Two-component acrylate adhesive for optical component and preparation method of two-component acrylate adhesive

By grafting the hindered phenol light stabilization additive into the acrylate polymer and using a sealing curing agent, the deformation and yellowing of the acrylate adhesive in high temperature and high humidity environment is solved, and the electronic optical components are improved Stability and secondary construction performance.

CN118995094AActive Publication Date: 2024-11-22WANHUA CHEM GRP CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411333257.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-24
Publication Date
2024-11-22
Estimated Expiration
2044-09-24

AI Technical Summary

Technical Problem

Existing acrylate adhesives are prone to deform and yellowing in high temperature and high humidity environments, affecting the stability and reliability of electronic and optical components, and it is difficult to complete tight attachment during secondary construction.

Method used

Through polymerization, the hindered phenol light stabilization additive containing double bond groups is grafted onto the acrylate polymer molecular chain to form a permanent photo-stabilizing polymer, and a partially blocked isocyanate curing agent is used to match the acrylate adhesive with a partially blocked isocyanate curing agent. , through a two-step maturation process, the macromolecular linear adhesive is generated to ensure the stability and strength of the film in a high temperature and high humidity environment.

Benefits of technology

It significantly improves the high-temperature yellowing performance and secondary construction performance of electronic optical components, enhances the stability and reliability in high-temperature and high-humidity environments, and solves the deformation and yellowing problems.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005057593830000031
    Figure BDA0005057593830000031
  • Figure BDA0005057593830000061
    Figure BDA0005057593830000061
  • Figure BDA0005057593830000071
    Figure BDA0005057593830000071
Patent Text Reader

Abstract

The invention discloses a two-component acrylate adhesive as well as a preparation method and application thereof. The two-component acrylate adhesive comprises: a component A comprising an acrylate polymer (a) dispersed in a solvent; the component B comprises a partially blocked isocyanate curing agent (b), the partially blocked isocyanate curing agent (b) is a reactant of an isocyanate tripolymer and ketoxime, and the blocking ratio of isocyanate groups in the partially blocked isocyanate curing agent (b) is 35%-65%; wherein the acrylate copolymer (a) comprises a unit derived from a (meth) acrylic monomer, a unit derived from an aryl (meth) acrylate monomer, a unit derived from a hydroxyl group-containing (meth) acrylate monomer, and is derived from (meth) Copolymers of units of an alkyl acrylate monomer and units derived from a radically polymerizable hindered amine light stabilizer. The two-component acrylate adhesive can obviously improve the high-temperature yellowing resistance, the secondary construction performance and the stability in a high-temperature and high-humidity environment.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of preparation of solvent-based acrylic ester adhesives, and in particular relates to a two-component acrylic ester adhesive for optical parts and a preparation method thereof. Background Art

[0002] In recent years, the market demand for liquid crystal display panels and touch screens has increased significantly, which has promoted the development and innovation of electronic optical component technology in the field of image display. Polaroid, one of the core components, is bonded with adhesives to meet the performance requirements of electronic optical components, such as lightness, high density and durability. Acrylic adhesives for optical components are very critical raw materials in the manufacturing and use of electronic optical components, and play an irreplaceable role in the performance release and stable use of electronic optical components.

[0003] Polarizers in electronic optical components require special performance advantages under special working conditions during use. The reliability of polarizers will deteriorate when exposed to heat. When working at high temperature for a long time, ordinary adhesives will discolor due to the heat of the resin, causing the film to turn yellow, which will affect the use effect. At the same time, during the construction and coating process, the film needs secondary construction and re-peeling. At this time, the conventional adhesive has undergone two-component activation and cross-linking, and the internal structure of the film has already shown body cross-linking. The secondary construction cannot complete the tight attachment to the substrate, which means that the secondary construction will result in scrapping. In high temperature and high humidity environments, large-size high-definition LCD panels and harsh usage scenarios will make the polarizer's reliability deteriorate when exposed to heat and the shrinkage and deformation in high humidity environments more serious. In order to meet the performance requirements of emerging industries for electronic optical components, as a key factor affecting the performance and quality of electronic optical components, acrylic adhesives for optical components also need technological innovation and breakthroughs.

[0004] The invention provides a two-component acrylic adhesive composition for optical parts and a preparation method thereof. A hindered phenol light stabilizing auxiliary agent containing a double bond group is grafted onto an acrylic polymer molecular chain through a polymerization reaction to form a permanent light stabilizing polymer with a hindered amine functional group. The light stabilizer can well avoid the loss of the light stabilizer caused by physical migration or volatilization, improve and enhance the dispersion performance and light stabilizing effect of the hindered amine light stabilizer in the polymer, so that the adhesive film can maintain an excellent light stabilizing effect in a subsequent long-term high-temperature working environment; at the same time, a partially blocked curing agent is used in combination with the acrylic adhesive, and a two-step aging process is performed. In the first step of aging, the hydroxyl group in the linear polymer acrylic resin reacts with the exposed isocyanate to produce a macromolecular linear adhesive. During the construction and coating process, the coating is removed and cut again. The adhesive film has a certain strength and can be completely removed. After the construction is completed, high-temperature aging is further performed. At this time, the blocked isocyanate is unblocked, and micro-crosslinking is continued. The subsequent film strength is further improved, the reliability in a high-temperature and high-humidity environment is enhanced, and the problem of shrinkage and deformation in a high-humidity environment is solved; the high-temperature and high-humidity resistance performance is further improved. Summary of the invention

[0005] The object of the present invention is to provide a two-component acrylic adhesive for optical components and a preparation method thereof. The two-component acrylic adhesive can be used for bonding optical components and can significantly improve the high-temperature yellowing resistance, secondary construction performance and stability of electronic optical components in high temperature and high humidity environments without affecting the mechanical properties of the optical components.

[0006] According to the method for preparing a two-component acrylic adhesive for optical parts of the present invention, a hindered phenol light stabilizing agent containing a double bond group is grafted onto an acrylic polymer molecular chain through a polymerization reaction to form a permanent light stabilizing polymer with a hindered amine functional group. This light stabilizer can well avoid the loss of light stabilizer caused by physical migration or volatilization, improve and enhance the dispersion performance and light stabilizing effect of the hindered amine light stabilizer in the polymer, so that the adhesive film can maintain an excellent light stabilizing effect in a subsequent long-term high-temperature working environment; at the same time, a partially blocked curing agent is used in combination with the acrylic adhesive, and a two-step aging process is performed. In the first step of aging, the hydroxyl groups in the linear polymer acrylic resin react with the exposed isocyanate to produce a macromolecular linear adhesive. During the construction and coating process, the coating is removed and cut again. The adhesive film has a certain strength and can be completely removed. After the construction is completed, high-temperature aging is further performed. At this time, the blocked isocyanate is unblocked and micro-crosslinking is continued. The subsequent film strength is further improved, the reliability in a high-temperature and high-humidity environment is enhanced, and the problem of shrinkage and deformation in a high-humidity environment is solved; the high-temperature and high-humidity resistance performance is further improved.

[0007] To achieve the above purpose, the technical solution adopted by the present invention is as follows:

[0008] According to a first aspect of the present invention, a two-component acrylic adhesive is provided, comprising component A and component B, wherein:

[0009] Component A comprises an acrylate polymer (a) dispersed in a solvent,

[0010] Component B comprises a partially blocked isocyanate curing agent (b), wherein:

[0011] The acrylic acid ester copolymer (a) is a copolymer comprising a unit derived from a (meth)acrylic acid monomer, a unit derived from an aryl (meth)acrylate monomer, a unit derived from a (meth)acrylate monomer containing a hydroxyl group, a unit derived from an alkyl (meth)acrylate monomer, and a unit derived from a free radical polymerizable hindered amine-based light stabilizer;

[0012] The partially blocked isocyanate curing agent (b) is a reaction product of isocyanate trimer and ketoxime, and the blocking ratio of isocyanate groups therein is 35% to 65%, preferably 40% to 60%.

[0013] Preferably, the content of the acrylate polymer (a) is 90 to 95 parts by weight, and the content of the partially blocked isocyanate curing agent (b) is 5 to 10 parts by weight.

[0014] Preferably, the weight average molecular weight of the acrylic acid ester polymer (a) is 1 million to 3 million, more preferably 1 million to 2 million.

[0015] Preferably, the solid content of component A is 10 wt% to 30 wt%, preferably 15 wt% to 25 wt%.

[0016] In addition, the weight average molecular weight in the present invention is the weight average molecular weight (Mw) of the polymer measured by gel permeation chromatography (GPC).

[0017] Preferably, the (meth) aryl acrylate monomer is (meth) acrylic acid C6-C 12 The aryl ester is more preferably selected from one or more of benzyl (meth)acrylate, phenyl (meth)acrylate, and phenoxyethyl (meth)acrylate.

[0018] Preferably, the hydroxyl-containing (meth)acrylate monomer is a hydroxy C1-C6 alkyl (meth)acrylate, more preferably one or more selected from 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate and 6-hydroxyhexyl (meth)acrylate.

[0019] Preferably, the (meth)acrylic acid alkyl ester is (meth)acrylic acid C1-C 12 The alkyl ester is more preferably one or more selected from methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, tert-butyl (meth)acrylate, pentyl (meth)acrylate, hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, n-octyl (meth)acrylate, isooctyl (meth)acrylate, n-nonyl (meth)acrylate, isononyl (meth)acrylate, n-decyl (meth)acrylate, isodecyl (meth)acrylate, undecyl (meth)acrylate and lauryl (meth)acrylate.

[0020] Preferably, the structure of the free radical polymerizable hindered amine light stabilizer is as follows:

[0021]

[0022] Preferably, relative to 100 wt % of the total weight of the monomers, the amount of the free radical polymerizable hindered amine light stabilizer is 0.01 wt % to 0.5 wt %, preferably 0.1 wt % to 0.2 wt %.

[0023] Preferably, in the process of preparing the acrylic ester polymer (a), relative to 100wt% of the total weight of the monomers used in preparing component A, the amount of the (meth)acrylic acid monomer is 1wt% to 3wt%, the amount of the (meth)acrylic acid aryl ester monomer is 3wt% to 40wt%, the amount of the hydroxyl-containing (meth)acrylic acid ester monomer is 3wt% to 5wt%, and the amount of the (meth)acrylic acid alkyl ester is 60wt% to 70wt%.

[0024] Preferably, the weight ratio of isocyanate trimer to ketoxime is 1 to 10:1, preferably 3.5 to 5:1.

[0025] Preferably, the ketoxime is one or more of methyl ethyl ketone oxime, butanone oxime, acetone oxime, formaldehyde oxime, acetaldehyde oxime and cyclohexanone oxime, more preferably methyl ethyl ketone oxime.

[0026] Preferably, the isocyanate trimer is HDI trimer.

[0027] Preferably, the solvent in component A is one or more selected from aromatic hydrocarbon solvents, aliphatic hydrocarbon solvents, alicyclic hydrocarbon solvents, ether solvents, halogenated hydrocarbon solvents, ester solvents, ketone solvents and nitrile solvents.

[0028] Preferably, the aromatic hydrocarbon solvent is selected from any one or more of benzene, toluene and xylene.

[0029] Preferably, the aliphatic hydrocarbon solvent is any one or more selected from n-pentane, n-hexane, n-heptane and n-octane.

[0030] Preferably, the alicyclic hydrocarbon solvent is one or more selected from cyclopentane, cyclohexane, cycloheptane and cyclooctane.

[0031] Preferably, the ether solvent is any one or more selected from diethyl ether, diisopropyl ether, dibutyl ether, tetrahydrofuran, anisole, phenethyl ether and diphenyl ether.

[0032] Preferably, the halogenated hydrocarbon solvent is any one or more selected from chloroform, carbon tetrachloride, ethylene dichloride and chlorobenzene.

[0033] Preferably, the ester solvent is any one or more selected from methyl acetate, ethyl acetate, propyl acetate, butyl acetate and methyl propionate.

[0034] Preferably, the ketone solvent is any one or more selected from acetone, methyl ethyl ketone, diethyl ketone, methyl isobutyl ketone and cyclohexanone.

[0035] Preferably, the nitrile solvent is any one or more selected from acetonitrile and benzonitrile.

[0036] It should be noted that, in the storage state, the acrylate polymer (a) and the partially blocked isocyanate curing agent (b) are stored separately. Before application, the two are mixed and applied for use.

[0037] According to a second aspect of the present invention, there is provided a method for preparing a two-component acrylic adhesive for optical components, comprising the following steps:

[0038] Step 1), preparation of component A: in the presence of a solvent, an acrylic acid monomer, a (meth)acrylic acid aryl ester monomer, a (meth)acrylic acid ester monomer containing a hydroxyl group, a (meth)acrylic acid alkyl ester and a free radical polymerizable hindered amine light stabilizer are polymerized in the presence of an initiator to obtain an acrylic acid ester polymer (a);

[0039] Step 2), preparation of component B: reacting an isocyanate trimer with a ketoxime to obtain a partially blocked isocyanate curing agent (b).

[0040] Preferably, the polymerization method in step 1) is solution polymerization.

[0041] Preferably, the solvent in step 1) is one or more selected from aromatic hydrocarbon solvents, aliphatic hydrocarbon solvents, alicyclic hydrocarbon solvents, ether solvents, halogenated hydrocarbon solvents, ester solvents, ketone solvents and nitrile solvents. The specific types of the aromatic hydrocarbon solvents, aliphatic hydrocarbon solvents, alicyclic hydrocarbon solvents, ether solvents, halogenated hydrocarbon solvents, ester solvents, ketone solvents and nitrile solvents are the same as described above.

[0042] Preferably, the polymerization in step 1) is carried out in the following manner:

[0043] Under an inert atmosphere, acrylic acid monomer, (meth) aryl acrylate monomer, hydroxyl-containing (meth) acrylate monomer, (meth) alkyl acrylate and free radical polymerizable hindered amine light stabilizer are added to a solvent, the temperature is raised to 60-80°C, an initiator is added, and the polymerization reaction is carried out at a constant temperature.

[0044] Preferably, the amount of the initiator used is 0.01 wt% to 0.5 wt%, preferably 0.05 wt% to 0.2 wt%, relative to 100 wt% of the monomer.

[0045] Preferably, the initiator is a thermal initiator and / or a redox initiator.

[0046] Preferably, the thermal initiator is a persulfate initiator, such as ammonium persulfate, sodium persulfate, potassium persulfate, etc.; a peroxide initiator, such as hydrogen peroxide, tert-butyl hydroperoxide, isopropyl benzene hydroperoxide, diisopropyl benzene hydroperoxide, di-tert-butyl hydroperoxide, di-tert-amyl hydroperoxide, di(3,3,5-trimethylhexanoyl) peroxide, di(tert-butylperoxyisopropyl) benzene, benzoyl peroxide, lauroyl peroxide, hexanoyl peroxide, di(4-methylbenzoyl) peroxide, diisopropyl peroxydicarbonate, di-2-ethylhexyl peroxydicarbonate, di(4-tert-butylcyclohexyl) peroxydicarbonate, 2,5-dimethyl-2, 5-di(tert-butylperoxy)hexane, 1,1-di-tert-butylperoxy-3,3,5-trimethylcyclohexane, 1,1-di-tert-butylperoxycyclohexane, 2,5-dimethyl-2,5-di(2-ethylhexanoic acid peroxy)hexane, tert-butyl peroxypivalate, tert-butyl peroxybenzoate, tert-butyl peroxyisononanoate, tert-butyl peroxy-2-ethylhexanoate, etc.; azo initiators, such as azobisisobutyronitrile, azobis(cyclohexane-1-carbonitrile), azobis(2-cyclopropylpropionitrile), azobis(2-methylbutyronitrile), azobis(2,4-dimethylvaleronitrile), azobis(4-methoxy-2,4-dimethylvaleronitrile), etc.

[0047] The redox initiator comprises one or more oxidants and one or more reducing agents. Preferably, the oxidant is selected from the thermal initiator, and the reducing agent is selected from one or more of sodium sulfite, sodium bisulfite, sodium pyrosulfite, sodium hydrosulfite, sodium sulfate, bleaching powder, and ascorbic acid.

[0048] Preferably, the reaction in step 2) is carried out in the following manner:

[0049] In an inert atmosphere, ketone is added dropwise to the isocyanate trimer to carry out the reaction. The reaction temperature is preferably 40 to 60°C.

[0050] According to a third aspect of the present invention, there is provided use of the two-component acrylic adhesive for optical components according to the present invention in bonding optical components.

[0051] According to a fourth aspect of the present invention, there is provided a method for applying the two-component acrylic adhesive for optical components according to the present invention, comprising the following steps:

[0052] 2-1) mixing the component A and the component B uniformly to obtain an adhesive composition, wherein the content of the acrylic ester polymer (a) in the component A is 90 to 95 parts by weight, and the content of the partially blocked isocyanate curing agent (b) in the component B is 5 to 10 parts by weight;

[0053] 2-2) applying the adhesive composition obtained in step 2-1) to form a uniform coating, and drying at a temperature of 40 to 70° C. to obtain an adhesive film;

[0054] 2-3) The adhesive film obtained in step 2-2) is placed between the objects to be adhered, and is subjected to high pressure treatment at 90-110° C. and 5-7 atmospheres for 20 minutes, and then cured at a temperature of 90-110° C.

[0055] The use of the two-component acrylic adhesive for optical components of the present invention is not particularly limited, and can be applicable to the application direction of the adhesive. Preferably, the two-component acrylic adhesive for optical components can be used for bonding optical components. When the two-component acrylic adhesive for optical components according to the present invention is used for bonding optical components, it can significantly improve the high temperature yellowing resistance, secondary construction performance and stability of electronic optical components in high temperature and high humidity environments without affecting the mechanical properties of the optical components. DETAILED DESCRIPTION

[0056] The technical solution of the present invention is further described below through specific embodiments. The embodiments of the present invention are only used to help understand the description of the present invention and do not specifically limit the scope of the present invention.

[0057] The information of raw materials involved in the specific embodiments of the present invention is shown in Table 1.

[0058] Table 1. Main raw material information

[0059]

[0060]

[0061] Unless otherwise specified, raw materials or reagents can be purchased from commercial sources.

[0062] Example 1

[0063] The two-component acrylic adhesive for optical components was prepared as follows:

[0064] Preparation of Component A: Preparation of Acrylate Polymer (a)

[0065] In a reaction vessel equipped with a stirring device, a reflux condenser, a thermometer and a nitrogen tube, 365g of solvent ethyl acetate and 86.22g of benzyl acrylate, 175g of n-butyl acrylate, 10g of 2-hydroxyethyl acrylate, 5g of acrylic acid, and 0.275g of a reactive hindered phenol light stabilizer (commercially available, Aidico hindered phenol light stabilizer LA-82, unless otherwise specified, other embodiments use the same reactive hindered phenol light stabilizer), stirring is started, and the air in the reaction vessel is replaced with nitrogen. After 10 minutes, heating is started, and the temperature in the reaction vessel is adjusted to 65°C. After the temperature in the reaction vessel is stable, 0.28g of an initiator tert-butyl pivalate is added to the reaction vessel at one time, and a polymerization reaction is carried out at 65°C for 3h;

[0066] After the polymerization reaction was completed, the temperature in the reaction vessel was maintained at 62°C, 331 g of ethyl acetate was added to the reaction vessel under stirring, stirred for 10 minutes, and then cooled to room temperature to obtain an acrylate polymer (a) dispersed in ethyl acetate solvent. The weight average molecular weight (Mw) of the polymer measured by gel permeation chromatography (GPC) was 1.6 million;

[0067] Preparation of component B: Preparation of partially blocked curing agent (b)

[0068] In a reaction vessel equipped with a stirring device, a reflux condenser, a thermometer and a nitrogen tube, 240 g of HT600 (curing agent) was added, stirring was started, and heating was started under nitrogen flow. The temperature in the reaction vessel was adjusted to 50° C. After the temperature in the reaction vessel stabilized, methyl ethyl ketone oxime was added dropwise. The reaction temperature was maintained at no more than 55° C. The addition time was 30 minutes, and a total of 60 g was added dropwise. During the reaction, stirring was continued to react, and a partially blocked curing agent (b) was finally obtained, wherein the blocking ratio of the isocyanate group was 50%.

[0069] Preparation of adhesive films for performance evaluation

[0070] The acrylate polymer (a) and the partially blocked curing agent (b) dispersed in the ethyl acetate solvent are uniformly mixed, wherein the weight ratio of the acrylate polymer (a) to the partially blocked curing agent (b) is 9.5:0.5. The acrylate polymer (a) is uniformly coated on the release film by a manual wire rod coating method, and the film is dried at 60°C for 2 hours, and the thickness of the film after drying is controlled to be 30±2μm. The film on the release film is transferred to the triacetate resin film, the release film is torn off, and a protective release film is covered on the adhesive layer. The triacetate resin film with the adhesive layer is cut into a size of 20cm×30cm, and the release film is torn off and pasted on the glass plate, and pressed. The glass plate with the triacetate resin film is placed under 100°C and 5 atmospheres for 20 minutes of high pressure treatment, and then left to stand for 6 hours in an environment of 100°C / 50%RH to prepare an optical component for performance evaluation.

[0071] Example 2

[0072] The two-component acrylic adhesive for optical components was prepared as follows:

[0073] Preparation of Component A: Preparation of Acrylate Polymer (a)

[0074] In a reaction vessel equipped with a stirring device, a reflux condenser, a thermometer and a nitrogen tube, 365 g of solvent ethyl acetate and 86.22 g of benzyl acrylate, 175 g of n-butyl acrylate, 10 g of 2-hydroxyethyl acrylate, 5 g of acrylic acid, and 0.275 g of a reactive hindered phenol light stabilizer were added, stirring was started, and the air in the reaction vessel was replaced with nitrogen. After 10 minutes, heating was started and the temperature in the reaction vessel was adjusted to 65° C. After the temperature in the reaction vessel was stable, 0.5 g of initiator tert-butyl pivalate was added to the reaction vessel at one time, and a polymerization reaction was carried out at 65° C. for 3 hours;

[0075] After the polymerization reaction was completed, the temperature in the reaction vessel was maintained at 62°C, 331 g of ethyl acetate was added to the reaction vessel under stirring, stirred for 10 minutes, and then cooled to room temperature to obtain an acrylate polymer (a) dispersed in ethyl acetate solvent. The weight average molecular weight (Mw) of the polymer measured by gel permeation chromatography (GPC) was 1 million;

[0076] Preparation of component B: Preparation of partially blocked curing agent (b)

[0077] In a reaction vessel equipped with a stirring device, a reflux condenser, a thermometer and a nitrogen tube, 240 g of HT600 was added, stirring was started, and heating was started under nitrogen flow. The temperature in the reaction vessel was adjusted to 50° C. After the temperature in the reaction vessel was stable, methyl ethyl ketone oxime was added dropwise. The reaction temperature was maintained at no more than 55° C. The addition time was 30 minutes, and a total of 60 g was added dropwise. During the reaction, stirring was continued to react, and finally a partially blocked curing agent (b) was obtained, in which the isocyanate group blocking ratio was 50%.

[0078] Preparation of adhesive films for performance evaluation

[0079] The acrylate polymer (a) and the partially blocked curing agent (b) dispersed in the ethyl acetate solvent are uniformly mixed, wherein the weight ratio of the acrylate polymer (a) to the partially blocked curing agent (b) is 9.5:0.5. The acrylate polymer (a) is uniformly coated on the release film by a manual wire rod coating method, and the film is dried at 60°C for 2 hours, and the thickness of the film after drying is controlled to be 30±2μm. The film on the release film is transferred to the triacetate resin film, the release film is torn off, and a protective release film is covered on the adhesive layer. The triacetate resin film with the adhesive layer is cut into a size of 20cm×30cm, and the release film is torn off and pasted on the glass plate, and pressed. The glass plate with the triacetate resin film is placed under 100°C and 5 atmospheres for 20 minutes of high pressure treatment, and then left to stand for 6 hours in an environment of 100°C / 50%RH to prepare an optical component for performance evaluation.

[0080] Example 3

[0081] The two-component acrylic adhesive for optical components was prepared as follows:

[0082] Preparation of Component A: Preparation of Acrylate Polymer (a)

[0083] In a reaction vessel equipped with a stirring device, a reflux condenser, a thermometer and a nitrogen tube, 365 g of solvent ethyl acetate and 86.22 g of benzyl acrylate, 175 g of n-butyl acrylate, 10 g of 2-hydroxyethyl acrylate, 5 g of acrylic acid, and 0.275 g of a reactive hindered phenol light stabilizer were added, stirring was started, and the air in the reaction vessel was replaced with nitrogen. After 10 minutes, heating was started and the temperature in the reaction vessel was adjusted to 65° C. After the temperature in the reaction vessel was stable, 0.15 g of initiator tert-butyl pivalate was added to the reaction vessel at one time, and a polymerization reaction was carried out at 65° C. for 3 hours;

[0084] After the polymerization reaction was completed, the temperature in the reaction vessel was maintained at 62°C, 331 g of ethyl acetate was added to the reaction vessel under stirring, stirred for 10 minutes, and then cooled to room temperature to obtain an acrylate polymer (a) dispersed in ethyl acetate solvent. The weight average molecular weight (Mw) of the polymer measured by gel permeation chromatography (GPC) was 2 million;

[0085] Preparation of component B: Preparation of partially blocked curing agent (b)

[0086] In a reaction vessel equipped with a stirring device, a reflux condenser, a thermometer and a nitrogen tube, 240 g of HT600 was added, stirring was started, and heating was started under nitrogen flow. The temperature in the reaction vessel was adjusted to 50° C. After the temperature in the reaction vessel was stable, methyl ethyl ketone oxime was added dropwise. The reaction temperature was maintained at no more than 55° C. The addition time was 30 minutes, and a total of 60 g was added dropwise. During the reaction, stirring was continued to react, and finally a partially blocked curing agent (b) was obtained, in which the isocyanate group blocking ratio was 50%.

[0087] Preparation of adhesive films for performance evaluation

[0088] The acrylate polymer (a) and the partially blocked curing agent (b) dispersed in the ethyl acetate solvent are uniformly mixed, wherein the weight ratio of the acrylate polymer (a) to the partially blocked curing agent (b) is 9.5:0.5. The acrylate polymer (a) is uniformly coated on the release film by a manual wire rod coating method, and the film is dried at 60°C for 2 hours, and the thickness of the film after drying is controlled to be 30±2μm. The film on the release film is transferred to the triacetate resin film, the release film is torn off, and a protective release film is covered on the adhesive layer. The triacetate resin film with the adhesive layer is cut into a size of 20cm×30cm, and the release film is torn off and pasted on the glass plate, and pressed. The glass plate with the triacetate resin film is placed under 100°C and 5 atmospheres for 20 minutes of high pressure treatment, and then left to stand for 6 hours in an environment of 100°C / 50%RH to prepare an optical component for performance evaluation.

[0089] Example 4

[0090] The two-component acrylic adhesive for optical components was prepared as follows:

[0091] Preparation of Component A: Preparation of Acrylate Polymer (a)

[0092] In a reaction vessel equipped with a stirring device, a reflux condenser, a thermometer and a nitrogen tube, 365 g of solvent ethyl acetate and 86.22 g of benzyl acrylate, 175 g of n-butyl acrylate, 10 g of 2-hydroxyethyl acrylate, 5 g of acrylic acid, and 0.275 g of a reactive hindered phenol light stabilizer were added, stirring was started, and the air in the reaction vessel was replaced with nitrogen. After 10 minutes, heating was started and the temperature in the reaction vessel was adjusted to 65° C. After the temperature in the reaction vessel was stable, 0.28 g of initiator tert-butyl pivalate was added to the reaction vessel at one time, and a polymerization reaction was carried out at 65° C. for 3 hours;

[0093] After the polymerization reaction was completed, the temperature in the reaction vessel was maintained at 62°C, 331 g of ethyl acetate was added to the reaction vessel under stirring, stirred for 10 minutes, and then cooled to room temperature to obtain an acrylate polymer (a) dispersed in ethyl acetate solvent. The weight average molecular weight (Mw) of the polymer measured by gel permeation chromatography (GPC) was 1.6 million;

[0094] Preparation of component B: Preparation of partially blocked curing agent (b)

[0095] In a reaction vessel equipped with a stirring device, a reflux condenser, a thermometer and a nitrogen tube, 240 g of HT600 was added, stirring was started, and heating was started under nitrogen flow. The temperature in the reaction vessel was adjusted to 50° C. After the temperature in the reaction vessel was stable, methyl ethyl ketone oxime was added dropwise. The reaction temperature was maintained at no more than 55° C. The addition time was 30 minutes, and a total of 45 g was added dropwise. During the reaction, stirring was continued to react, and a partially blocked curing agent (b) was finally obtained, wherein the isocyanate group blocking ratio was 40%.

[0096] Preparation of adhesive films for performance evaluation

[0097] The acrylate polymer (a) and the partially blocked curing agent (b) dispersed in the ethyl acetate solvent are mixed uniformly, wherein the weight ratio of the acrylate polymer (a) to the partially blocked curing agent (b) is 9.5:0.5. The acrylate polymer (a) is evenly coated on the release film by a manual wire rod coating method, and the film is dried at 60°C for 2 hours, and the thickness of the film after drying is controlled to be 30±2μm. The film on the release film is transferred to the triacetate resin film, the release film is torn off, and a protective release film is covered on the adhesive layer. The triacetate resin film with the adhesive layer is cut into a size of 20cm×30cm, and the release film is torn off and pasted on the glass plate, and pressed. The glass plate with the triacetate resin film is placed under 100°C and 5 atmospheres for 20 minutes of high pressure treatment, and then left to stand for 6 hours in an environment of 100°C / 50%RH to prepare an optical component for performance evaluation.

[0098] Example 5

[0099] The two-component acrylic adhesive for optical components was prepared as follows:

[0100] Preparation of Component A: Preparation of Acrylate Polymer (a)

[0101] In a reaction vessel equipped with a stirring device, a reflux condenser, a thermometer and a nitrogen tube, 365 g of solvent ethyl acetate and 86.22 g of benzyl acrylate, 175 g of n-butyl acrylate, 10 g of 2-hydroxyethyl acrylate, 5 g of acrylic acid, and 0.275 g of a reactive hindered phenol light stabilizer were added, stirring was started, and the air in the reaction vessel was replaced with nitrogen. After 10 minutes, heating was started and the temperature in the reaction vessel was adjusted to 65° C. After the temperature in the reaction vessel was stable, 0.28 g of initiator tert-butyl pivalate was added to the reaction vessel at one time, and a polymerization reaction was carried out at 65° C. for 3 hours;

[0102] After the polymerization reaction was completed, the temperature in the reaction vessel was maintained at 62°C, 331 g of ethyl acetate was added to the reaction vessel under stirring, stirred for 10 minutes, and then cooled to room temperature to obtain an acrylate polymer (a) dispersed in ethyl acetate solvent. The weight average molecular weight (Mw) of the polymer measured by gel permeation chromatography (GPC) was 1.6 million;

[0103] B. Preparation of partially blocked curing agent (b)

[0104] In a reaction vessel equipped with a stirring device, a reflux condenser, a thermometer and a nitrogen tube, 240 g of HT600 was added, stirring was started, and heating was started under nitrogen flow. The temperature in the reaction vessel was adjusted to 50° C. After the temperature in the reaction vessel stabilized, methyl ethyl ketone oxime was added dropwise. The reaction temperature was maintained at no more than 55° C. The addition time was 30 minutes, and a total of 70 g was added dropwise. During the reaction, stirring was continued to react, and a partially blocked curing agent (b) was finally obtained, wherein the blocking ratio of the isocyanate group was 60%.

[0105] Preparation of adhesive films for performance evaluation

[0106] The acrylate polymer (a) and the partially blocked curing agent (b) dispersed in the ethyl acetate solvent are uniformly mixed, wherein the weight ratio of the acrylate polymer (a) to the partially blocked curing agent (b) is 9.5:0.5. The acrylate polymer (a) is uniformly coated on the release film by a manual wire rod coating method, and the film is dried at 60°C for 2 hours, and the thickness of the film after drying is controlled to be 30±2μm. The film on the release film is transferred to the triacetate resin film, the release film is torn off, and a protective release film is covered on the adhesive layer. The triacetate resin film with the adhesive layer is cut into a size of 20cm×30cm, and the release film is torn off and pasted on the glass plate, and pressed. The glass plate with the triacetate resin film is placed under 100°C and 5 atmospheres for 20 minutes of high pressure treatment, and then left to stand for 6 hours in an environment of 100°C / 50%RH to prepare an optical component for performance evaluation.

[0107] Comparative Example 1

[0108] The same operation as in Example 1 was performed except that no reactive hindered phenol light stabilizer was added during the preparation of Component A.

[0109] More specifically, the two-component adhesive was prepared as follows:

[0110] Preparation of Component A: Preparation of Acrylate Polymer

[0111] In a reaction vessel equipped with a stirring device, a reflux condenser, a thermometer and a nitrogen tube, 365 g of solvent ethyl acetate and 86.22 g of benzyl acrylate, 175 g of n-butyl acrylate, 10 g of 2-hydroxyethyl acrylate and 5 g of acrylic acid were added, stirring was started, and the air in the reaction vessel was replaced with nitrogen. After 10 minutes, heating was started and the temperature in the reaction vessel was adjusted to 65° C. After the temperature in the reaction vessel was stable, 0.28 g of initiator tert-butyl pivalate was added to the reaction vessel at one time, and a polymerization reaction was carried out at 65° C. for 3 hours;

[0112] After the polymerization reaction was completed, the temperature in the reaction vessel was maintained at 62°C, 331 g of ethyl acetate was added to the reaction vessel under stirring, stirred for 10 minutes, and then cooled to room temperature to obtain an acrylate polymer dispersed in ethyl acetate solvent. The weight average molecular weight (Mw) of the polymer measured by gel permeation chromatography (GPC) was 1.6 million;

[0113] Preparation of component B: Preparation of partially blocked curing agent

[0114] In a reaction vessel equipped with a stirring device, a reflux condenser, a thermometer and a nitrogen tube, 240g HT600 was added, stirring was started, heating was started under nitrogen flow, and the temperature in the reaction vessel was adjusted to 50°C. After the temperature in the reaction vessel was stable, methyl ethyl ketone oxime was added dropwise. The reaction temperature was maintained at no more than 55°C during the addition process. The addition time was 30 minutes, and a total of 60g was added dropwise. During the reaction, stirring was continued to react, and a partially blocked curing agent was finally obtained, in which the blocking ratio of the isocyanate group was 50%.

[0115] Preparation of adhesive films for performance evaluation

[0116] The acrylate polymer and the partially blocked curing agent dispersed in the ethyl acetate solvent are mixed uniformly, wherein the weight ratio of the acrylate polymer to the partially blocked curing agent is 9.5:0.5. The release film is evenly coated on the release film by a manual wire rod coating method, and the film is dried at 60°C for 2 hours, and the thickness of the film after drying is controlled to be 30±2μm. The film on the release film is transferred to the triacetate resin film, the release film is torn off, and a protective release film is covered on the adhesive layer. The triacetate resin film with the adhesive layer is cut into a size of 20cm×30cm, and the release film is torn off and pasted on the glass plate, and pressed. The glass plate with the triacetate resin film is placed under 100°C and 5 atmospheres for 20 minutes of high pressure treatment, and then left to stand for 6 hours in an environment of 100°C / 50%RH to prepare an optical component for performance evaluation.

[0117] Comparative Example 2

[0118] The same operation as in Example 1 was performed except that all trimers in component B were blocked.

[0119] More specifically, a two-component acrylate adhesive was prepared as follows:

[0120] Preparation of Component A: Preparation of Acrylate Polymer

[0121] In a reaction vessel equipped with a stirring device, a reflux condenser, a thermometer and a nitrogen tube, 365 g of solvent ethyl acetate and 86.22 g of benzyl acrylate, 175 g of n-butyl acrylate, 10 g of 2-hydroxyethyl acrylate, 5 g of acrylic acid, and 0.275 g of a reactive hindered phenol light stabilizer were added, stirring was started, and the air in the reaction vessel was replaced with nitrogen. After 10 minutes, heating was started and the temperature in the reaction vessel was adjusted to 65° C. After the temperature in the reaction vessel was stable, 0.28 g of initiator tert-butyl pivalate was added to the reaction vessel at one time, and a polymerization reaction was carried out at 65° C. for 3 hours;

[0122] After the polymerization reaction was completed, the temperature in the reaction vessel was maintained at 62°C, 331 g of ethyl acetate was added to the reaction vessel under stirring, stirred for 10 minutes, and then cooled to room temperature to obtain an acrylate polymer dispersed in ethyl acetate solvent. The weight average molecular weight (Mw) of the polymer measured by gel permeation chromatography (GPC) was 1.6 million;

[0123] Preparation of component B: Preparation of all blocked curing agents

[0124] In a reaction vessel equipped with a stirring device, a reflux condenser, a thermometer and a nitrogen tube, 240g HT600 was added, stirring was started, and heating was started under nitrogen flow. The temperature in the reaction vessel was adjusted to 50°C. After the temperature in the reaction vessel was stable, methyl ethyl ketone oxime was added dropwise. The reaction temperature was maintained at no more than 55°C during the addition process. The addition time was 30 minutes, and a total of 115g was added dropwise. During the reaction, stirring was continued to react, and a blocked curing agent was finally obtained, in which the isocyanate group blocking ratio was 100%.

[0125] Preparation of adhesive films for performance evaluation

[0126] The acrylate polymer and all the blocked curing agents dispersed in the ethyl acetate solvent are mixed uniformly, wherein the weight ratio of the acrylate polymer to the all the blocked curing agents is 9.5:0.5. The release film is evenly coated on the release film by a manual wire rod coating method, and the film is dried at 60°C for 2 hours, and the thickness of the film after drying is controlled to be 30±2μm. The film on the release film is transferred to the triacetate resin film, the release film is torn off, and a protective release film is covered on the adhesive layer. The triacetate resin film with the adhesive layer is cut into a size of 20cm×30cm, and the release film is torn off and pasted on the glass plate, and pressed. The glass plate with the triacetate resin film is placed under 100°C and 5 atmospheres for 20 minutes of high pressure treatment, and then left to stand for 6 hours in an environment of 100°C / 50%RH to prepare the optical component for performance evaluation.

[0127] Comparative Example 3

[0128] The operation was carried out in the same manner as in Example 1, except that component B was a non-blocked curing agent.

[0129] More specifically, a two-component acrylate adhesive was prepared as follows:

[0130] Preparation of Component A: Preparation of Acrylate Polymer

[0131] In a reaction vessel equipped with a stirring device, a reflux condenser, a thermometer and a nitrogen tube, 365 g of solvent ethyl acetate and 86.22 g of benzyl acrylate, 175 g of n-butyl acrylate, 10 g of 2-hydroxyethyl acrylate, 5 g of acrylic acid, and 0.275 g of a reactive hindered phenol light stabilizer were added, stirring was started, and the air in the reaction vessel was replaced with nitrogen. After 10 minutes, heating was started and the temperature in the reaction vessel was adjusted to 65° C. After the temperature in the reaction vessel was stable, 0.28 g of initiator tert-butyl pivalate was added to the reaction vessel at one time, and a polymerization reaction was carried out at 65° C. for 3 hours;

[0132] After the polymerization reaction was completed, the temperature in the reaction vessel was maintained at 62°C, 331 g of ethyl acetate was added to the reaction vessel under stirring, stirred for 10 minutes, and then cooled to room temperature to obtain an acrylate polymer dispersed in ethyl acetate solvent. The weight average molecular weight (Mw) of the polymer measured by gel permeation chromatography (GPC) was 1.6 million;

[0133] Preparation of component B: Use HT600 as component B

[0134] Preparation of adhesive films for performance evaluation

[0135] The acrylate polymer and HT600 dispersed in the ethyl acetate solvent are mixed evenly, wherein the weight ratio of the acrylate polymer to HT600 is 9.5:0.5. The acrylate polymer is evenly coated on the release film by a manual wire rod coating method, and the film is dried at 60°C for 2 hours, and the thickness of the film after drying is controlled to be 30±2μm. The film on the release film is transferred to the triacetate resin film, the release film is torn off, and a protective release film is covered on the adhesive layer. The triacetate resin film with the adhesive layer is cut into a size of 20cm×30cm, and the release film is torn off and pasted on the glass plate, and pressed. The glass plate with the triacetate resin film is placed under 100°C and 5 atmospheres for 20 minutes of high pressure treatment, and then left to stand for 6 hours in an environment of 100°C / 50%RH to prepare the optical component for performance evaluation.

[0136] Comparative Example 4

[0137] The same operation as in Example 1 was performed except that a mixed type light stabilizer was used in place of the radical polymerizable hindered amine light stabilizer during the preparation of Component A.

[0138] More specifically, a two-component acrylate adhesive was prepared as follows:

[0139] Preparation of Component A: Preparation of Acrylate Polymer

[0140] In a reaction vessel equipped with a stirring device, a reflux condenser, a thermometer and a nitrogen tube, 365 g of solvent ethyl acetate and 86.22 g of benzyl acrylate, 175 g of n-butyl acrylate, 10 g of 2-hydroxyethyl acrylate and 5 g of acrylic acid were added, stirring was started, and the air in the reaction vessel was replaced with nitrogen. After 10 minutes, heating was started and the temperature in the reaction vessel was adjusted to 65° C. After the temperature in the reaction vessel was stable, 0.28 g of initiator tert-butyl pivalate was added to the reaction vessel at one time, and a polymerization reaction was carried out at 65° C. for 3 hours;

[0141] After the polymerization reaction was completed, the temperature in the reaction vessel was maintained at 62°C, 331 g of ethyl acetate and 0.27 g of 1024 light stabilizer were added to the reaction vessel under stirring, stirred for 10 min, and then cooled to room temperature to obtain an acrylate polymer dispersed in ethyl acetate solvent. The weight average molecular weight (Mw) of the polymer measured by gel permeation chromatography (GPC) was 1.6 million;

[0142] Preparation of component B: Preparation of partially blocked curing agent

[0143] In a reaction vessel equipped with a stirring device, a reflux condenser, a thermometer and a nitrogen tube, 240g HT600 was added, stirring was started, heating was started under nitrogen flow, and the temperature in the reaction vessel was adjusted to 50°C. After the temperature in the reaction vessel was stable, methyl ethyl ketone oxime was added dropwise. The reaction temperature was maintained at no more than 55°C during the addition process. The addition time was 30 minutes, and a total of 60g was added dropwise. During the reaction, stirring was continued to react, and a partially blocked curing agent was finally obtained, in which the blocking ratio of the isocyanate group was 50%.

[0144] Preparation of adhesive films for performance evaluation

[0145] The acrylate polymer and the partially blocked curing agent dispersed in the ethyl acetate solvent are mixed uniformly, wherein the weight ratio of the acrylate polymer to the partially blocked curing agent is 9.5:0.5. The release film is evenly coated on the release film by a manual wire rod coating method, and the film is dried at 60°C for 2 hours, and the thickness of the film after drying is controlled to be 30±2μm. The film on the release film is transferred to the triacetate resin film, the release film is torn off, and a protective release film is covered on the adhesive layer. The triacetate resin film with the adhesive layer is cut into a size of 20cm×30cm, and the release film is torn off and pasted on the glass plate, and pressed. The glass plate with the triacetate resin film is placed under 100°C and 5 atmospheres for 20 minutes of high pressure treatment, and then left to stand for 6 hours in an environment of 100°C / 50%RH to prepare an optical component for performance evaluation.

[0146] Comparative Example 5

[0147] The same operation as in Example 1 was performed except that a mixture of partially blocked and unblocked trimers was used instead of the blocked curing agent during the preparation of the film.

[0148] More specifically, a two-component acrylate adhesive was prepared as follows:

[0149] Preparation of Component A: Preparation of Acrylate Polymer

[0150] In a reaction vessel equipped with a stirring device, a reflux condenser, a thermometer and a nitrogen tube, 365 g of solvent ethyl acetate and 86.22 g of benzyl acrylate, 175 g of n-butyl acrylate, 10 g of 2-hydroxyethyl acrylate and 5 g of acrylic acid were added, stirring was started, and the air in the reaction vessel was replaced with nitrogen. After 10 minutes, heating was started and the temperature in the reaction vessel was adjusted to 65° C. After the temperature in the reaction vessel was stable, 0.28 g of initiator tert-butyl pivalate was added to the reaction vessel at one time, and a polymerization reaction was carried out at 65° C. for 3 hours;

[0151] After the polymerization reaction was completed, the temperature in the reaction vessel was maintained at 62°C, 331 g of ethyl acetate and 0.27 g of 1024 light stabilizer were added to the reaction vessel under stirring, stirred for 10 min, and then cooled to room temperature to obtain an acrylate polymer dispersed in ethyl acetate solvent. The weight average molecular weight (Mw) of the polymer measured by gel permeation chromatography (GPC) was 1.6 million;

[0152] Preparation of component B: Preparation of partially blocked curing agent

[0153] In a reaction vessel equipped with a stirring device, a reflux condenser, a thermometer and a nitrogen tube, 240g HT600 was added, stirring was started, heating was started under nitrogen flow, and the temperature in the reaction vessel was adjusted to 50°C. After the temperature in the reaction vessel was stable, methyl ethyl ketone oxime was added dropwise. The reaction temperature was maintained at no more than 55°C during the addition process. The addition time was 30 minutes, and a total of 60g was added dropwise. During the reaction, stirring was continued to react, and a partially blocked curing agent was finally obtained, in which the blocking ratio of the isocyanate group was 50%.

[0154] Preparation of adhesive films for performance evaluation

[0155] The acrylate polymer and partially blocked curing agent dispersed in ethyl acetate solvent and the unblocked HT600 trimer are mixed evenly, wherein the mass ratio of the acrylate polymer, the partially blocked curing agent prepared above and the HT600 trimer is 9.5:0.25:0.25. The release film is evenly coated on the release film by manual wire rod coating, and the film is dried at 60°C for 2 hours, and the thickness of the film after drying is controlled to be 30±2μm. The film on the release film is transferred to the triacetate resin film, the release film is torn off, and a protective release film is covered on the adhesive layer. The triacetate resin film with the adhesive layer is cut into a size of 20cm×30cm, and the release film is torn off and pasted on the glass plate, and pressed. The glass plate with the triacetate resin film is placed under 100°C and 5 atmospheres for 20 minutes of high pressure treatment, and then left to stand for 6 hours in an environment of 100°C / 50%RH to prepare the optical component for performance evaluation.

[0156] Comparative Example 6

[0157] The same operation as in Example 1 was performed except that the film was prepared under the conditions of 60° C. and 5 atmospheres for 20 minutes of high pressure treatment and then allowed to stand in an environment of 60° C. / 50% RH for 12 hours.

[0158] More specifically, a two-component acrylate adhesive was prepared as follows:

[0159] Preparation of Component A: Preparation of Acrylate Polymer

[0160] In a reaction vessel equipped with a stirring device, a reflux condenser, a thermometer and a nitrogen tube, 365 g of solvent ethyl acetate and 86.22 g of benzyl acrylate, 175 g of n-butyl acrylate, 10 g of 2-hydroxyethyl acrylate, 5 g of acrylic acid, and 0.275 g of a reactive hindered phenol light stabilizer were added, stirring was started, and the air in the reaction vessel was replaced with nitrogen. After 10 minutes, heating was started and the temperature in the reaction vessel was adjusted to 65° C. After the temperature in the reaction vessel was stable, 0.28 g of initiator tert-butyl pivalate was added to the reaction vessel at one time, and a polymerization reaction was carried out at 65° C. for 3 hours;

[0161] After the polymerization reaction was completed, the temperature in the reaction vessel was maintained at 62°C, 331 g of ethyl acetate was added to the reaction vessel under stirring, stirred for 10 minutes, and then cooled to room temperature to obtain an acrylate polymer dispersed in ethyl acetate solvent. The weight average molecular weight (Mw) of the polymer measured by gel permeation chromatography (GPC) was 1.6 million;

[0162] Preparation of component B: Preparation of blocked curing agent

[0163] In a reaction vessel equipped with a stirring device, a reflux condenser, a thermometer and a nitrogen tube, 240g HT600 was added, stirring was started, heating was started under nitrogen flow, and the temperature in the reaction vessel was adjusted to 50°C. After the temperature in the reaction vessel was stable, methyl ethyl ketone oxime was added dropwise. The reaction temperature was maintained at no more than 55°C during the addition process. The addition time was 30 minutes, and a total of 60g was added dropwise. During the reaction, stirring was continued to react, and a partially blocked curing agent was finally obtained, in which the blocking ratio of the isocyanate group was 50%.

[0164] Preparation of adhesive films for performance evaluation

[0165] The acrylate polymer and the partially blocked curing agent dispersed in the ethyl acetate solvent are mixed uniformly, wherein the weight ratio of the acrylate polymer to the partially blocked curing agent is 9.5:0.5. The release film is evenly coated on the release film by a manual wire rod coating method, and the film is dried at 60°C for 2 hours, and the thickness of the film after drying is controlled to be 30±2μm. The film on the release film is transferred to the triacetate resin film, the release film is torn off, and a protective release film is covered on the adhesive layer. The triacetate resin film with the adhesive layer is cut into a size of 20cm×30cm, and the release film is torn off and pasted on the glass plate, and pressed. The glass plate with the triacetate resin film is placed under 60°C and 5 atmospheres for 20 minutes of high pressure treatment, and then left to stand for 12 hours in an environment of 60°C / 50%RH to prepare an optical component for performance evaluation.

[0166] Comparative Example 7

[0167] The same operation as in Example 1 was performed except that the conditions during the preparation of the film were changed to aging at 100°C.

[0168] More specifically, a two-component acrylate adhesive was prepared as follows:

[0169] Preparation of Component A: Preparation of Acrylate Polymer

[0170] In a reaction vessel equipped with a stirring device, a reflux condenser, a thermometer and a nitrogen tube, 365 g of solvent ethyl acetate and 86.22 g of benzyl acrylate, 175 g of n-butyl acrylate, 10 g of 2-hydroxyethyl acrylate, 5 g of acrylic acid, and 0.275 g of a reactive hindered phenol light stabilizer were added, stirring was started, and the air in the reaction vessel was replaced with nitrogen. After 10 minutes, heating was started and the temperature in the reaction vessel was adjusted to 65° C. After the temperature in the reaction vessel was stable, 0.28 g of initiator tert-butyl pivalate was added to the reaction vessel at one time, and a polymerization reaction was carried out at 65° C. for 3 hours;

[0171] After the polymerization reaction was completed, the temperature in the reaction vessel was maintained at 62°C, 331 g of ethyl acetate was added to the reaction vessel under stirring, stirred for 10 minutes, and then cooled to room temperature to obtain an acrylate polymer dispersed in ethyl acetate solvent. The weight average molecular weight (Mw) of the polymer measured by gel permeation chromatography (GPC) was 1.6 million;

[0172] Preparation of component B: Preparation of partially blocked curing agent

[0173] In a reaction vessel equipped with a stirring device, a reflux condenser, a thermometer and a nitrogen tube, 240g HT600 was added, stirring was started, and heating was started under nitrogen flow. The temperature in the reaction vessel was adjusted to 50°C. After the temperature in the reaction vessel was stable, methyl ethyl ketone oxime was added dropwise. The reaction temperature was maintained at no more than 55°C during the addition process. The addition time was 30 minutes, and a total of 60g was added dropwise. During the reaction, stirring was continued to react, and a blocked curing agent was finally obtained, in which the isocyanate group blocking ratio was 50%.

[0174] Preparation of adhesive films for performance evaluation

[0175] The acrylic polymer and the blocked curing agent dispersed in the ethyl acetate solvent are mixed uniformly, wherein the weight ratio of the acrylic polymer to the partially blocked curing agent is 9.5:0.5. The release film is evenly coated on the release film by a manual wire rod coating method, and the film is dried at 100°C for 2 hours, and the thickness of the film after drying is controlled to be 30±2μm. The film on the release film is transferred to the triacetate resin film, the release film is torn off, and a protective release film is covered on the adhesive layer. The triacetate resin film with the adhesive layer is cut into a size of 20cm×30cm, and the release film is torn off and pasted on the glass plate, and pressed. The glass plate with the triacetate resin film is placed under 100°C and 5 atmospheres for 20 minutes of high pressure treatment, and then left to stand for 6 hours in an environment of 100°C / 50%RH to prepare an optical component for performance evaluation.

[0176] Comparative Example 8 (the blocking ratio of the partially blocked curing agent is 30%)

[0177] The two-component acrylic adhesive for optical components was prepared as follows:

[0178] Preparation of Component A: Preparation of Acrylate Polymer

[0179] In a reaction vessel equipped with a stirring device, a reflux condenser, a thermometer and a nitrogen tube, 365 g of solvent ethyl acetate and 86.22 g of benzyl acrylate, 175 g of n-butyl acrylate, 10 g of 2-hydroxyethyl acrylate, 5 g of acrylic acid, and 0.275 g of a reactive hindered phenol light stabilizer were added, stirring was started, and the air in the reaction vessel was replaced with nitrogen. After 10 minutes, heating was started and the temperature in the reaction vessel was adjusted to 65° C. After the temperature in the reaction vessel was stable, 0.28 g of initiator tert-butyl pivalate was added to the reaction vessel at one time, and a polymerization reaction was carried out at 65° C. for 3 hours;

[0180] After the polymerization reaction was completed, the temperature in the reaction vessel was maintained at 62°C, 331 g of ethyl acetate was added to the reaction vessel under stirring, stirred for 10 minutes, and then cooled to room temperature to obtain an acrylate polymer dispersed in ethyl acetate solvent. The weight average molecular weight (Mw) of the polymer measured by gel permeation chromatography (GPC) was 1.6 million;

[0181] Preparation of component B: Preparation of partially blocked curing agent

[0182] In a reaction vessel equipped with a stirring device, a reflux condenser, a thermometer and a nitrogen tube, 240g HT600 was added, stirring was started, and heating was started under nitrogen flow. The temperature in the reaction vessel was adjusted to 50°C. After the temperature in the reaction vessel was stable, methyl ethyl ketone oxime was added dropwise. The reaction temperature was maintained at no more than 55°C during the addition process. The addition time was 30 minutes, and a total of 35g was added dropwise. During the reaction, stirring was continued to react, and a partially blocked curing agent was finally obtained, in which the isocyanate group blocking ratio was 30%.

[0183] Preparation of adhesive films for performance evaluation

[0184] The acrylate polymer and the partially blocked curing agent dispersed in the ethyl acetate solvent are mixed uniformly, wherein the weight ratio of the acrylate polymer to the partially blocked curing agent is 9.5:0.5. The release film is evenly coated on the release film by a manual wire rod coating method, and the film is dried at 60°C for 2 hours, and the thickness of the film after drying is controlled to be 30±2μm. The film on the release film is transferred to the triacetate resin film, the release film is torn off, and a protective release film is covered on the adhesive layer. The triacetate resin film with the adhesive layer is cut into a size of 20cm×30cm, and the release film is torn off and pasted on the glass plate, and pressed. The glass plate with the triacetate resin film is placed under 100°C and 5 atmospheres for 20 minutes of high pressure treatment, and then left to stand for 6 hours in an environment of 100°C / 50%RH to prepare an optical component for performance evaluation.

[0185] Comparative Example 9 (the blocking ratio of the partially blocked curing agent is 70%)

[0186] The two-component acrylic adhesive for optical components was prepared as follows:

[0187] Preparation of Component A: Preparation of Acrylate Polymer

[0188] In a reaction vessel equipped with a stirring device, a reflux condenser, a thermometer and a nitrogen tube, 365 g of solvent ethyl acetate and 86.22 g of benzyl acrylate, 175 g of n-butyl acrylate, 10 g of 2-hydroxyethyl acrylate, 5 g of acrylic acid, and 0.275 g of a reactive hindered phenol light stabilizer were added, stirring was started, and the air in the reaction vessel was replaced with nitrogen. After 10 minutes, heating was started and the temperature in the reaction vessel was adjusted to 65° C. After the temperature in the reaction vessel was stable, 0.28 g of initiator tert-butyl pivalate was added to the reaction vessel at one time, and a polymerization reaction was carried out at 65° C. for 3 hours;

[0189] After the polymerization reaction was completed, the temperature in the reaction vessel was maintained at 62°C, 331 g of ethyl acetate was added to the reaction vessel under stirring, stirred for 10 minutes, and then cooled to room temperature to obtain an acrylate polymer dispersed in ethyl acetate solvent. The weight average molecular weight (Mw) of the polymer measured by gel permeation chromatography (GPC) was 1.6 million;

[0190] Preparation of component B: Preparation of partially blocked curing agent

[0191] In a reaction vessel equipped with a stirring device, a reflux condenser, a thermometer and a nitrogen tube, 240g HT600 was added, stirring was started, heating was started under nitrogen conditions, and the temperature in the reaction vessel was adjusted to 50°C. After the temperature in the reaction vessel was stable, methyl ethyl ketone oxime was added dropwise. During the addition, the reaction temperature was maintained at no more than 55°C. The addition time was 30 minutes, and a total of 80g was added dropwise. During the reaction, stirring was continued to react, and a partially blocked curing agent was finally obtained, in which the isocyanate group blocking ratio was 70%.

[0192] Preparation of adhesive films for performance evaluation

[0193] The acrylate polymer and the partially blocked curing agent dispersed in the ethyl acetate solvent are mixed uniformly, wherein the weight ratio of the acrylate polymer to the partially blocked curing agent is 9.5:0.5. The release film is evenly coated on the release film by a manual wire rod coating method, and the film is dried at 60°C for 2 hours, and the thickness of the film after drying is controlled to be 30±2μm. The film on the release film is transferred to the triacetate resin film, the release film is torn off, and a protective release film is covered on the adhesive layer. The triacetate resin film with the adhesive layer is cut into a size of 20cm×30cm, and the release film is torn off and pasted on the glass plate, and pressed. The glass plate with the triacetate resin film is placed under 100°C and 5 atmospheres for 20 minutes of high pressure treatment, and then left to stand for 6 hours in an environment of 100°C / 50%RH to prepare an optical component for performance evaluation.

[0194] Comparative Example 10 (Excess of (meth)acrylic acid)

[0195] The two-component acrylic adhesive for optical components was prepared as follows:

[0196] Preparation of Component A: Preparation of Acrylate Polymer

[0197] In a reaction vessel equipped with a stirring device, a reflux condenser, a thermometer and a nitrogen tube, 365g of solvent ethyl acetate and 86.22g of benzyl acrylate, 175g of n-butyl acrylate, 10g of 2-hydroxyethyl acrylate, 10g of acrylic acid, and 0.275g of a reactive hindered phenol light stabilizer (commercially available, Aidico hindered phenol light stabilizer LA-82, unless otherwise specified, other embodiments use the same reactive hindered phenol light stabilizer), stirring is started, and the air in the reaction vessel is replaced with nitrogen. After 10 minutes, heating is started, and the temperature in the reaction vessel is adjusted to 65°C. After the temperature in the reaction vessel is stable, 0.28g of an initiator tert-butyl pivalate is added to the reaction vessel at one time, and a polymerization reaction is carried out at 65°C for 3h;

[0198] After the polymerization reaction was completed, the temperature in the reaction vessel was maintained at 62°C, 331 g of ethyl acetate was added to the reaction vessel under stirring, stirred for 10 minutes, and then cooled to room temperature to obtain an acrylate polymer dispersed in ethyl acetate solvent. The weight average molecular weight (Mw) of the polymer measured by gel permeation chromatography (GPC) was 1.6 million;

[0199] Preparation of component B: Preparation of partially blocked curing agent

[0200] In a reaction vessel equipped with a stirring device, a reflux condenser, a thermometer and a nitrogen tube, 240g of HT600 (curing agent) was added, stirring was started, and heating was started under nitrogen flow. The temperature in the reaction vessel was adjusted to 50°C. After the temperature in the reaction vessel was stable, methyl ethyl ketone oxime was added dropwise. The reaction temperature was maintained at no more than 55°C during the addition process. The addition time was 30 minutes, and a total of 60g was added dropwise. During the reaction, stirring was continued to react, and a partially blocked curing agent was finally obtained, in which the isocyanate group blocking ratio was 50%.

[0201] Preparation of adhesive films for performance evaluation

[0202] The acrylate polymer and the partially blocked curing agent dispersed in the ethyl acetate solvent are mixed uniformly, wherein the weight ratio of the acrylate polymer to the partially blocked curing agent is 9.5:0.5. The release film is evenly coated on the release film by a manual wire rod coating method, and the film is dried at 60°C for 2 hours, and the thickness of the film after drying is controlled to be 30±2μm. The film on the release film is transferred to the triacetate resin film, the release film is torn off, and a protective release film is covered on the adhesive layer. The triacetate resin film with the adhesive layer is cut into a size of 20cm×30cm, and the release film is torn off and pasted on the glass plate, and pressed. The glass plate with the triacetate resin film is placed under 100°C and 5 atmospheres for 20 minutes of high pressure treatment, and then left to stand for 6 hours in an environment of 100°C / 50%RH to prepare an optical component for performance evaluation.

[0203] Comparative Example 11 (Excessive amount of (meth)acrylate monomer containing hydroxyl group)

[0204] The two-component acrylic adhesive for optical components was prepared as follows:

[0205] Preparation of Component A: Preparation of Acrylate Polymer

[0206] In a reaction vessel equipped with a stirring device, a reflux condenser, a thermometer and a nitrogen tube, 365g of solvent ethyl acetate and 86.22g of benzyl acrylate, 175g of n-butyl acrylate, 20g of 2-hydroxyethyl acrylate, 5g of acrylic acid, and 0.275g of a reactive hindered phenol light stabilizer (commercially available, Aidico hindered phenol light stabilizer LA-82, unless otherwise specified, other embodiments use the same reactive hindered phenol light stabilizer), stirring is started, and the air in the reaction vessel is replaced with nitrogen. After 10 minutes, heating is started, and the temperature in the reaction vessel is adjusted to 65°C. After the temperature in the reaction vessel is stable, 0.28g of an initiator tert-butyl pivalate is added to the reaction vessel at one time, and a polymerization reaction is carried out at 65°C for 3h;

[0207] After the polymerization reaction was completed, the temperature in the reaction vessel was maintained at 62°C, 331 g of ethyl acetate was added to the reaction vessel under stirring, stirred for 10 minutes, and then cooled to room temperature to obtain an acrylate polymer dispersed in ethyl acetate solvent. The weight average molecular weight (Mw) of the polymer measured by gel permeation chromatography (GPC) was 1.6 million;

[0208] Preparation of component B: Preparation of partially blocked curing agent

[0209] In a reaction vessel equipped with a stirring device, a reflux condenser, a thermometer and a nitrogen tube, 240g of HT600 (curing agent) was added, stirring was started, and heating was started under nitrogen flow. The temperature in the reaction vessel was adjusted to 50°C. After the temperature in the reaction vessel was stable, methyl ethyl ketone oxime was added dropwise. The reaction temperature was maintained at no more than 55°C during the addition process. The addition time was 30 minutes, and a total of 60g was added dropwise. During the reaction, stirring was continued to react, and a partially blocked curing agent was finally obtained, in which the isocyanate group blocking ratio was 50%.

[0210] Preparation of adhesive films for performance evaluation

[0211] The acrylate polymer and the partially blocked curing agent dispersed in the ethyl acetate solvent are mixed uniformly, wherein the weight ratio of the acrylate polymer to the partially blocked curing agent is 9.5:0.5. The release film is evenly coated on the release film by a manual wire rod coating method, and the film is dried at 60°C for 2 hours, and the thickness of the film after drying is controlled to be 30±2μm. The film on the release film is transferred to the triacetate resin film, the release film is torn off, and a protective release film is covered on the adhesive layer. The triacetate resin film with the adhesive layer is cut into a size of 20cm×30cm, and the release film is torn off and pasted on the glass plate, and pressed. The glass plate with the triacetate resin film is placed under 100°C and 5 atmospheres for 20 minutes of high pressure treatment, and then left to stand for 6 hours in an environment of 100°C / 50%RH to prepare an optical component for performance evaluation.

[0212] According to the above test method, the performance of the samples provided in Examples 1 to 5 and Comparative Examples 1 to 11 was comprehensively evaluated, and the evaluation results are shown in Table 2 below:

[0213] Table 2: Performance evaluation data

[0214]

[0215] Each performance item is scored, with 1 to 5 representing performance from low to high, and 0 indicating loss of this performance item.

[0216] According to the performance data in Table 2 above, the embodiment is compared with comparative examples 1 and 4. The hindered phenol light stabilizer containing double bond groups is grafted onto the acrylate polymer molecular chain through polymerization reaction to form a permanent light stabilized polymer with hindered amine functional groups. This light stabilizer can well avoid the loss of light stabilizer caused by physical migration or volatilization, improve and enhance the dispersion performance and light stabilization effect of hindered amine light stabilizer in the polymer, so that the film can maintain excellent light stabilization effect in the subsequent long-term high-temperature working environment, which cannot be achieved by conventional physical mixing;

[0217] At the same time, a partially blocked curing agent is used in combination with an acrylic adhesive through a two-step aging process. In the first step of aging, the hydroxyl groups in the linear polymer acrylic resin react with the exposed isocyanate to produce a large molecular linear adhesive. During the construction and coating process, the coating is removed and cut again. The adhesive film has a certain strength and can be completely removed. After the construction is completed, it is further aged at high temperature. At this time, the blocked isocyanate is unblocked and micro-cross-linking continues. The subsequent film strength is further improved, the reliability in high temperature and high humidity environments is enhanced, and the problem of shrinkage and deformation in high humidity environments is solved; the high temperature and high humidity resistance performance is taken to a higher level.

[0218] The present invention uses the above-mentioned embodiments to illustrate a two-component acrylic adhesive for optical components and a preparation method thereof, but the present invention is not limited to the above-mentioned embodiments, that is, it does not mean that the present invention must rely on the above-mentioned embodiments to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of various raw materials of the product of the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

Claims

1. A two-component acrylic adhesive comprising component A and component B, wherein: Component A comprises an acrylate polymer (a) dispersed in a solvent, Component B comprises a partially blocked isocyanate curing agent (b), Wherein, the acrylic acid ester copolymer (a) is a copolymer comprising a unit derived from a (meth)acrylic acid monomer, a unit derived from a (meth)acrylic acid aryl ester monomer, a unit derived from a (meth)acrylic acid ester monomer containing a hydroxyl group, a unit derived from a (meth)acrylic acid alkyl ester monomer, and a unit derived from a free radical polymerizable hindered amine light stabilizer; The partially blocked isocyanate curing agent (b) is a reaction product of isocyanate trimer and ketoxime, and the blocking ratio of isocyanate groups therein is 35% to 65%, preferably 40% to 60%.

2. The two-component acrylate adhesive according to claim 1, wherein: The content of the acrylic ester polymer (a) is 90 to 95 parts by weight, and the content of the partially blocked isocyanate curing agent (b) is 5 to 10 parts by weight; and / or The weight average molecular weight of the acrylic acid ester polymer (a) is 1 million to 3 million, preferably 1 million to 2 million; and / or The solid content of component A is 10 wt% to 30 wt%, preferably 15 wt% to 25 wt%.

3. The two-component acrylate adhesive according to claim 1 or 2, wherein: The (meth) aryl acrylate monomer is (meth) acrylic acid C6~C 12 Aryl ester, preferably one or more selected from benzyl (meth)acrylate, phenyl (meth)acrylate, phenoxyethyl (meth)acrylate; and / or The hydroxyl-containing (meth)acrylate monomer is a (meth)acrylate hydroxy C1-C6 alkyl ester, preferably one or more selected from 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate and 6-hydroxyhexyl (meth)acrylate; and / or The (meth) acrylic acid alkyl ester is (meth) acrylic acid C1-C 12 The alkyl ester is preferably one or more selected from methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, tert-butyl (meth)acrylate, pentyl (meth)acrylate, hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, n-octyl (meth)acrylate, isooctyl (meth)acrylate, n-nonyl (meth)acrylate, isononyl (meth)acrylate, n-decyl (meth)acrylate, isodecyl (meth)acrylate, undecyl (meth)acrylate and lauryl (meth)acrylate; and / or The structure of the free radical polymerizable hindered amine light stabilizer is as follows:

4. The two-component acrylate adhesive according to any one of claims 1 to 3, wherein: The amount of the free radical polymerizable hindered amine light stabilizer is 0.01 wt% to 0.5 wt%, preferably 0.1 wt% to 0.2 wt%, relative to 100 wt% of the total weight of the monomers used in preparing component A; and / or Relative to 100wt% of the total weight of the monomers used in preparing component A, the amount of (meth)acrylic acid monomer is 1wt% to 3wt%, the amount of (meth)acrylic acid aryl ester monomer is 3wt% to 40wt%, the amount of (meth)acrylic acid ester monomer containing hydroxyl group is 3wt% to 5wt%, and the amount of (meth)acrylic acid alkyl ester is 60wt% to 70wt%; and / or The weight ratio of isocyanate trimer to ketoxime is 1 to 10:1, preferably 3.5 to 5:

1.

5. The two-component acrylate adhesive according to any one of claims 1 to 4, wherein The ketoxime is one or more selected from methyl ethyl ketone oxime, butanone oxime, acetone oxime, formaldehyde oxime, acetaldehyde oxime and cyclohexanone oxime, preferably methyl ethyl ketone oxime; and / or The isocyanate trimer is an HDI trimer; and / or The solvent in component A is one or more selected from aromatic hydrocarbon solvents, aliphatic hydrocarbon solvents, alicyclic hydrocarbon solvents, ether solvents, halogenated hydrocarbon solvents, ester solvents, ketone solvents and nitrile solvents.

6. A method for preparing a two-component acrylate adhesive according to any one of claims 1 to 5, comprising the following steps: Step 1), preparation of component A: in the presence of a solvent, an acrylic acid monomer, a (meth)acrylic acid aryl ester monomer, a (meth)acrylic acid ester monomer containing a hydroxyl group, a (meth)acrylic acid alkyl ester and a free radical polymerizable hindered amine light stabilizer are polymerized in the presence of an initiator to obtain an acrylic acid ester polymer (a); Step 2), preparation of component B: reacting an isocyanate trimer with a ketoxime to obtain a partially blocked isocyanate curing agent (b).

7. The method for preparing the two-component acrylate adhesive according to claim 6, wherein: The polymerization method in step 1) is solution polymerization; and / or The solvent in step 1) is one or more selected from aromatic hydrocarbon solvents, aliphatic hydrocarbon solvents, alicyclic hydrocarbon solvents, ether solvents, halogenated hydrocarbon solvents, ester solvents, ketone solvents and nitrile solvents.

8. The method for preparing the two-component acrylate adhesive according to claim 6 or 7, wherein: The polymerization in step 1) is carried out as follows: In an inert atmosphere, acrylic acid monomer, (meth) aryl acrylate monomer, (meth) acrylate monomer containing hydroxyl group, (meth) alkyl acrylate and free radical polymerizable hindered amine light stabilizer are added to a solvent, the temperature is raised to 60-80° C., an initiator is added, and the polymerization reaction is carried out at a constant temperature; and / or Relative to 100 wt% of the monomer, the amount of the initiator is 0.01 wt% to 0.5 wt%, preferably 0.05 wt% to 0.2 wt%; and / or The initiator is a thermal initiator and / or a redox initiator; and / or The reaction of step 2) is carried out in the following manner: In an inert atmosphere, ketone is added dropwise to the isocyanate trimer to carry out the reaction. The reaction temperature is preferably 40 to 60°C.

9. Use of the two-component acrylate adhesive according to any one of claims 1 to 5 for bonding optical parts.

10. A method for applying a two-component acrylate adhesive according to any one of claims 1 to 5, comprising the following steps: 2-1) uniformly mixing the component A and the component B to obtain an adhesive composition, wherein: The content of the acrylic ester polymer (a) in component A is 90 to 95 parts by weight, and the content of the partially blocked isocyanate curing agent (b) in component B is 5 to 10 parts by weight; 2-2) applying the adhesive composition obtained in step 2-1) to form a uniform coating, and drying at a temperature of 40 to 70° C. to obtain an adhesive film; 2-3) The adhesive film obtained in step 2-2) is placed between the objects to be adhered, and is subjected to high pressure treatment at 90-110° C. and 5-7 atmospheres for 20 minutes, and then cured at a temperature of 90-110° C.

Citation Information

Patent Citations

  • Solvent type double-component, high-smoothness vanish composition as well as preparation method and application

    CN108192488A

  • Polyurethane composition having polymeric plasticizer and low content of monomeric diisocyanates

    CN112533973A

  • Primary cured film, secondary cured film, method for producing same, method for using same, thin film laminate, composition for forming thin film, and article

    CN116675832A

  • High-solids binder combinations for scratch-resistant topcoats

    CN1572856A

  • Novel peptide for specific detection of Klebsiella pneumoniae

    KR1020220167973A