Recyclable epoxy resin glass polymer solid adhesive

By performing transesterification reaction and hot pressing at high temperatures, a solvent-free epoxy resin glass polymer solid adhesive was prepared, which solved the problem of volume shrinkage and irreversible crosslinking of traditional adhesives, and achieved high Performance, recyclable and environmentally friendly solid adhesives with excellent mechanical properties and water resistance.

CN118995100AActive Publication Date: 2024-11-22TSINGHUA UNIVERSITY

Patent Information

Application Number
CN202410950438.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-16
Publication Date
2024-11-22
Estimated Expiration
2044-07-16

AI Technical Summary

Technical Problem

Traditional epoxy resin adhesives will produce volume shrinkage and internal stress during the curing process, affecting the adhesion effect, and the irreversible crosslinking structure will lead to inability to recycle, causing environmental pressure, and also contain solvents that are harmful to health.

Method used

A high-performance solid adhesive without solvent was designed, and the transesterification reaction of diglycidyl ether and diacid or anhydride at high temperature was carried out to form a epoxy resin-based glass polymer solid adhesive that can be recycled and utilized multiple times. The agent is prepared by hot pressing to achieve deformation and direct recycling of the crosslinking network.

Benefits of technology

It realizes solvent-free, low-cost, reusable and degradable high-performance solid adhesive, avoids volume shrinkage and volatile problems, and has excellent mechanical properties and water resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004947071290000021
    Figure BDA0004947071290000021
  • Figure BDA0004947071290000033
    Figure BDA0004947071290000033
  • Figure BDA0004947071290000071
    Figure BDA0004947071290000071
Patent Text Reader

Abstract

The invention discloses a recoverable epoxy resin type glass polymer solid adhesive, and particularly discloses a method for preparing the recoverable glass polymer solid adhesive, which comprises the following steps: S1, adding diglycidyl ether and diacid or anhydride into a tetrafluoroethylene mold, and carrying out first heating treatment to obtain a mixture; s2, carrying out second heating treatment and cooling treatment on the mixture and a catalyst to obtain a polymer; s3, the polymer is subjected to slicing treatment, and the solid adhesive is obtained. The method does not need a solvent and is simple to operate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of polymer materials, and in particular to a recyclable epoxy resin glass polymer solid adhesive and a preparation method thereof. Background Art

[0002] People's daily life and production are inseparable from the use of various adhesives. Among them, epoxy resin adhesive is a classic type among many adhesives. Because of its excellent mechanical properties, it is widely used in daily life and production. However, traditional epoxy resin adhesives often need to be obtained through a two-component reaction, which makes the final bonding effect extremely sensitive to the reaction conditions. The proportion, temperature, time, stirring and other conditions will affect the final bonding effect. Secondly, the curing process often causes a volume shrinkage of about 4%, and will also produce internal stress to a certain extent, affecting the final bonding effect. In addition, the product often contains volatiles such as solvents, which will have a certain impact on physical health; and the irreversible cross-linked structure of the final product makes it impossible to be re-plasticized and recycled, which puts pressure on environmental protection. In this regard, solid adhesives not only do not have the influence of solvents, but also do not shrink in volume due to the curing process, and there are no volatiles, and they are very simple to use. In contrast, solid adhesives often have the problem of poor bonding effect.

[0003] Therefore, there is an urgent need to design a high-performance, environmentally friendly, sustainable, low-cost and recyclable solid adhesive. Summary of the invention

[0004] Aiming at the shortcomings of existing traditional adhesives, the present invention uses traditional commercially available raw materials to design a high-performance solid adhesive that does not require solvents and can be recycled and reused multiple times. It promotes the development of sustainable and recyclable technologies and also provides new ideas for the design and preparation of new recyclable and environmentally friendly materials.

[0005] In one aspect of the present invention, the present invention provides a method for preparing a recyclable glass polymer solid adhesive. According to an embodiment of the present invention, the method comprises:

[0006] S1: adding diglycidyl ether and diacid or acid anhydride into a tetrafluoroethylene mold, and performing a first heating treatment to obtain a mixture;

[0007] S2: subjecting the mixture and the catalyst to a second heating treatment and a cooling treatment to obtain a polymer;

[0008] S3: Slice the polymer to obtain the solid adhesive. The method according to the embodiment of the present invention does not require a solvent and is simple to operate. The solid adhesive prepared according to the method of the embodiment of the present invention has high performance and can be recycled and used multiple times and is degradable. The method according to the embodiment of the present invention is to stimulate the exchange reaction (ester exchange reaction) of the thermosetting polymer material at high temperature. When the exchange reaction occurs for a sufficiently long time, the cross-linking network of the material changes while the cross-linking density remains unchanged, thereby realizing the direct deformation processing and direct recycling of the thermosetting polymer material. The recyclable glass-like polymer solid adhesive prepared by the method according to the embodiment of the present invention includes but is not limited to epoxy resin and the like.

[0009] According to an embodiment of the present invention, the above method may further include at least one of the following additional technical features:

[0010] According to an embodiment of the present invention, the diglycidyl ether is bisphenol A diglycidyl ether, 1,4-butanediol diglycidyl ether, neopentyl glycol diglycidyl ether or 1,4-dihydroxybiphenyl diglycidyl ether.

[0011] According to an embodiment of the present invention, the structure of bisphenol A diglycidyl ether is

[0012]

[0013] According to an embodiment of the present invention, the diacid is an aliphatic diacid, an aromatic diacid or a polyethylene glycol diacid.

[0014] According to an embodiment of the present invention, the diacid is adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, dodecyl diacid, hexadecyl diacid, octadecyl diacid, hexadecyl diacid, octadecyl diacid, eicosyl diacid, docosyl diacid, terephthalic acid, phthalic acid, isophthalic acid or polyethylene glycol dicarboxylic acid.

[0015] According to an embodiment of the present invention, the aliphatic diacid is n1 is selected from 1-22.

[0016] According to an embodiment of the present invention, the aromatic diacid is terephthalic acid, phthalic acid or isophthalic acid.

[0017] According to an embodiment of the present invention, the polyethylene glycol diacid is The molecular weight range is 400-2000.

[0018] According to an embodiment of the present invention, the acid anhydride is glutaric anhydride, adipic anhydride or succinic anhydride.

[0019] According to an embodiment of the present invention, the molar ratio of the diglycidyl ether to the diacid or anhydride is 2:1-1:2.

[0020] According to an embodiment of the present invention, the structure of the polymer is

[0021]

[0022] R is n1 is 1-22; or Polyethylene glycol diacid The molecular weight range is 400-2000.

[0023] According to an embodiment of the present invention, the ratio of the amount of the catalyst to the amount of the diacid or anhydride is 2-10 mol%. According to an embodiment of the present invention, this ratio means that if the amount of the diacid is 100 mol, then the amount of the catalyst is 2-10 mol. According to an embodiment of the present invention, the catalytic effect is high and a material with good mechanical properties can be obtained.

[0024] According to an embodiment of the present invention, the organic amine catalyst is tetramethylguanidine, 1,8-diazabicyclo[5.4.0]undec-7-ene or 1,5,7-triazabicyclo-[4.4.0]-decene-5-ene.

[0025] According to an embodiment of the present invention, the organic metal salt catalyst is zinc acetate, aluminum acetate, lead acetate, zinc acetylacetonate, iron acetylacetonate, aluminum acetylacetonate or lead acetylacetonate.

[0026] According to an embodiment of the present invention, the temperature of the first heating treatment is 80-200° C. The inventors have found that too low a temperature will result in the raw materials not being melted, causing an uneven reaction.

[0027] According to an embodiment of the present invention, the first heating treatment time is 5-20 minutes. The inventors have found that if the time is too short, the raw materials will not be completely melted and mixed, resulting in uneven reaction.

[0028] According to an embodiment of the present invention, the temperature of the second heating treatment is 80-200°C.

[0029] According to an embodiment of the present invention, the second heating treatment lasts for 5-20 minutes. The inventors have found that if the time is too short, the viscosity will be insufficient and it will be difficult to perform subsequent hot pressing.

[0030] According to an embodiment of the present invention, the slicing process is performed at a temperature of 80-200° C. and a pressure of 2-10 MPa. The inventors have found that if the temperature or pressure is not within this range, the exchange reaction efficiency may not be fast enough, resulting in a long heating time.

[0031] According to an embodiment of the present invention, the thickness of the slice obtained after the slicing process is 0.03-10 mm. The inventors found that this thickness reflects that the product can be processed into a custom thickness, showing excellent utilization efficiency.

[0032] In another aspect of the present invention, the present invention also provides a method for preparing a recyclable glass polymer solid adhesive. According to an embodiment of the present invention, the method comprises:

[0033] S1: adding bisphenol A diglycidyl ether and diacid or acid anhydride in a molar ratio of 2:1-1:2 into a tetrafluoroethylene mold, heating to melt and stirring sufficiently to obtain a mixture;

[0034] S2: adding 2-10 mol% of 1,5,7-tripropylheptyloxytrimethylammonium salt relative to the amount of the diacid or anhydride to the mixture, continuing heating and stirring for 5-20 minutes until the system gradually becomes viscous and can be drawn into a wire, then stopping heating to obtain a polymer;

[0035] S3: hot-pressing the cooled polymer into a 0.03-10 mm thin sheet at a temperature of 80-200° C. and a pressure of 2-10 MPa, and cutting the thin sheet into a suitable size to obtain the solid adhesive. The method according to the embodiment of the present invention does not require a solvent and is simple to operate. The solid adhesive prepared according to the method of the embodiment of the present invention has high performance and can be recycled and used multiple times and is degradable.

[0036] In another aspect of the present invention, the present invention also provides a recyclable glass polymer solid adhesive. According to an embodiment of the present invention, the solid adhesive is prepared by the method described above.

[0037] The present invention has at least one of the following technical effects:

[0038] 1) No solvent is required during the preparation method according to the embodiment of the present invention, and the cost is low;

[0039] 2) The process parameters of the preparation method according to the embodiment of the present invention are easy to control;

[0040] 3) The simplicity of the preparation method according to the embodiment of the present invention:

[0041] 4) The solid adhesive according to the embodiment of the present invention can be reused;

[0042] 5) Degradation of the solid adhesive according to the embodiment of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0043] The above and / or additional aspects and advantages of the present invention will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:

[0044] Figure 1 is an infrared spectrum diagram of Example 1 according to an embodiment of the present invention;

[0045] Figure 2 The bonding effect of various metals according to Example 1 of the embodiment of the present invention;

[0046] Figure 3 The comparison of adhesive strength after Example 1 according to the embodiment of the present invention was placed in water for 48 hours;

[0047] Figure 4 It is the adhesive strength recovered and reused according to Example 1 of the embodiment of the present invention. DETAILED DESCRIPTION

[0048] Embodiments of the present invention are described in detail below, and examples of the embodiments are shown in the accompanying drawings. The embodiments described below with reference to the accompanying drawings are exemplary and intended to be used to explain the present invention, but should not be understood as limiting the present invention.

[0049] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include at least one of the features. In the description of the present invention, the meaning of "plurality" is at least two, such as two, three, etc., unless otherwise clearly and specifically defined.

[0050] Embodiment 1:

[0051] The recyclable epoxy resin glass polymer solid adhesive used in this embodiment is a material that can undergo an ester exchange reaction inside, and is solidified by bisphenol A diglycidyl ether and dodecyl diacid.

[0052] The specific preparation method of the recyclable epoxy resin glass polymer solid adhesive of this embodiment is as follows:

[0053] In a polytetrafluoroethylene mold, add bisphenol A diglycidyl ether (340 mg, 1 mmol) and dodecane diacid (230 mg, 1 mmol) and heat to melt at 160°C. After stirring evenly, add 1,5,7-triazabicyclo[4.4.0]dec-5-ene (14 mg) and continue heating and stirring for about 5 minutes. The obtained polymer solid is processed into a sheet with a thickness of about 0.25 mm at 180°C using hot pressing technology, and finally the obtained solid adhesive is cut into the required shape using tools such as scissors.

[0054]

[0055] like Figure 1As shown: The structure determination is characterized by infrared spectroscopy to determine the functional groups in the polymer. Among them, 912cm -1 No obvious absorption was found on the left and right, indicating that the free epoxy groups have been completely consumed by the reaction. The remaining absorptions come from chemical bonds such as benzene ring, OH, -CH2-, C=O, and COC.

[0056] Its bonding effect on various metals is shown in Figure 2 , where SS stands for stainless steel, Fe stands for iron, Al stands for aluminum, Cu stands for copper, and the roughness of the metal is r3.2. All metal surfaces were cleaned with acetone and isopropyl alcohol before bonding, without additional grinding to increase the contact area.

[0057] Comparison of adhesive strength after 48 hours in water Figure 3 ,After the sample was placed in tap water for 48 hours, the adhesive strength did not change significantly, indicating excellent water resistance.

[0058] Depend on Figure 4 It can be seen that the sample can be recycled three times and still retains about 82% of its original adhesive strength, indicating excellent reusability.

[0059] Embodiment 2:

[0060] The specific recycling and utilization processing method of the recyclable epoxy resin glass polymer solid adhesive according to Example 1 of the present invention is as follows:

[0061] The recyclable epoxy resin glass polymer solid adhesive fragments collected with a knife or scissors are heated to 80-200°C, hot-pressed at 2-10MPa for 0.5-2 hours, then cooled to room temperature, and finally cut into the required shape using scissors or other tools for reuse.

[0062] The above embodiment uses one example for illustration, but it should be understood that the present invention is not limited to the above materials. Any recyclable epoxy resin glass polymer solid adhesive material that can undergo ester exchange reaction can be recycled.

[0063] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.

[0064] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.

Claims

1. A method for preparing a recyclable glass polymer solid adhesive, It is characterized in that include: S1: adding diglycidyl ether and diacid or acid anhydride into a tetrafluoroethylene mold, and performing a first heating treatment to obtain a mixture; S2: subjecting the mixture and the catalyst to a second heating treatment and a cooling treatment to obtain a polymer; S3: Slicing the polymer to obtain the solid adhesive.

2. The method according to claim 1, It is characterized in that The diglycidyl ether is bisphenol A diglycidyl ether, 1,4-butanediol diglycidyl ether, neopentyl glycol diglycidyl ether or 1,4-dihydroxybiphenyl diglycidyl ether; Optionally, the structure of the bisphenol A diglycidyl ether is 3. The method according to claim 1, It is characterized in that The diacid is an aliphatic diacid, an aromatic diacid or a polyethylene glycol diacid; Optionally, the diacid is malonic acid, succinic acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, and dodecyl diacid, hexadecyl diacid, octadecyl diacid, hexadecyl diacid, octadecyl diacid, eicosyl diacid, docosyl diacid, terephthalic acid, phthalic acid, isophthalic acid or polyethylene glycol dicarboxylic acid; Optionally, the aliphatic diacid is n1 is selected from 1 to 22; Optionally, the aryl diacid is terephthalic acid, phthalic acid or isophthalic acid; Optionally, the polyethylene glycol diacid is The molecular weight range is 400-2000; Optionally, the anhydride is glutaric anhydride, adipic anhydride or succinic anhydride; Optionally, the molar ratio of the diglycidyl ether to the diacid or anhydride is 2:1-1:

2.

4. The method according to claim 1, It is characterized in that The structure of the polymer is R is n1 is 1-22; or Polyethylene glycol diacid The molecular weight range is 400-2000.

5. The method according to claim 1, It is characterized in that The amount of the catalyst used is 2-10 mol% relative to the amount of the diacid or anhydride; Optionally, the catalyst is an organic amine catalyst or an organic metal salt catalyst; Optionally, the organic amine catalyst is tetramethylguanidine, 1,8-diazabicyclo[5.4.0]undec-7-ene or 1,5,7-triazabicyclo-[4.4.0]-decene-5-ene; Optionally, the organic metal salt catalyst is zinc acetate, aluminum acetate, lead acetate, zinc acetylacetonate, iron acetylacetonate, aluminum acetylacetonate or lead acetylacetonate.

6. The method according to claim 1, It is characterized in that The temperature of the first heating treatment is 80-200°C; Optionally, the first heating treatment time is 5-20 minutes.

7. The method according to claim 1, It is characterized in that The temperature of the second heating treatment is 80-200°C; Optionally, the second heating treatment is performed for 5-20 minutes.

8. The method according to claim 1, It is characterized in that The slicing process is carried out at a temperature of 80-200°C and a pressure of 2-10MPa; Optionally, the thickness of the slices obtained after the slicing process is 0.03 to 10 mm.

9. A method for preparing a recyclable glass polymer solid adhesive, It is characterized in that include: S1: adding bisphenol A diglycidyl ether and diacid or acid anhydride in a molar ratio of 2:1-1:2 into a tetrafluoroethylene mold, heating to melt and stirring sufficiently to obtain a mixture; S2: adding 2-10 mol% of 1,5,7-triazabicyclo[4.4.0]dec-5-ene to the mixture relative to the amount of the diacid or anhydride, continuing heating and stirring for 5-20 minutes until the system gradually becomes viscous and can be drawn into a wire, then stopping heating to obtain a polymer; S3: hot-pressing the cooled polymer at 80-200° C. and 2-10 MPa to form a sheet of 0.03-10 mm, and cutting the sheet into a suitable size to obtain the solid adhesive.

10. A recyclable glass polymer solid adhesive, It is characterized in that The solid adhesive is prepared by the method according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Normal-temperature curing epoxy resin-based vitrimer adhesive and preparation method thereof

    CN113337234A

  • High-strength epoxy resin composition and preparation method thereof

    CN113621333A

  • Epoxy glass polymer containing dynamic ester bonds, glass fiber cloth laminated board as well as preparation method and application of glass fiber cloth laminated board

    CN116731288A

  • Water processing method and application of glass-like epoxy resin

    CN117659438A

  • Mixed epoxy resin-mixed anhydride adhesive compositions

    US3932343A

Cited By

  • Detachable heat-conducting epoxy resin adhesive based on ester exchange and preparation method thereof

    CN119899613A