Application of flame-retardant modified carbon fiber in flame-retardant reinforced polyamide
By modifying the random copolymer of the carbon fiber surface with focused piperazine phosphate-melamine polyphosphate, it forms flame retardant modified carbon fibers, and combines them with nylon and other materials, the problem of unsatisfactory flame retardant performance of carbon fiber reinforced polymer materials is solved, and the flame retardant performance of carbon fiber reinforced polymer materials is achieved. Improve the mechanical properties and antistatic properties, while reducing the use of flame retardant.
Patent Information
- Application Number
- CN202411372561.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-29
- Publication Date
- 2024-11-22
AI Technical Summary
In the prior art, the flame retardant performance of carbon fiber reinforced polymer materials is not ideal, and the addition of a large amount of flame retardant will affect the mechanical properties, resulting in a decrease in the gain effect.
Using flame retardant modified carbon fibers by weight, the random copolymer of piperazine phosphate-melamine polyphosphate random copolymer is prepared by random copolymer synthesis and amino modification methods, and the surface of the carbon fiber is modified to form flame retardant modification. Carbon fiber and combine it with nylon, melamine polyphosphate, organic aluminum hypophosphate and flame retardant synergist to form a flame retardant-reinforced polyamide composite material.
The mechanical properties, antistatic properties and flame retardant properties of the composite material are significantly improved, the amount of flame retardant is added is reduced, the negative impact on the mechanical properties is avoided, and the overall performance of the material is enhanced.
Smart Images

Figure CN118994899A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of flame-retardant polyamide materials, and in particular to application of flame-retardant modified carbon fiber in flame-retardant reinforced polyamide. Background Art
[0002] Nylon is an extremely important thermoplastic engineering plastic. Since the industrial production of DuPont in the United States in the 1950s, it has a development history of nearly 50 years and currently ranks first among engineering plastics. Although nylon itself is an engineering plastic with excellent performance, it has high hygroscopicity, poor dimensional stability of products, and its strength and hardness are far inferior to metals. In addition, in the chemical and coal industries, there are high requirements for the mechanical properties and antistatic properties of the material to meet the requirements of working pressure and antistatic during use and achieve safe production. In order to overcome these shortcomings, as early as the 1970s, people used carbon fiber or other types of fibers to enhance their performance. In recent years, the use of carbon fiber to reinforce nylon materials has developed rapidly, because nylon and carbon fiber are both materials with excellent performance in the field of engineering plastics. The composite of the two comprehensively reflects their respective advantages, with much higher strength and rigidity than unreinforced nylon, small creep, good dimensional accuracy, significantly improved thermal stability, wear resistance, and excellent damping. Carbon fiber has better performance than glass fiber reinforcement. For nylon / carbon fiber composite systems, most foreign countries currently use nylon 6 or nylon 66 as the matrix material, and short or long (continuous) carbon fiber as the reinforcement material. Carbon fiber reinforced PA6 composite materials combine the advantages of both, improve the shortcomings and deficiencies of raw materials, and focus on improving the mechanical properties and antistatic properties of the materials. They have broad application prospects in the fields of automobiles, ships, aerospace, transportation, etc.
[0003] In order to reduce the flammability of carbon fiber reinforced polymer materials, the current more widespread solution is to suppress the "wick effect" by adding sufficient high-quality flame retardants to polymer / CF composite materials. However, the addition of a large amount of flame retardants will seriously affect the mechanical properties of polymer materials, resulting in a reduction in the gain effect of carbon fiber in polymer materials. How to effectively increase the flame retardancy of carbon fiber reinforced polymer materials while ensuring the mechanical properties of the materials is an urgent problem to be solved in this field. Summary of the invention
[0004] The present invention aims to provide an application of flame-retardant modified carbon fiber in flame-retardant reinforced polyamide to solve the technical problem of unsatisfactory mechanical properties of flame-retardant carbon fiber reinforced polyamide materials in the prior art.
[0005] In order to achieve the above object, the present invention adopts the following technical scheme:
[0006] A flame retardant reinforced polyamide composite material, whose raw materials include, by weight: 30-80 parts of nylon, 5-60 parts of flame retardant modified carbon fiber, 5-20 parts of melamine polyphosphate, 5-20 parts of organic aluminum hypophosphite, 0.5-4 parts of flame retardant synergist, 0.3-2 parts of nucleating agent, 0.5-2 parts of coupling agent, 0.3-3 parts of lubricant and 0.2-1 parts of antioxidant.
[0007] Furthermore, the flame retardant modified carbon fiber is prepared by the following method:
[0008] S1 Synthesis of random copolymer: The melamine polyphosphate represented by formula (8) and the focused piperazine phosphate represented by formula (1) are subjected to thermal polymerization reaction to obtain a focused piperazine phosphate-melamine polyphosphate random copolymer represented by formula (10);
[0009]
[0010] Wherein, 500<m<10000, 500<n<10000, x>0, y>0, p>0; In formula (10), MPP represents formula (8), PAPP represents formula (1), and the mass ratio of PAPP to MPP is 1:0.2-5;
[0011] S2 Amination modification: Use amino coupling agents to modify the surface of carbon fiber to obtain amination carbon fiber;
[0012] S3 random copolymer modification: The surface of amino carbon fiber was modified using focused piperazine phosphate-melamine polyphosphate random copolymer to obtain flame retardant modified carbon fiber.
[0013] Further, in S1, the mass ratio of piperazine phosphate to melamine polyphosphate is 1:0.2-5; the conditions of the thermal polymerization reaction are: 200-280°C reaction temperature, 0.1-1.5MPa nitrogen atmosphere, and 30-180min reaction time;
[0014] Preferably, the mass ratio of piperazine phosphate to melamine polyphosphate is 1:0.8; the conditions of the thermal polymerization reaction are: 280° C. reaction temperature, 0.5 MPa nitrogen atmosphere, and 180 min reaction time.
[0015] Further, in S1, the focused piperazine phosphate is obtained by the following method: dipiperazine phosphate is heat-treated for 30-240 min under a nitrogen atmosphere, a pressure environment of 0.05-0.3 MPa, and a condition of 120-320° C. to thermally polymerize and dehydrate to form focused piperazine phosphate;
[0016] The melamine polyphosphate is obtained by the following method: melamine phosphate is heat-treated for 60-300 minutes under a nitrogen atmosphere, a pressure environment of 0.05-0.3 MPa, and a temperature of 220-360° C. to thermally polymerize and dehydrate and condense to obtain the melamine polyphosphate.
[0017] Further, in S2, the carbon fiber is dispersed in an ethanol solution, and then an amino coupling agent is added under stirring conditions of 200-1500 rpm, and the mixture is reacted at 60-100° C. for 4-8 hours to obtain amino carbon fiber.
[0018] Furthermore, in S2, the length of the carbon fiber is 2.5-7.5 mm; and the ratio of the carbon fiber to the ethanol solution is 100 g: 250-750 ml.
[0019] Further, in S3, the aminated carbon fiber is dispersed in a solvent, and then the focused piperazine phosphate-melamine polyphosphate random copolymer is added, and the reaction is carried out at 20-50° C. for 2-12 hours to obtain a flame retardant modified carbon fiber;
[0020] The solvent includes any one of ethanol, water, DMF, DMSO, acetonitrile and ethanol solution. The ratio of the amino carbon fiber, the focused piperazine phosphate-melamine polyphosphate random copolymer and the solvent is 80-160g: 0.1-5g: 200-1000mL.
[0021] Further, the nylon includes at least one of nylon 6, nylon 66, nylon 46, nylon 610, nylon 612, nylon 9, nylon 11, nylon 12, nylon 1010, nylon 1012 and nylon 1212;
[0022] The organic aluminum hypophosphite is aluminum diethylphosphinate; the nucleating agent is BRUGGOLEN P22;
[0023] The 1% thermal weight loss of the melamine polyphosphate is greater than or equal to 360° C., and the melamine polyphosphate is prepared by the following method: melamine phosphate is heat-treated for 60-300 minutes under a nitrogen atmosphere, a pressure environment of 0.05-0.3 MPa, and a temperature of 220-360° C. to thermally polymerize and dehydrate to condense into the melamine polyphosphate;
[0024] The flame retardant synergist includes at least one of anhydrous zinc borate, 3.5 hydrate zinc borate, zinc sulfide, zinc oxide, and zirconium phosphate;
[0025] The coupling agent includes at least one of KH-9120, KT-930, KH-1006 and KH-9130;
[0026] The lubricant comprises at least one of white oil, silicone oil, polyethylene wax, ethylene bis stearamide, pentaerythritol stearate, silicone and amide wax;
[0027] The antioxidant includes at least one of antioxidant 168 , antioxidant 1010 , and antioxidant 1098 .
[0028] The technical scheme also provides a method for preparing a flame-retardant reinforced polyamide composite material, which is characterized by: adding nylon, melamine polyphosphate, organic aluminum hypophosphite and a flame-retardant synergist into a mixer and stirring at room temperature for 5-30 minutes; raising the temperature of the mixer to 80-180°C, adding a coupling agent and continuing stirring for 10-30 minutes; after cooling to room temperature, adding a lubricant, a nucleating agent and an antioxidant, stirring for 5-30 minutes to obtain a premix; extruding the premix with a twin-screw extruder, adding CF-NH2-FR through side feeding, the temperature during extrusion is 200-300°C, and then obtaining a flame-retardant reinforced polyamide granular material through strip drawing, pelletizing, screening and dehydration.
[0029] The technical solution also provides an application of a flame retardant modified carbon fiber in a flame retardant reinforced polyamide, characterized in that: the flame retardant modified carbon fiber is prepared by the following method:
[0030] S1 Synthesis of random copolymer: The melamine polyphosphate represented by formula (8) and the focused piperazine phosphate represented by formula (1) are subjected to thermal polymerization reaction to obtain a focused piperazine phosphate-melamine polyphosphate random copolymer represented by formula (10);
[0031]
[0032] Wherein, 500<m<10000, 500<n<10000, x>0, y>0, p>0; In formula (10), MPP represents formula (8), PAPP represents formula (1), and the mass ratio of PAPP to MPP is 1:0.2-5;
[0033] S2 Amination modification: Use amino coupling agents to modify the surface of carbon fiber to obtain amination carbon fiber;
[0034] S3 random copolymer modification: The surface of amino carbon fiber was modified using focused piperazine phosphate-melamine polyphosphate random copolymer to obtain flame retardant modified carbon fiber.
[0035] The principle and beneficial effects of this technical solution are:
[0036] The present invention modifies the surface of carbon fiber, and coats the macromolecular intumescent flame retardant with excellent carbonization effect on the surface of carbon fiber, so that the polymer / carbon fiber composite material quickly forms an expanded, dense and hard carbon layer on the surface of carbon fiber at high temperature, thereby greatly suppressing the "candle wick effect". In addition, after the surface of carbon fiber is modified with a focused piperazine phosphate-melamine polyphosphate random copolymer (PAPP-co-MPP) with a certain molecular chain, the compatibility of carbon fiber and flame-retardant polyamide composite material can be improved, which plays a bridge and anchoring role between carbon fiber and other raw materials, thereby improving the mechanical properties of its flame-retardant reinforced polyamide composite material. In addition, the surface modification of carbon fiber by PAPP-co-MPP can further improve the antistatic performance of the composite material. The inventor analyzed that the reason is that the flame retardant carries hydroxyl groups, and the hydroxyl groups on the surface of some strips and the water molecules in the air form intermolecular forces, thereby improving the antistatic ability of the material.
[0037] The carbon fiber (CF) used in this technical solution has the advantages of light weight, good fineness and high tensile strength, and has the characteristics of general carbon materials, such as high temperature resistance, friction resistance, electrical conductivity, thermal conductivity, small expansion coefficient, etc. The carbon fiber composite material formed by compounding with resin, metal, ceramic and other matrices also has a series of excellent properties such as high specific strength, specific modulus, fatigue resistance, thermal conductivity, electrical conductivity, etc., and is widely used in modern industry. Polymer materials contain a large amount of hydrocarbon elements and have flammable characteristics. Polymer composite materials (polymer / CF composite materials) with carbon fiber added will infiltrate the surface of carbon fiber and generate interfacial tension at high temperature, resulting in a "candle wick effect", that is, the polymer melt will quickly infiltrate, spread and flow to the combustion area through the surface of carbon fiber, further increasing the fire hazard of polymer composite materials, making the flame retardant modification of polymer composite materials with carbon fiber added much more difficult, and limiting their development and application. In order to reduce the flammability of carbon fiber reinforced polymer materials, the current more widespread solution is to suppress the "wick effect" by adding sufficient high-quality flame retardants to polymer / carbon fiber composites. However, the addition of a large amount of flame retardants will seriously affect the mechanical properties of polymer materials, resulting in a reduction in the gain effect of carbon fiber in polymer materials.
[0038] The focused piperazine phosphate-melamine polyphosphate random copolymer (PAPP-co-MPP) modified carbon fiber provided by the present technical solution overcomes the problems of the prior art and can simultaneously improve the mechanical properties, antistatic properties and flame retardant properties of the composite material. The PAPP-co-MPP of the present solution is formed by random copolymerization of focused piperazine phosphate and melamine polyphosphate under certain conditions, and has a significant effect on improving mechanical properties, antistatic properties and flame retardant properties compared to the modification of carbon fiber by focused piperazine phosphate alone, the modification of carbon fiber by melamine polyphosphate alone, and the modification of carbon fiber by focused piperazine phosphate and melamine polyphosphate without copolymerization. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] Figure 1 Schematic diagram of the amino modification and flame retardant modification of carbon fiber in Example 2. DETAILED DESCRIPTION
[0040] The present invention is further described in detail below in conjunction with examples, but the embodiments of the present invention are not limited thereto. Unless otherwise specified, the technical means used in the following examples and experimental examples are conventional means well known to those skilled in the art, and the materials, reagents, etc. used can be obtained from commercial sources.
[0041] Example 1: Preparation of flame retardant reinforced polyamide
[0042] The raw materials of flame retardant reinforced polyamide include, by weight: 30-80 parts of nylon, 5-60 parts of CF-NH2-FR (flame retardant modified carbon fiber), 5-20 parts of melamine polyphosphate, 5-20 parts of organic aluminum hypophosphite, 0.5-4 parts of flame retardant synergist, 0.3-2 parts of nucleating agent, 0.5-2 parts of coupling agent, 0.3-3 parts of lubricant and 0.2-1 parts of antioxidant.
[0043] Wherein, nylon includes at least one of nylon 6, nylon 66, nylon 46, nylon 610, nylon 612, nylon 9, nylon 11, nylon 12, nylon 1010, nylon 1012, and nylon 1212. The organic aluminum hypophosphite is aluminum diethylphosphinate; the nucleating agent is BRUGGOLEN P22; the 1% thermal weight loss of melamine polyphosphate is greater than or equal to 360°C, and its specific preparation method is shown in Example 2. The flame retardant synergist is any one or a mixture of anhydrous zinc borate, 3.5-water zinc borate, zinc sulfide, zinc oxide, and zirconium phosphate. The coupling agent is a silane coupling agent, which can be any one or a mixture of silane coupling agents such as aminosilane coupling agent KH-9120, isocyanate silane coupling agent KT-930, epoxy silane coupling agent KH-1006 and KH-9130. The lubricant is one or more of white oil, silicone oil, polyethylene wax, ethylene bis stearamide (EBS), pentaerythritol stearate, silicone and amide wax. The antioxidant includes at least one of antioxidant 168, antioxidant 1010 and antioxidant 1098. The preparation method of CF-NH2-FR (flame retardant modified carbon fiber) is shown in Example 2.
[0044] The preparation process is as follows:
[0045] Step 1: Add nylon, melamine polyphosphate, organic aluminum hypophosphite and flame retardant synergist into a mixer and stir for 5-30 minutes at room temperature.
[0046] Step 2: Increase the mixer temperature to 80-180°C, add the coupling agent and continue stirring for 10-30 minutes.
[0047] Step 3: After cooling to room temperature, add lubricant, nucleating agent and antioxidant, and stir for 5-30 minutes to obtain a premix.
[0048] Step 4: extrude the premix by a twin-screw extruder, add CF-NH2-FR by side feeding, the temperature during extrusion is 200-300°C, and then obtain flame-retardant reinforced polyamide granules by strip drawing and pelletizing, screening and dehydration.
[0049] Example 2: Preparation of flame retardant modified carbon fiber
[0050] (1) Focus on the synthesis of piperazine phosphate (PAPP)
[0051] The structure of the focused piperazine phosphate is shown in formula (1), n=500-10000, and it is synthesized from piperazine diphosphate (formula (4)). The synthesis of piperazine diphosphate is a conventional method in the prior art (using a conventional reactor in the prior art), specifically, phosphoric acid (formula (2)) and piperazine (formula (3)) are used in a molar ratio of 2.0-2.2:1, under reaction conditions of 60-150°C and 0.1-1.0MPa (in a reaction system with water or alcohol as solvent), and the reaction is carried out for 30-300 minutes to obtain. The reaction equation is shown in formula (5).
[0052] The piperazine diphosphate obtained and purified by the above-mentioned chemical reaction is heat-treated in a nitrogen atmosphere, a pressure environment of 0.05-0.3 MPa, and a temperature of 120-320° C. for 30-240 min to undergo thermal polymerization, dehydration, and condensation to obtain piperazine phosphate (Formula (1)). The reaction equation is shown in Formula (6).
[0053]
[0054]
[0055] (2) Synthesis of melamine polyphosphate (MPP)
[0056] Using deionized water as solvent, melamine (ME) and H3PO4 are reacted by acid-base neutralization to prepare melamine phosphate (MP) with high purity, high whiteness and high thermal stability, and then MP is subjected to high-temperature thermal polymerization to obtain melamine polyphosphate (MPP). The above synthesis process can be found in the inventor's previously published paper "Zhong Zhiqiang, Synthesis of Melamine Polyphosphate and Properties of Flame-Retardant Polypropylene, Engineering Plastics Application, 2018". Specifically, in this embodiment, the method for preparing melamine phosphate is: the molar ratio of ME to H3PO4 is 1:1.05, the reaction time is 2.0h, the reaction temperature is 95°C, and the molar ratio of ME to deionized water is 3:97. Melamine phosphate (Formula (7)) was synthesized under the above conditions.
[0057] Then, melamine phosphate is used to synthesize melamine polyphosphate (MPP). Melamine phosphate is heat treated at 220-360° C. for 60-300 min in an inert gas environment (such as nitrogen) and a pressure environment of 0.05-0.3 MPa to undergo thermal polymerization and dehydration condensation to obtain melamine polyphosphate (MPP, formula (8)). The reaction formula is shown in formula (9).
[0058]
[0059] (3) Focus on the synthesis of piperazine phosphate (PAPP)-melamine polyphosphate (MPP) random copolymer (PAPP-co-MPP)
[0060] Focused piperazine phosphate and melamine polyphosphate are reacted at a mass ratio of 1:0.2-5 under reaction conditions of 200-280°C and 0.1-1.5MPa (nitrogen atmosphere) for 30-180 minutes, and then thermally polymerized and dehydrated to obtain a focused piperazine phosphate-melamine polyphosphate random copolymer (PAPP-co-MPP), the structural formula of which is shown in Formula (10), and the reaction equation of which is shown in Formula (11). The polymerization degrees of focused piperazine phosphate (PAPP, Formula (6)) and melamine polyphosphate (MPP, Formula (8)) are both greater than 500 and less than 10000, that is, 500<m<10000, and 500<n<10000. In Formula (10), x>0, y>0, and p>0, and in PAPP-co-MPP, the mass ratio of PAPP to MPP is 1:0.2-5.
[0061]
[0062]
[0063] (4) Amide modification of carbon fiber (CF-NH2)
[0064] Disperse 100 g of carbon fiber CF (T300 (6K), Toray, Japan, cut to a length of 2.5-7.5 mm) in ethanol / water (250-750 ml, for example, a 450:50 ethanol solution), add 1-5 wt % of an amino coupling agent (KH550, etc.) under high-speed stirring (200-1500 rpm), raise the temperature from room temperature to 60-100 ° C and react for 4-8 hours. After the reaction is completed, filter, wash and dry at 80 ° C to obtain CF-NH2.
[0065] (5) Preparation of flame-retardant modified carbon fiber (CF-NH2-FR)
[0066] CF-NH2 (80-160 g) is dispersed in 200-1000 mL of solvent (ethanol, water, DMF, DMSO, acetonitrile and other organic solvents), PAPP-co-MPP (0.1-5 g) is added to the solution, and the reaction is continued at 20-50 ° C for 2-12 hours, and the stirring speed is maintained at 50-1500 rpm. After the reaction is completed, filter, wash and dry at 80 ° C to obtain CF-NH2-FR.
[0067] The schematic diagram of the synthesis process of steps (4) and (5), the schematic diagram of the amino modification of carbon fiber (CF-NH2) and its flame retardant modification (CF-NH2-FR) are shown in detail. Figure 1 .
[0068] Experimental Example 1
[0069] The flame retardant reinforced polyamide composition comprises the following raw material components in parts by weight: 53 parts of nylon (PA66-EPR27), 30 parts of CF-NH2-FR, 5 parts of melamine polyphosphate, 10 parts of aluminum diethylphosphinate, 0.5 parts of zinc sulfide, 0.2 parts of nucleating agent BRUGGOLEN P22, 0.5 parts of coupling agent KH1006, 0.5 parts of ethylene bis stearamide (EBS), and 0.3 parts of antioxidant 1098. In the above formula, the addition amount of the flame retardant is 15% (melamine polyphosphate and aluminum diethylphosphinate).
[0070] Prepared as follows: Add nylon, melamine polyphosphate, organic aluminum hypophosphite and flame retardant synergist into a mixer and stir at room temperature for 30 minutes. Raise the mixer temperature to 150°C, add the coupling agent and continue stirring for 30 minutes. After cooling to room temperature, add lubricant, nucleating agent and antioxidant, stir for 30 minutes to obtain a premix. Extrude the premix with a twin-screw extruder, add CF-NH2-FR through side feeding, the temperature during extrusion is 200-300°C (preferably 220-250°C), and then obtain flame retardant reinforced polyamide granules after drawing and pelletizing, sieving and dehydrating. More specifically, the twin-screw extruder is divided into 10 temperature zones, and the temperatures of each temperature zone are 220, 230, 240, 250, 260, 260, 250, 240, 240, 220°C in the order of material movement.
[0071] The melamine polyphosphate used in the above process is prepared as follows: melamine phosphate is synthesized according to the method described in Example 2, and the melamine phosphate is heat treated at 320°C for 240 min, and is thermally polymerized and dehydrated to melamine polyphosphate (MPP, 500<m<10000) in a nitrogen environment and a pressure environment of 0.15 MPa.
[0072] Phosphoric acid and piperazine are mixed in a molar ratio of 2.05:1, reacted at 80°C and 0.1MPa for 210min in an ethanol aqueous solution environment (ethanol volume fraction 50%, phosphoric acid mass fraction of ethanol aqueous solution can be selected to be 5%-30%, 15% in specific experimental operation), and then purified and dried by conventional methods to obtain the intermediate piperazine diphosphate. The intermediate piperazine diphosphate is heat treated at 290°C and 0.1MPa nitrogen atmosphere for 240min, and thermally polymerized and dehydrated to obtain focused piperazine phosphate (PAPP, 500<n<10000).
[0073] The focused piperazine phosphate obtained in the above steps and melamine polyphosphate were mixed (according to the mass ratio of PAPP:MPP = 1:0.8), and thermally polymerized at 280°C for 180min in a 0.5MPa nitrogen atmosphere to obtain PAPP-co-MPP. After a large number of experimental studies, the PAPP-co-MPP prepared according to the above technical parameters was applied to carbon fiber modification, and a polyamide composite material was prepared. The polyamide composite material can obtain more excellent effects in mechanical properties, antistatic properties and flame retardant properties, which is the optimal parameter for preparing PAPP-co-MPP for carbon fiber modification and preparing polyamide composite materials adopted in this scheme. As a comparison, for example, a polyamide composite material prepared by a PAPP:MPP mass ratio of 1:0.6 and a pressure environment of 0.2MPa (except for the above differences, the rest is prepared by referring to the method of Experimental Example 1), and its flame retardancy UL 94 (1.0mm) is V-1 level.
[0074] Disperse 100g of carbon fiber CF (chopped CF, T300 (6K), Toray, Japan, length of about 5mm) in ethanol / water (500ml, 450:50), add 1wt% (1g) of amino coupling agent KH550 under high-speed stirring (about 1000rpm), raise the temperature from room temperature to 90℃ for 6h, and after the reaction is completed, filter, wash and dry at 80℃ to obtain CF-NH2.
[0075] CF-NH2 (100 g) was evenly dispersed in an ethanol solution (500 ml, 400:100), PAPP-co-MPP (1 g) was added to the solution, and the reaction was continued at 50 °C for 11 h (maintaining a stirring speed of about 500 rpm). After the reaction was completed, CF-NH2-FR was obtained by filtering, washing, and drying at 80 °C.
[0076] Experimental Example 2
[0077] This experimental example is basically the same as the experimental example 1, except that the amount of the flame retardant added is 12% (melamine polyphosphate and diethyl aluminum phosphinate), and the specific formula is: 56 parts of nylon (PA66-EPR27), 30 parts of CF-NH2-FR, 4 parts of melamine polyphosphate, 8 parts of diethyl aluminum phosphinate, 0.5 parts of zinc sulfide, 0.2 parts of nucleating agent, 0.5 parts of coupling agent KH1006, 0.5 parts of ethylene bis stearic acid amide, and 0.3 parts of antioxidant 1098. A flame retardant reinforced polyamide composition was prepared according to the above formula.
[0078] Comparative Experiment Example 1
[0079] The flame retardant reinforced polyamide composition was prepared in the same manner as in Experimental Example 1, except that an equal amount of untreated chopped CF was used instead of CF-NH2-FR.
[0080] Comparative Experiment Example 2
[0081] The flame retardant reinforced polyamide composition was prepared in the same manner as in Experimental Example 2, except that an equal amount of untreated chopped CF was used instead of CF-NH2-FR.
[0082] Comparative Experiment 3
[0083] The flame retardant reinforced polyamide composition was prepared in the same manner as in Experimental Example 1, except that CF-NH2 was used in an equal amount to replace CF-NH2-FR. The specific preparation method of CF-NH2 is shown in Experimental Example 1.
[0084] Comparative Experiment Example 4
[0085] The same method as in Experimental Example 1 is used, but an equal amount of PAPP-modified CF (CF-NH2-PAPP) is used to replace CF-NH2-FR to prepare a flame retardant reinforced polyamide composition. The preparation method of CF-NH2-PAPP is similar to that in Experimental Example 1, except that an equal amount of PAPP-co-MPP in Experimental Example 1 is replaced by focused piperazine phosphate (PAPP), and the preparation method of focused piperazine phosphate is also the same as that in Experimental Example 1.
[0086] Comparative Experiment Example 5
[0087] The same method as in Experimental Example 1 is used, but an equal amount of MPP-modified CF (CF-NH2-MPP) is used to replace CF-NH2-FR to prepare a flame retardant reinforced polyamide composition. The preparation method of CF-NH2-MPP is as in Experimental Example 1, except that an equal amount of PAPP-co-MPP in Experimental Example 1 is replaced by melamine polyphosphate (MPP), and the preparation method of melamine polyphosphate is also the same as in Experimental Example 1.
[0088] Comparative Experiment Example 6
[0089] The same method as in Experimental Example 1 is used, but CF modified by PAPP and MPP (CF-NH2-PAPP / MPP) is used in equal amounts instead of CF-NH2-FR to prepare a flame retardant reinforced polyamide composition. The preparation method of CF-NH2-PAPP / MPP is similar to that in Experimental Example 1, except that 1 g of PAPP-co-MPP in Experimental Example 1 is replaced by a mixture of PAPP and MPP in a mass ratio of 1:0.8, and the preparation method of focused piperazine phosphate and melamine polyphosphate is also the same as that in Experimental Example 1.
[0090] The formula compositions of the experimental examples and comparative experimental examples are summarized in Table 1, and the experimental results are shown in Table 2.
[0091] Table 1: Composition of the formula of the experimental example and the comparative experimental example
[0092]
[0093]
[0094] The flame retardant reinforced polyamide composite materials (flame retardant reinforced polyamide compositions) synthesized in the experimental examples and comparative experimental examples were subjected to performance tests. The performance indicators include flame retardancy test, oxygen index (LOI) test, surface resistance, tensile strength, and notched impact strength. The flame retardancy test was conducted according to Test for Flammability of Plastic Materials for Parts in Devices and Appliances-UL 94. The reference standard for oxygen index (LOI) test is GB / T 2406. The reference standard for surface resistance is MT 113. The reference standard for tensile strength is GB / T1040. The reference standard for notched impact strength is GB / T1843.
[0095] Table 2: Test results of various properties of the flame retardant reinforced polyamide compositions synthesized in the experimental examples and comparative experimental examples
[0096]
[0097] Experimental Example 1 adopts the flame retardant modified carbon fiber (CF-NH2-FR) of this scheme. When the flame retardant is added less, a relatively ideal flame retardant effect can be achieved, and the mechanical properties and antistatic properties of the material are guaranteed. Experimental Example 2 has a reduced amount of flame retardant (melamine polyphosphate and diethyl phosphinate aluminum) added compared to Experimental Example 1, and the flame retardant performance has a certain decline. Comparative Experimental Example 1 does not use flame retardant modified carbon fiber (CF-NH2-FR), but uses ordinary carbon fiber. Compared with Comparative Experimental Example 1, Experimental Example 2 is similar in flame retardant performance indicators, but the amount of flame retardant (melamine polyphosphate and diethyl phosphinate aluminum) added in Experimental Example 2 is less. When the amount of flame retardant added is less, Experimental Example 2 can maintain a certain flame retardant effect, which shows that the flame retardant modified carbon fiber (CF-NH2-FR) of this scheme has the effect of increasing the flame retardant effect of the composite material, and a smaller amount of flame retardant can be added to the composite material to save flame retardant raw materials and reduce the impact of flame retardant on the performance of the composite material.
[0098] This scheme adopts the scheme of synthesizing random copolymers (PAPP-co-MPP) by focusing piperazine phosphate PAPP and melamine polyphosphate MPP. The surface modification of carbon fiber using this new material can improve the effect of carbon fiber on polyamide material, eliminate or inhibit the "candle wick effect", and enhance flame retardant properties. The carbon fiber in comparative experimental example 1 was not modified, the carbon fiber in comparative experimental example 3 was only amino-modified, the carbon fiber in comparative experimental example 4 was modified with PAPP, and the carbon fiber in comparative experimental example 5 was modified with MPP. The flame retardant properties of the composite material were not ideal, and there was a relatively large gap between the composite material synthesized in experimental example 1. In addition, the inventor also tried to use PAPP and MPP for the modification of carbon fiber at the same time, but did not synthesize PAPP-co-MPP (Comparative Experimental Example 6), and found that this operation mode had little effect on improving the flame retardant effect of the composite material (comparable to the flame retardant properties of the composite materials of comparative experimental examples 4 and comparative experimental examples 5). From the flame retardant test results of Comparative Experimental Example 1, Comparative Experimental Example 4, and Comparative Experimental Example 5, it can be seen that the combined modification of carbon fiber with PAPP and MPP can effectively improve the flame retardant properties of the composite material and produce a certain synergistic effect, and this combined use must be achieved in the form of a synthetic random copolymer.
[0099] The composite material of Experimental Example 1 has a significant improvement in mechanical properties relative to Comparative Experimental Example 1. Although the carbon fiber can be improved to varying degrees in mechanical strength (when the carbon fiber of Comparative Experimental Example 1 is not modified) after amino modification (Comparative Experimental Example 3), PAPP modification (Comparative Experimental Example 4), MPP modification (Comparative Experimental Example 5), and PAPP and MPP combined modification (without random copolymer synthesis, Comparative Experimental Example 6) of the carbon fiber, the mechanical properties of the carbon fiber after random copolymer modification (Experimental Example 1) are more significant. It can be seen that after the surface of the carbon fiber is modified with PAPP-co-MPP having a certain molecular chain, the compatibility of carbon fiber and nylon can be improved, which plays a bridge and anchoring role between carbon fiber and other flame retardants / nylon, thereby improving the mechanical properties of its flame retardant reinforced polyamide composite material.
[0100] In terms of antistatic performance, the use of PAPP-co-MPP modified carbon fiber of this scheme can effectively reduce the surface resistance of the material and improve the antistatic performance of the material. The inventor analyzed the reason because: the conductivity of the carbon fiber itself, after the carbon fiber surface is modified with PAPP-co-MPP, because the flame retardant has hydroxyl groups, the hydroxyl groups on the surface of some splines and the water molecules in the air form intermolecular forces, which improve the antistatic ability of the material. And the enhancement effect of PAPP-co-MPP modification on antistatic ability is significantly better than PAPP modification alone, MPP modification alone, and PAPP and MPP simple mixture modification. The surface resistance of the composite materials of Comparative Experimental Example 4, Comparative Experimental Example 5, and Comparative Experimental Example 6 is only about 1 times lower than that of Comparative Experimental Example 1 without any carbon fiber modification, but the surface resistance of the composite material of Experimental Example 1 is relative to the composite materials of Comparative Experimental Example 4, Comparative Experimental Example 5, and Comparative Experimental Example 6. It has dropped by an order of magnitude. This shows that PAPP and MPP can produce a synergistic effect on the antistatic performance of the material under a specific polymerization method.
[0101] The above is only an embodiment of the present invention, and the common knowledge such as the known specific technical solutions and / or characteristics in the solution is not described in detail here. It should be pointed out that for those skilled in the art, without departing from the technical solution of the present invention, several modifications and improvements can be made, which should also be regarded as the protection scope of the present invention, and these will not affect the effect of the implementation of the present invention and the practicality of the patent. The scope of protection required by this application shall be based on the content of its claims, and the specific implementation methods and other records in the specification can be used to interpret the content of the claims.
Claims
1. A flame retardant reinforced polyamide composite material, characterized in that: The raw materials include, by weight: 30-80 parts of nylon, 5-60 parts of flame retardant modified carbon fiber, 5-20 parts of melamine polyphosphate, 5-20 parts of organic aluminum hypophosphite, 0.5-4 parts of flame retardant synergist, 0.3-2 parts of nucleating agent, 0.5-2 parts of coupling agent, 0.3-3 parts of lubricant and 0.2-1 parts of antioxidant.
2. The flame retardant reinforced polyamide composite material according to claim 1, characterized in that: The flame retardant modified carbon fiber is prepared by the following method: S1 Synthesis of random copolymer: The melamine polyphosphate represented by formula (8) and the focused piperazine phosphate represented by formula (1) are subjected to thermal polymerization reaction to obtain a focused piperazine phosphate-melamine polyphosphate random copolymer represented by formula (10); Wherein, 500<m<10000, 500<n<10000, x>0, y>0, p>0; In formula (10), MPP represents formula (8), PAPP represents formula (1), and the mass ratio of PAPP to MPP is 1:0.2-5; S2 Amination modification: Use amino coupling agents to modify the surface of carbon fiber to obtain amination carbon fiber; S3 random copolymer modification: The surface of amino carbon fiber was modified using focused piperazine phosphate-melamine polyphosphate random copolymer to obtain flame retardant modified carbon fiber.
3. The flame retardant reinforced polyamide composite material according to claim 2, characterized in that: In S1, the mass ratio of piperazine phosphate to melamine polyphosphate is 1:0.2-5; the conditions of the thermal polymerization reaction are: 200-280°C reaction temperature, 0.1-1.5MPa nitrogen atmosphere, and 30-180min reaction time; Preferably, the mass ratio of piperazine phosphate to melamine polyphosphate is 1:0.8; the conditions of the thermal polymerization reaction are: 280° C. reaction temperature, 0.5 MPa nitrogen atmosphere, and 180 min reaction time.
4. The flame retardant reinforced polyamide composite material according to claim 3, characterized in that: In S1, the focused piperazine phosphate is obtained by the following method: dipiperazine phosphate is heat-treated for 30-240 min in a nitrogen atmosphere, a pressure environment of 0.05-0.3 MPa, and a temperature of 120-320° C. to obtain the focused piperazine phosphate by thermal polymerization and dehydration condensation; The melamine polyphosphate is obtained by the following method: melamine phosphate is heat-treated for 60-300 minutes under a nitrogen atmosphere, a pressure environment of 0.05-0.3 MPa, and a temperature of 220-360° C. to thermally polymerize and dehydrate and condense to obtain the melamine polyphosphate.
5. The flame retardant reinforced polyamide composite material according to claim 2, characterized in that: In S2, the carbon fiber is dispersed in an ethanol solution, and then an amino coupling agent is added under stirring conditions of 200-1500 rpm, and the mixture is reacted at 60-100° C. for 4-8 hours to obtain amino carbon fiber.
6. The flame retardant reinforced polyamide composite material according to claim 5, characterized in that: In S2, the length of the carbon fiber is 2.5-7.5 mm; the ratio of the carbon fiber to the ethanol solution is 100 g: 250-750 ml.
7. The flame retardant reinforced polyamide composite material according to claim 2, characterized in that: In S3, the aminated carbon fiber is dispersed in a solvent, and then the focused piperazine phosphate-melamine polyphosphate random copolymer is added, and the reaction is carried out at 20-50° C. for 2-12 hours to obtain a flame retardant modified carbon fiber; The solvent includes any one of ethanol, water, DMF, DMSO, acetonitrile and ethanol solution. The ratio of the amino carbon fiber, the focused piperazine phosphate-melamine polyphosphate random copolymer and the solvent is 80-160g: 0.1-5g: 200-1000mL.
8. The method for preparing a flame retardant reinforced polyamide composite material according to claim 1, characterized in that: The nylon includes at least one of nylon 6, nylon 66, nylon 46, nylon 610, nylon 612, nylon 9, nylon 11, nylon 12, nylon 1010, nylon 1012 and nylon 1212; The organic aluminum hypophosphite is aluminum diethylphosphinate; the nucleating agent is BRUGGOLEN P22; The 1% thermal weight loss of the melamine polyphosphate is greater than or equal to 360° C., and the melamine polyphosphate is prepared by the following method: melamine phosphate is heat-treated for 60-300 minutes under a nitrogen atmosphere, a pressure environment of 0.05-0.3 MPa, and a temperature of 220-360° C. to thermally polymerize and dehydrate to condense into the melamine polyphosphate; The flame retardant synergist includes at least one of anhydrous zinc borate, 3.5 hydrate zinc borate, zinc sulfide, zinc oxide, and zirconium phosphate; The coupling agent includes at least one of KH-9120, KT-930, KH-1006 and KH-9130; The lubricant comprises at least one of white oil, silicone oil, polyethylene wax, ethylene bis stearamide, pentaerythritol stearate, silicone and amide wax; The antioxidant includes at least one of antioxidant 168 , antioxidant 1010 , and antioxidant 1098 .
9. A method for preparing a flame retardant reinforced polyamide composite material according to any one of claims 1 to 8, characterized in that: Add nylon, melamine polyphosphate, organic aluminum hypophosphite and flame retardant synergist into a mixer and stir for 5-30 minutes at room temperature; increase the temperature of the mixer to 80-180°C, add a coupling agent and continue stirring for 10-30 minutes; after cooling to room temperature, add a lubricant, a nucleating agent and an antioxidant, stir for 5-30 minutes to obtain a premix; extrude the premix with a twin-screw extruder, add CF-NH2-FR through side feeding, the temperature during extrusion is 200-300°C, and then obtain flame retardant reinforced polyamide granules through drawing, pelletizing, screening and dehydration.
10. Application of flame retardant modified carbon fiber in flame retardant reinforced polyamide, characterized in that: The flame retardant modified carbon fiber is prepared by the following method: S1 Synthesis of random copolymer: The melamine polyphosphate represented by formula (8) and the focused piperazine phosphate represented by formula (1) are subjected to thermal polymerization reaction to obtain a focused piperazine phosphate-melamine polyphosphate random copolymer represented by formula (10); Wherein, 500<m<10000, 500<n<10000, x>0, y>0, p>0; In formula (10), MPP represents formula (8), PAPP represents formula (1), and the mass ratio of PAPP to MPP is 1:0.2-5; S2 Amination modification: Use amino coupling agents to modify the surface of carbon fiber to obtain amination carbon fiber; S3 random copolymer modification: The surface of amino carbon fiber was modified using focused piperazine phosphate-melamine polyphosphate random copolymer to obtain flame retardant modified carbon fiber.
Citation Information
Cited By
Halogen-free compound flame retardant and application thereof in antistatic nylon 66 composite material
CN121136199A