 8 in the preparation of molded parts.
Citation Information
Patent Citations
Long glass fiber reinforced bio-based polyamide 56, alloy and preparation method of long glass fiber reinforced bio-based polyamide 56
CN113429781A
Cited By
High-toughness biaxially oriented polyamide film and preparation method thereof
CN119749003A