Method for preparing graphene conductive adhesive by recovering graphene film composite water-based resin
By recycling graphene film waste, combining microcrystalline nanofibers and aqueous resins, a high-performance graphene conductive film is prepared, which solves the problem of waste resources in graphene film production and achieves the effect of improving conductivity and reducing environmental protection costs.
Patent Information
- Application Number
- CN202411102466.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-12
- Publication Date
- 2024-11-22
AI Technical Summary
Unqualified products generated during the production of existing graphene films are regarded as industrial waste, resulting in waste of resources. Graphene powders occupy a dominant market position, and the film accounts for a small proportion, and waste resources are not effectively utilized.
The method of recycling graphene film composite aqueous resin is used to prepare graphene conductive glue. Through crushing, sanding, dispersing, mixing and baking, the graphene film waste is converted into conductive filler and is combined with microcrystalline nanofibers and aqueous resin. Combined, a high-performance conductive film is formed.
It improves the conductive properties of graphene conductive film, reduces resistivity, realizes the recycling of waste materials, saves resources, reduces environmental protection costs, and increases the added value of the product.
Smart Images

Figure CN118995114A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of graphene conductive adhesives, in particular to a method for preparing graphene conductive adhesive by recycling graphene film composite water-based resin. Background Art
[0002] Graphene is a two-dimensional (2D) material composed of a single layer of carbon atoms arranged in a honeycomb pattern. It is also the basic unit of carbon materials of other dimensions. It can be wrapped into zero-dimensional (0D) fullerene, rolled into one-dimensional (1D) carbon nanotubes, and stacked into (3D) graphite. In 2004, Professors Andre Geim (AK Geim) and Konstantin (K.S Novoselov) of the University of Manchester in the UK discovered single-layer graphene in an experiment using the transparent tape peeling method. This opened the curtain of the graphene era, and the two professors also won the 2010 Nobel Prize in Physics for their outstanding contributions in the field of graphene. Graphene, known as the "king of new materials", is one of the thinnest, hardest, and best conductive and thermally conductive materials currently known.
[0003] As the output of graphene film increases, the current Chinese graphene material market is mainly dominated by graphene powder. In 2022, graphene powder accounts for 90.7% of the overall market, and graphene film accounts for 9.3%. Graphene film is mainly produced through the coating process. During the startup and adjustment of the machine before and after coating, there will be a large number of unqualified products. These unqualified products are treated as industrial waste, and the treatment of these industrial wastes requires 400 to 600 yuan per ton, which will cause great waste. Summary of the invention
[0004] In order to solve the defects of the prior art, the present invention provides a method for preparing graphene conductive adhesive by recycling graphene film composite water-based resin.
[0005] In order to solve the above technical problems, the present invention provides the following technical solutions:
[0006] The present invention discloses a method for preparing graphene conductive adhesive by recycling graphene film composite water-based resin, and the specific preparation steps are as follows:
[0007] (1) Preparation of graphite powder from recycled graphene membrane waste: Recycling graphene membrane waste, crushing the recycled graphene membrane waste, preliminarily crushing and sieving the recycled graphene membrane waste to obtain graphene powder with a size of 40 to 100 meshes, and further sand-grinding the preliminarily crushed and sifted graphene powder to obtain graphene powder with a size of 2000 to 2500 meshes;
[0008] (2) Preparation of dispersion of recycled graphene film waste: The graphene powder obtained by sand grinding was mixed with N-methylpyrrolidone (NMP) at concentrations of 1%, 3%, 5%, and 10% to obtain graphene dispersions of different concentrations at concentrations of 1%, 3%, 5%, and 10% of the graphene powder;
[0009] (3) Preparation of microcrystalline nanofiber dispersion: Zinc chloride, formic acid, and water were stirred at room temperature to obtain a nanocellulose solvent, and the nanocellulose solvent was ultrasonically dispersed at high speed with microcrystalline nanofibers at concentrations of 1%, 3%, 5%, and 10% at room temperature to obtain microcrystalline nanocellulose dispersions of different concentrations at microcrystalline nanofiber concentrations of 1%, 3%, 5%, and 10%;
[0010] (4) Preparation of a mixed solution of recycled graphene membrane waste dispersion liquid / microcrystalline nanocellulose dispersion liquid: ultrasonically stirring the graphene membrane waste dispersion liquid and the microcrystalline nanofiber dispersion liquid at a ratio of 1:1.3 to obtain a mixed solution of recycled graphene membrane waste and microcrystalline nanofiber;
[0011] (5) Preparation of a dispersion of composite hydrazine hydrate / graphene membrane waste: The mixed solution of the recycled graphene membrane waste and microcrystalline nanofibers is stirred, and hydrazine hydrate and ammonia water are added successively to obtain a dispersion of composite hydrazine hydrate / graphene membrane waste.
[0012] (6) Preparation of graphene conductive paste: Graphene was stirred with water-based resin at a concentration of 1%, 3%, 5%, and 10%, and a leveling agent, a catalyst, a defoaming agent, and a promoter were added to obtain graphene conductive pastes at a concentration of 1%, 3%, 5%, and 10%.
[0013] (7) Preparation of graphene conductive film: The graphene conductive slurry and non-woven fabric are formed into a film by using a coating and dipping process, and the coated / dipped graphene conductive film is baked to obtain a graphene conductive film.
[0014] As a preferred technical solution of the present invention, the graphene powder obtained by sand milling in step (2) is mixed with N-methylpyrrolidone (NMP) and subjected to ultrasound for 30 minutes and high-speed dispersion at 1000 r / min for 30 minutes.
[0015] As a preferred technical solution of the present invention, in the step (3), the ratio of sodium chloride, formic acid and water is 1:3.2:2.2, and stirring is performed at 500 r / min for 30 min.
[0016] As a preferred technical solution of the present invention, in the step (3), the nanocellulose solvent and the microcrystalline nanofibers are ultrasonicated at room temperature for 30 minutes and dispersed at high speed for 1 hour.
[0017] As a preferred technical solution of the present invention, in the step (4), the graphene membrane waste dispersion and the microcrystalline nanofiber dispersion are ultrasonically treated for 30 minutes and stirred at 500 r / min for 20 minutes.
[0018] As a preferred technical solution of the present invention, in the step (5), the mass ratio of hydrazine hydrate to the graphene membrane waste dispersion is 1:500, and the mass ratio of ammonia water to hydrazine hydrate is 5:1. Hydrazine hydrate and ammonia water are added successively to the mixed solution of the recovered graphene membrane waste and microcrystalline nanofibers under stirring at 300 r / min, and stirred at 85°C and 500 r / min for 2 hours.
[0019] As a preferred technical solution of the present invention, the water-based resin in step (6) includes water-based epoxy ester, water-based polyurethane, and water-based acrylic resin.
[0020] As a preferred technical solution of the present invention, in step (6), the leveling agent is a modified dimethyl silicone polymer, the catalyst is an organic-inorganic modified nanopolymer, the defoaming agent is a non-ionic surfactant polymer, and the accelerator is a modified epoxy phosphate polymer.
[0021] As a preferred technical solution of the present invention, in the step (6), during the stirring process of graphene and one or two of the water-based epoxy ester, water-based polyurethane, and water-based acrylic resin at 500 r / min, 1.5% to 2% of leveling agent, 1.5% to 2% of catalyst, 1.5% to 2% of defoaming agent, and 1.5% to 2% of accelerator are added, and the mixture is stirred at 800 r / min for 1 hour.
[0022] As a preferred technical solution of the present invention, the graphene conductive film coated / impregnated in step (7) is baked in a drying oven at 60° C. for 1 hour.
[0023] The beneficial effects of the present invention are:
[0024] The method for preparing graphene conductive adhesive by recycling graphene film and compounding water-based resin, the graphene conductive film is a collection of recycled graphene waste, and as a conductive filler, it has excellent conductivity, and the introduction of microcrystalline nanocellulose can improve the compatibility of recycled graphene and water-based resin, the better the compatibility, the more uniform the dispersion of the filler in the water-based resin, the particles of the conductive filler are in close contact with each other, and a conductive path is formed, that is, the higher the concentration of the added recycled graphene waste, the lower the resistivity, and the better the conductive performance, and the discarded graphene scraps are recycled, turning waste into treasure, saving resources, and preparing high value-added conductive adhesive, which can not only achieve energy saving and emission reduction in environmental protection, but also reduce costs and increase profits. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] The accompanying drawings are used to provide a further understanding of the present invention and constitute a part of the specification. Together with the embodiments of the present invention, they are used to explain the present invention and do not constitute a limitation of the present invention. In the accompanying drawings:
[0026] Figure 1 Table 1 is the experimental data of a method for recycling graphene film composite water-based resin to prepare graphene conductive adhesive according to the present invention. DETAILED DESCRIPTION
[0027] The preferred embodiments of the present invention are described below in conjunction with the accompanying drawings. It should be understood that the preferred embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.
[0028] Embodiment 1: A method for preparing graphene conductive adhesive by recycling graphene film composite water-based resin according to the present invention, wherein the specific preparation steps are as follows:
[0029] (1) Preparation of graphite powder from recycled graphene membrane waste: Recycling graphene membrane waste, crushing the recycled graphene membrane waste, preliminarily crushing and sieving the recycled graphene membrane waste to obtain graphene powder with a size of 40 to 100 meshes, and further sand-grinding the preliminarily crushed and sifted graphene powder to obtain graphene powder with a size of 2000 to 2500 meshes;
[0030] (2) Preparation of dispersion of recycled graphene film waste: The graphene powder obtained by sand grinding was mixed with N-methylpyrrolidone (NMP) at a concentration of 1% to obtain graphene dispersions of different concentrations at a concentration of 1% of graphene powder;
[0031] (3) Preparation of microcrystalline nanofiber dispersion: Zinc chloride, formic acid, and water are stirred at room temperature to obtain a nanocellulose solvent, and the nanocellulose solvent is respectively dispersed with microcrystalline nanofibers at a concentration of 1% by ultrasonication at room temperature at high speed to obtain microcrystalline nanocellulose dispersions of different concentrations at a concentration of 1% of microcrystalline nanofibers;
[0032] (4) Preparation of a mixed solution of recycled graphene membrane waste dispersion liquid / microcrystalline nanocellulose dispersion liquid: ultrasonically stirring the graphene membrane waste dispersion liquid and the microcrystalline nanofiber dispersion liquid at a ratio of 1:1.3 to obtain a mixed solution of recycled graphene membrane waste and microcrystalline nanofiber;
[0033] (5) Preparation of a dispersion of composite hydrazine hydrate / graphene membrane waste: The mixed solution of the recycled graphene membrane waste and microcrystalline nanofibers is stirred, and hydrazine hydrate and ammonia water are added successively to obtain a dispersion of composite hydrazine hydrate / graphene membrane waste.
[0034] (6) Preparation of graphene conductive paste: Graphene was stirred with water-based resin at a concentration of 1%, and a leveling agent, a catalyst, a defoaming agent and a promoter were added to obtain a graphene conductive paste at a concentration of 1%.
[0035] (7) Preparation of graphene conductive film: The graphene conductive slurry and non-woven fabric are formed into a film by using a coating and dipping process, and the coated / dipped graphene conductive film is baked to obtain a graphene conductive film.
[0036] The graphene powder obtained by sand milling in step (2) is mixed with N-methylpyrrolidone (NMP) and subjected to ultrasound for 30 minutes and high-speed dispersion at 1000 r / min for 30 minutes.
[0037] Wherein, in the step (3), the ratio of sodium chloride, formic acid and water is 1:3.2:2.2, and stirring is performed at 500 r / min for 30 min. In the step (3), the nanocellulose solvent and the microcrystalline nanofibers are ultrasonicated at room temperature for 30 min and dispersed at high speed for 1 h.
[0038] Wherein, in the step (4), the graphene membrane waste dispersion and the microcrystalline nanofiber dispersion are ultrasonically treated for 30 minutes and stirred at 500 r / min for 20 minutes.
[0039] Wherein, in the step (5), the mass ratio of hydrazine hydrate to the graphene membrane waste dispersion is 1:500, the mass ratio of ammonia water to hydrazine hydrate is 5:1, and the mixed solution of the recovered graphene membrane waste and microcrystalline nanofibers is successively added with hydrazine hydrate and ammonia water under stirring at 300 r / min, and stirred for 2 hours at 85°C and 500 r / min.
[0040] Wherein, in the step (5), the mass ratio of hydrazine hydrate to the graphene membrane waste dispersion is 1:500, the mass ratio of ammonia water to hydrazine hydrate is 5:1, and the mixed solution of the recovered graphene membrane waste and microcrystalline nanofibers is successively added with hydrazine hydrate and ammonia water under stirring at 300 r / min, and stirred for 2 hours at 85°C and 500 r / min.
[0041] The aqueous resin in step (6) comprises aqueous epoxy ester, aqueous polyurethane and aqueous acrylic resin; the leveling agent in step (6) is a modified dimethyl silicone polymer; the catalyst is an organic inorganic modified nano polymer; the defoaming agent is a nonionic surfactant polymer; the accelerator is a modified epoxy phosphate polymer; in step (6), 1.5% to 2% of the leveling agent, 1.5% to 2% of the catalyst, 1.5% to 2% of the defoaming agent and 1.5% to 2% of the accelerator are added during the stirring process at 500 r / min to the graphene and one or two of the aqueous epoxy ester, aqueous polyurethane and aqueous acrylic resin; and the stirring is performed at 800 r / min for 1 hour.
[0042] The graphene conductive film coated / impregnated in step (7) is baked in a drying oven at 60° C. for 1 hour.
[0043] The graphene conductive film obtained after cooling to room temperature was taken out and tested using a HP-S2662 precision four-probe resistivity tester. When the graphene filler concentration was 1%, its resistivity was found to be 1517 Ω·m.
[0044] Embodiment 2: A method for preparing graphene conductive adhesive by recycling graphene film composite water-based resin according to the present invention, wherein the specific preparation steps are as follows:
[0045] (1) Preparation of graphite powder from recycled graphene membrane waste: Recycling graphene membrane waste, crushing the recycled graphene membrane waste, preliminarily crushing and sieving the recycled graphene membrane waste to obtain graphene powder with a size of 40 to 100 meshes, and further sand-grinding the preliminarily crushed and sifted graphene powder to obtain graphene powder with a size of 2000 to 2500 meshes;
[0046] (2) Preparation of dispersion of recycled graphene film waste: mixing graphene powder obtained by sand grinding with N-methylpyrrolidone (NMP) at a concentration of 3% to obtain graphene dispersions of different concentrations at a concentration of 3% graphene powder;
[0047] (3) Preparation of microcrystalline nanofiber dispersion: Zinc chloride, formic acid, and water were stirred at room temperature to obtain a nanocellulose solvent, and the nanocellulose solvent was respectively dispersed at high speed by ultrasonication at room temperature with a concentration of 1% of microcrystalline nanofibers to obtain microcrystalline nanocellulose dispersions of different concentrations at a concentration of 3% of microcrystalline nanofibers;
[0048] (4) Preparation of a mixed solution of recycled graphene membrane waste dispersion liquid / microcrystalline nanocellulose dispersion liquid: ultrasonically stirring the graphene membrane waste dispersion liquid and the microcrystalline nanofiber dispersion liquid at a ratio of 1:1.3 to obtain a mixed solution of recycled graphene membrane waste and microcrystalline nanofiber;
[0049] (5) Preparation of a dispersion of composite hydrazine hydrate / graphene membrane waste: The mixed solution of the recycled graphene membrane waste and microcrystalline nanofibers is stirred, and hydrazine hydrate and ammonia water are added successively to obtain a dispersion of composite hydrazine hydrate / graphene membrane waste.
[0050] (6) Preparation of graphene conductive paste: Graphene was stirred with water-based resin at a concentration of 3%, and a leveling agent, a catalyst, a defoaming agent and a promoter were added to obtain a graphene conductive paste at a concentration of 3%.
[0051] (7) Preparation of graphene conductive film: The graphene conductive slurry and non-woven fabric are formed into a film by using a coating and dipping process, and the coated / dipped graphene conductive film is baked to obtain a graphene conductive film.
[0052] The graphene powder obtained by sand milling in step (2) is mixed with N-methylpyrrolidone (NMP) and subjected to ultrasound for 30 minutes and high-speed dispersion at 1000 r / min for 30 minutes.
[0053] Wherein, in the step (3), the ratio of sodium chloride, formic acid and water is 1:3.2:2.2, and stirring is performed at 500 r / min for 30 min. In the step (3), the nanocellulose solvent and the microcrystalline nanofibers are ultrasonicated at room temperature for 30 min and dispersed at high speed for 1 h.
[0054] Wherein, in the step (4), the graphene membrane waste dispersion and the microcrystalline nanofiber dispersion are ultrasonically treated for 30 minutes and stirred at 500 r / min for 20 minutes.
[0055] Wherein, in the step (5), the mass ratio of hydrazine hydrate to the graphene membrane waste dispersion is 1:500, the mass ratio of ammonia water to hydrazine hydrate is 5:1, and the mixed solution of the recovered graphene membrane waste and microcrystalline nanofibers is successively added with hydrazine hydrate and ammonia water under stirring at 300 r / min, and stirred for 2 hours at 85°C and 500 r / min.
[0056] Wherein, in the step (5), the mass ratio of hydrazine hydrate to the graphene membrane waste dispersion is 1:500, the mass ratio of ammonia water to hydrazine hydrate is 5:1, and the mixed solution of the recovered graphene membrane waste and microcrystalline nanofibers is successively added with hydrazine hydrate and ammonia water under stirring at 300 r / min, and stirred for 2 hours at 85°C and 500 r / min.
[0057] The aqueous resin in step (6) comprises aqueous epoxy ester, aqueous polyurethane and aqueous acrylic resin; the leveling agent in step (6) is a modified dimethyl silicone polymer; the catalyst is an organic inorganic modified nano polymer; the defoaming agent is a nonionic surfactant polymer; the accelerator is a modified epoxy phosphate polymer; in step (6), 1.5% to 2% of the leveling agent, 1.5% to 2% of the catalyst, 1.5% to 2% of the defoaming agent and 1.5% to 2% of the accelerator are added during the stirring process at 500 r / min to the graphene and one or two of the aqueous epoxy ester, aqueous polyurethane and aqueous acrylic resin; and the stirring is performed at 800 r / min for 1 hour.
[0058] The graphene conductive film coated / impregnated in step (7) is baked in a drying oven at 60° C. for 1 hour.
[0059] After cooling to room temperature, a graphene conductive film was obtained. Using a HP-S2662 precision four-probe resistivity tester, when the concentration of graphene filler was 3%, its resistivity was tested to be 637Ω·m.
[0060] Embodiment 3: A method for preparing graphene conductive adhesive by recycling graphene film composite water-based resin according to the present invention, wherein the specific preparation steps are as follows:
[0061] (1) Preparation of graphite powder from recycled graphene membrane waste: Recycling graphene membrane waste, crushing the recycled graphene membrane waste, preliminarily crushing and sieving the recycled graphene membrane waste to obtain graphene powder with a size of 40 to 100 meshes, and further sand-grinding the preliminarily crushed and sifted graphene powder to obtain graphene powder with a size of 2000 to 2500 meshes;
[0062] (2) Preparation of dispersion of recycled graphene film waste: mixing graphene powder obtained by sand grinding with N-methylpyrrolidone (NMP) at a concentration of 5% to obtain graphene dispersions of different concentrations at a concentration of 5% graphene powder;
[0063] (3) Preparation of microcrystalline nanofiber dispersion: Zinc chloride, formic acid, and water were stirred at room temperature to obtain a nanocellulose solvent, and the nanocellulose solvent was respectively dispersed at high speed by ultrasonication at room temperature with a concentration of 1% of microcrystalline nanofibers to obtain microcrystalline nanocellulose dispersions of different concentrations at a concentration of 5% of microcrystalline nanofibers;
[0064] (4) Preparation of a mixed solution of recycled graphene membrane waste dispersion liquid / microcrystalline nanocellulose dispersion liquid: ultrasonically stirring the graphene membrane waste dispersion liquid and the microcrystalline nanofiber dispersion liquid at a ratio of 1:1.3 to obtain a mixed solution of recycled graphene membrane waste and microcrystalline nanofiber;
[0065] (5) Preparation of a dispersion of composite hydrazine hydrate / graphene membrane waste: The mixed solution of the recycled graphene membrane waste and microcrystalline nanofibers is stirred, and hydrazine hydrate and ammonia water are added successively to obtain a dispersion of composite hydrazine hydrate / graphene membrane waste.
[0066] (6) Preparation of graphene conductive paste: Graphene was stirred with water-based resin at a concentration of 5%, and a leveling agent, a catalyst, a defoaming agent and a promoter were added to obtain a graphene conductive paste at a concentration of 5%.
[0067] (7) Preparation of graphene conductive film: The graphene conductive slurry and non-woven fabric are formed into a film by using a coating and dipping process, and the coated / dipped graphene conductive film is baked to obtain a graphene conductive film.
[0068] The graphene powder obtained by sand milling in step (2) is mixed with N-methylpyrrolidone (NMP) and subjected to ultrasound for 30 minutes and high-speed dispersion at 1000 r / min for 30 minutes.
[0069] Wherein, in the step (3), the ratio of sodium chloride, formic acid and water is 1:3.2:2.2, and stirring is performed at 500 r / min for 30 min. In the step (3), the nanocellulose solvent and the microcrystalline nanofibers are ultrasonicated at room temperature for 30 min and dispersed at high speed for 1 h.
[0070] Wherein, in the step (4), the graphene membrane waste dispersion and the microcrystalline nanofiber dispersion are ultrasonically treated for 30 minutes and stirred at 500 r / min for 20 minutes.
[0071] Wherein, in the step (5), the mass ratio of hydrazine hydrate to the graphene membrane waste dispersion is 1:500, the mass ratio of ammonia water to hydrazine hydrate is 5:1, and the mixed solution of the recovered graphene membrane waste and microcrystalline nanofibers is successively added with hydrazine hydrate and ammonia water under stirring at 300 r / min, and stirred for 2 hours at 85°C and 500 r / min.
[0072] Wherein, in the step (5), the mass ratio of hydrazine hydrate to the graphene membrane waste dispersion is 1:500, the mass ratio of ammonia water to hydrazine hydrate is 5:1, and the mixed solution of the recovered graphene membrane waste and microcrystalline nanofibers is successively added with hydrazine hydrate and ammonia water under stirring at 300 r / min, and stirred for 2 hours at 85°C and 500 r / min.
[0073] The aqueous resin in step (6) comprises aqueous epoxy ester, aqueous polyurethane and aqueous acrylic resin; the leveling agent in step (6) is a modified dimethyl silicone polymer; the catalyst is an organic inorganic modified nano polymer; the defoaming agent is a nonionic surfactant polymer; the accelerator is a modified epoxy phosphate polymer; in step (6), 1.5% to 2% of the leveling agent, 1.5% to 2% of the catalyst, 1.5% to 2% of the defoaming agent and 1.5% to 2% of the accelerator are added during the stirring process at 500 r / min to the graphene and one or two of the aqueous epoxy ester, aqueous polyurethane and aqueous acrylic resin; and the stirring is performed at 800 r / min for 1 hour.
[0074] The graphene conductive film coated / impregnated in step (7) is baked in a drying oven at 60° C. for 1 hour.
[0075] After cooling to room temperature, a graphene conductive film was obtained. Using a HP-S2662 precision four-probe resistivity tester, when the concentration of graphene filler was 5%, its resistivity was tested to be 9.4Ω·m.
[0076] Embodiment 4: A method for preparing graphene conductive adhesive by recycling graphene film composite water-based resin according to the present invention, wherein the specific preparation steps are as follows:
[0077] (1) Preparation of graphite powder from recycled graphene membrane waste: Recycling graphene membrane waste, crushing the recycled graphene membrane waste, preliminarily crushing and sieving the recycled graphene membrane waste to obtain graphene powder with a size of 40 to 100 meshes, and further sand-grinding the preliminarily crushed and sifted graphene powder to obtain graphene powder with a size of 2000 to 2500 meshes;
[0078] (2) Preparation of dispersion of recycled graphene film waste: mixing graphene powder obtained by sand grinding with N-methylpyrrolidone (NMP) at a concentration of 10% to obtain graphene dispersions of different concentrations at a concentration of 10% graphene powder;
[0079] (3) Preparation of microcrystalline nanofiber dispersion: Zinc chloride, formic acid, and water were stirred at room temperature to obtain a nanocellulose solvent, and the nanocellulose solvent was respectively dispersed at high speed by ultrasonication at room temperature with a concentration of 1% of microcrystalline nanofibers to obtain microcrystalline nanocellulose dispersions of different concentrations at a concentration of 10% of microcrystalline nanofibers;
[0080] (4) Preparation of a mixed solution of recycled graphene membrane waste dispersion liquid / microcrystalline nanocellulose dispersion liquid: ultrasonically stirring the graphene membrane waste dispersion liquid and the microcrystalline nanofiber dispersion liquid at a ratio of 1:1.3 to obtain a mixed solution of recycled graphene membrane waste and microcrystalline nanofiber;
[0081] (5) Preparation of a dispersion of composite hydrazine hydrate / graphene membrane waste: The mixed solution of the recycled graphene membrane waste and microcrystalline nanofibers is stirred, and hydrazine hydrate and ammonia water are added successively to obtain a dispersion of composite hydrazine hydrate / graphene membrane waste.
[0082] (6) Preparation of graphene conductive paste: Graphene was stirred with water-based resin at a concentration of 10%, and a leveling agent, a catalyst, a defoaming agent and a promoter were added to obtain a graphene conductive paste at a concentration of 10%.
[0083] (7) Preparation of graphene conductive film: The graphene conductive slurry and non-woven fabric are formed into a film by using a coating and dipping process, and the coated / dipped graphene conductive film is baked to obtain a graphene conductive film.
[0084] The graphene powder obtained by sand milling in step (2) is mixed with N-methylpyrrolidone (NMP) and subjected to ultrasound for 30 minutes and high-speed dispersion at 1000 r / min for 30 minutes.
[0085] Wherein, in the step (3), the ratio of sodium chloride, formic acid and water is 1:3.2:2.2, and stirring is performed at 500 r / min for 30 min. In the step (3), the nanocellulose solvent and the microcrystalline nanofibers are ultrasonicated at room temperature for 30 min and dispersed at high speed for 1 h.
[0086] Wherein, in the step (4), the graphene membrane waste dispersion and the microcrystalline nanofiber dispersion are ultrasonically treated for 30 minutes and stirred at 500 r / min for 20 minutes.
[0087] Wherein, in the step (5), the mass ratio of hydrazine hydrate to the graphene membrane waste dispersion is 1:500, the mass ratio of ammonia water to hydrazine hydrate is 5:1, and the mixed solution of the recovered graphene membrane waste and microcrystalline nanofibers is successively added with hydrazine hydrate and ammonia water under stirring at 300 r / min, and stirred for 2 hours at 85°C and 500 r / min.
[0088] Wherein, in the step (5), the mass ratio of hydrazine hydrate to the graphene membrane waste dispersion is 1:500, the mass ratio of ammonia water to hydrazine hydrate is 5:1, and the mixed solution of the recovered graphene membrane waste and microcrystalline nanofibers is successively added with hydrazine hydrate and ammonia water under stirring at 300 r / min, and stirred for 2 hours at 85°C and 500 r / min.
[0089] The aqueous resin in step (6) comprises aqueous epoxy ester, aqueous polyurethane and aqueous acrylic resin; the leveling agent in step (6) is a modified dimethyl silicone polymer; the catalyst is an organic inorganic modified nano polymer; the defoaming agent is a nonionic surfactant polymer; the accelerator is a modified epoxy phosphate polymer; in step (6), 1.5% to 2% of the leveling agent, 1.5% to 2% of the catalyst, 1.5% to 2% of the defoaming agent and 1.5% to 2% of the accelerator are added during the stirring process at 500 r / min to the graphene and one or two of the aqueous epoxy ester, aqueous polyurethane and aqueous acrylic resin; and the stirring is performed at 800 r / min for 1 hour.
[0090] The graphene conductive film coated / impregnated in step (7) is baked in a drying oven at 60° C. for 1 hour.
[0091] After cooling to room temperature, a graphene conductive film was obtained. Using a HP-S2662 precision four-probe resistivity tester, when the concentration of graphene filler was 10%, its resistivity was tested to be 3.1Ω·m.
[0092] As can be seen from Table 1, the graphene conductive film is a collection of recycled graphene waste. As a conductive filler, it has excellent conductivity. The introduction of microcrystalline nanocellulose can improve the compatibility of recycled graphene and water-based resin. The better the compatibility, the more uniform the dispersion of the filler in the water-based resin. The particles of the conductive filler are in close contact with each other to form a conductive path. That is, the higher the concentration of the added recycled graphene waste, the lower the resistivity and the better the conductive performance.
[0093] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing graphene conductive adhesive by recycling graphene film composite water-based resin, characterized in that: The specific preparation steps are as follows: (1) Preparation of graphite powder from recycled graphene membrane waste: Recycling graphene membrane waste, crushing the recycled graphene membrane waste, preliminarily crushing and sieving the recycled graphene membrane waste to obtain graphene powder with a size of 40 to 100 meshes, and further sand-grinding the preliminarily crushed and sifted graphene powder to obtain graphene powder with a size of 2000 to 2500 meshes; (2) Preparation of dispersion of recycled graphene film waste: The graphene powder obtained by sand grinding was mixed with N-methylpyrrolidone (NMP) at concentrations of 1%, 3%, 5%, and 10% to obtain graphene dispersions of different concentrations at concentrations of 1%, 3%, 5%, and 10% of the graphene powder; (3) Preparation of microcrystalline nanofiber dispersion: Zinc chloride, formic acid, and water were stirred at room temperature to obtain a nanocellulose solvent, and the nanocellulose solvent was ultrasonically dispersed at high speed with microcrystalline nanofibers at concentrations of 1%, 3%, 5%, and 10% at room temperature to obtain microcrystalline nanocellulose dispersions of different concentrations at microcrystalline nanofiber concentrations of 1%, 3%, 5%, and 10%; (4) Preparation of a mixed solution of recycled graphene membrane waste dispersion liquid / microcrystalline nanocellulose dispersion liquid: ultrasonically stirring the graphene membrane waste dispersion liquid and the microcrystalline nanofiber dispersion liquid at a ratio of 1:1.3 to obtain a mixed solution of recycled graphene membrane waste and microcrystalline nanofiber; (5) Preparation of a dispersion of composite hydrazine hydrate / graphene membrane waste: The mixed solution of the recycled graphene membrane waste and microcrystalline nanofibers is stirred, and hydrazine hydrate and ammonia water are added successively to obtain a dispersion of composite hydrazine hydrate / graphene membrane waste. (6) Preparation of graphene conductive paste: Graphene was stirred with water-based resin at a concentration of 1%, 3%, 5%, and 10%, and a leveling agent, a catalyst, a defoaming agent, and a promoter were added to obtain graphene conductive pastes at a concentration of 1%, 3%, 5%, and 10%. (7) Preparation of graphene conductive film: The graphene conductive slurry and non-woven fabric are formed into a film by using a coating and dipping process, and the coated / dipped graphene conductive film is baked to obtain a graphene conductive film.
2. The method for preparing graphene conductive adhesive by recycling graphene film composite water-based resin according to claim 1, characterized in that: The graphene powder obtained by sand grinding in the step (2) is mixed with N-methylpyrrolidone (NMP), subjected to ultrasound for 30 minutes, and high-speed dispersion at 1000 r / min for 30 minutes.
3. The method for preparing graphene conductive adhesive by recycling graphene film composite water-based resin according to claim 1, characterized in that: In the step (3), the ratio of sodium chloride, formic acid and water is 1:3.2:2.2, and stirring is performed at 500 r / min for 30 min.
4. The method for preparing graphene conductive adhesive by recycling graphene film composite water-based resin according to claim 3, characterized in that: In the step (3), the nanocellulose solvent and the microcrystalline nanofibers are ultrasonically dispersed at room temperature for 30 minutes and at high speed for 1 hour.
5. The method for preparing graphene conductive adhesive by recycling graphene film composite water-based resin according to claim 1, characterized in that: In the step (4), the graphene membrane waste dispersion and the microcrystalline nanofiber dispersion are ultrasonically treated for 30 minutes and stirred at 500 r / min for 20 minutes.
6. The method for preparing graphene conductive adhesive by recycling graphene film composite water-based resin according to claim 1, characterized in that: In the step (5), the mass ratio of hydrazine hydrate to the graphene membrane waste dispersion is 1:500, and the mass ratio of ammonia water to hydrazine hydrate is 5:
1. Hydrazine hydrate and ammonia water are added successively to the mixed solution of the recovered graphene membrane waste and microcrystalline nanofibers under stirring at 300 r / min, and stirred at 85°C and 500 r / min for 2 hours.
7. The method for preparing graphene conductive adhesive by recycling graphene film composite water-based resin according to claim 1, characterized in that: The water-based resin in step (6) includes water-based epoxy ester, water-based polyurethane, and water-based acrylic resin.
8. The method for preparing graphene conductive adhesive by recycling graphene film composite water-based resin according to claim 7, characterized in that: In the step (6), the leveling agent is a modified dimethyl silicone polymer, the catalyst is an organic-inorganic modified nano polymer, the defoaming agent is a non-ionic surfactant polymer, and the accelerator is a modified epoxy phosphate polymer.
9. The method for preparing graphene conductive adhesive by recycling graphene film composite water-based resin according to claim 8, characterized in that: In the step (6), during the stirring of graphene and one or two of the water-based epoxy ester, water-based polyurethane, and water-based acrylic resin at 500 r / min, 1.5% to 2% of leveling agent, 1.5% to 2% of catalyst, 1.5% to 2% of defoaming agent, and 1.5% to 2% of accelerator are added, and the mixture is stirred at 800 r / min for 1 hour.
10. The method for preparing graphene conductive adhesive by recycling graphene film composite water-based resin according to claim 1, characterized in that: The graphene conductive film coated / impregnated in step (7) is baked in a drying oven at 60° C. for 1 hour.