High-thermal-conductivity organic silicon electronic pouring sealant for power module and preparation method of high-thermal-conductivity organic silicon electronic pouring sealant

Solve by combining single-ended vinyl polydimethylsiloxane with double-ended vinyl polydimethylsiloxane in silicone thermal flame retardant potting agents, combined with specific crosslinking agents and filler treatment agents The problem of difficult to take into account both thermal conductivity and mechanical properties is achieved, and potting glue with high thermal conductivity, low thermal expansion, excellent mechanical properties and easy processing is achieved.

CN118995127APending Publication Date: 2024-11-22北京中天鹏宇科技发展有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411133630.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-19
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

Existing silicone thermal flame retardant potting adhesives are difficult to take into account both thermal conductivity and mechanical properties, which leads to the inability to effectively resist heat accumulation and vibration damage in high-precision devices, and the high viscosity is not conducive to potting operations.

Method used

Single-ended vinyl polydimethylsiloxane and double-ended vinyl polydimethylsiloxane with different viscosity are used as the basic polymer, and hydrogen-containing silicone oil with hydrogen containing both end groups and side chains is used as cross-linked. For agents and chain extenders, vinyl silicone resin is used as reinforcement agents, and long-chain vinyl modified silicone is used as filler treatment agents to form potting adhesives with high thermal conductivity, low linear thermal expansion coefficient and excellent mechanical properties.

Benefits of technology

实现了导热系数≥3.0W.m-1.K-1、线性热膨胀系数≤110μm/(m.℃)、UL 94V0级阻燃性能、较高的拉伸强度和断裂伸长率,适合高功率器件的散热和抗热疲劳需求,同时便于拆卸返修和加工。

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118995127A_ABST
    Figure CN118995127A_ABST
Patent Text Reader

Abstract

The invention discloses a high-thermal-conductivity organic silicon electronic pouring sealant for a power module. The high-thermal-conductivity organic silicon electronic pouring sealant comprises a component A and a component B, the component A is prepared from the following components in parts by weight: 0.5 to 10 parts of basic polymer, 0.15 to 10 parts of silicon resin, 0.5 to 5 parts of plasticizer, 0.01 to 0.2 part of color paste, 70 to 120 parts of heat-conducting filler, 2 to 8 parts of filler treating agent and 0.1 to 2 parts of catalyst; the component B is prepared from the following components in parts by weight: 0.5 to 10 parts of basic polymer, 0.15 to 10 parts of silicon resin, 0.5 to 5 parts of plasticizer, 70 to 120 parts of heat-conducting filler, 0.1 to 10 parts of cross-linking agent, 0.1 to 10 parts of chain extender and 0.01 to 1 part of cross-linking inhibitor; the invention further discloses a preparation method and application of the high-thermal-conductivity organic silicon electronic pouring sealant for the power module. The tensile strength and the elongation at break of the high-thermal-conductivity and high-flame-retardancy pouring sealant are improved, and the pouring sealant has a good damping effect, is convenient to disassemble and repair and has good processability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of potting adhesives, and in particular to a high thermal conductivity organic silicon electronic potting adhesive for a power module and a preparation method thereof. Background Art

[0002] As electronic products, especially new energy-saving products such as LED and solar energy, develop towards high power, the heat generated by electronic components in accessories increases, and it is urgent to transfer the heat generated to the outside world to avoid burning the electronic components due to heat accumulation. At the same time, these accessories are directly exposed to the atmosphere and are constantly exposed to alternating cold, hot, dry and wet conditions. They need to be encapsulated with organic silicone that is moisture-proof, dust-proof and oil-proof to extend their service life.

[0003] Thermally conductive flame retardant potting glue is commonly used in new energy start-stop batteries and their modules, electronic components and drive power supplies. With the development of science and technology, the industry has put forward higher and higher requirements on the thermal conductivity, tensile strength, deformation resistance, disassembly and repair process application performance of potting materials. The thermal conductivity of silicone materials without filling and modification is only 0.2Wm -1 .K -1 It is difficult to meet the thermal conductivity requirements of high-power, intensive electronic devices. Therefore, in actual use, it is usually modified by adding thermal conductive fillers to achieve the purpose of thermal conductivity.

[0004] However, with the increase of thermal conductive fillers, the tensile and other mechanical properties of thermal conductive flame retardant potting glue have decreased accordingly. Currently, the silicone thermal conductive flame retardant potting glue on the market basically uses double-terminal vinyl polydimethylsiloxane as the base glue and side chain hydrogen silicone oil as the cross-linking agent. The potting glue obtained has imperfect performance and it is difficult to take into account both thermal conductivity and tensile and other mechanical properties at the same time. It is difficult to effectively protect high-precision devices such as power modules with increasing power from internal heat accumulation damage and external vibration damage.

[0005] Moreover, most commercially available silicone heat-conductive flame-retardant potting adhesives have high viscosity, which is not conducive to potting operations and has poor process applicability. In addition, the prior art CN 112940674B discloses a high-temperature resistant flame-retardant silicone potting adhesive, which has good high-temperature stability and flame retardant properties, but the use of a side-chain hydrogen-containing cross-linking agent results in a high hardness of the potting adhesive product, which is difficult to disassemble and repair, and has poor shock absorption effect. Summary of the invention

[0006] The object of the present invention is to provide a high thermal conductivity organic silicon electronic potting glue for power module and a preparation method thereof, so as to solve the technical problem that it is difficult to take both the thermal conductivity and mechanical properties of the potting glue into consideration at the same time in the prior art.

[0007] In order to solve the above technical problems, the present invention specifically provides the following technical solutions:

[0008] The present invention provides a high thermal conductivity organic silicon electronic potting adhesive for a power module, comprising component A and component B;

[0009] In parts by weight, the component A includes: 0.5-10 parts of base polymer, 0.15-10 parts of silicone resin, 0.5-5 parts of plasticizer, 0.01-0.2 parts of color paste, 70-120 parts of thermal conductive filler, 2-8 parts of filler treatment agent, and 0.1-2 parts of catalyst;

[0010] In parts by weight, the B component includes: 0.5-10 parts of base polymer, 0.15-10 parts of silicone resin, 0.5-5 parts of plasticizer, 70-120 parts of thermal conductive filler, 0.1-10 parts of crosslinking agent, 0.1-10 parts of chain extender, and 0.01-1 parts of crosslinking inhibitor;

[0011] Wherein, the crosslinking agent is a hydrogen-containing silicone oil containing hydrogen in both the end group and the side chain, and the structural formula is shown in Formula I:

[0012]

[0013] The chain extender is a hydrogen-containing silicone oil with hydrogen at both ends, and the structural formula is shown in Formula II:

[0014]

[0015] When the hydrogen-containing silicone oil containing hydrogen in both the end group and the side chain is mixed with the base polymer, an addition cross-linking reaction is carried out to form a three-dimensional network structure;

[0016] The double-terminal hydrogen-containing silicone oil lengthens the molecular chain of the base polymer and reduces the cross-linking density of the three-dimensional network structure;

[0017] The hydrogen-containing silicone oil containing hydrogen in both the end group and the side chain has a dynamic viscosity of 10-500 mPa.s at 25°C and a hydrogen content of 0.01-1 wt%;

[0018] The dual-end hydrogen-containing silicone oil has a dynamic viscosity of 10-500 mPa.s at 25° C. and a hydrogen content of 0.01-1 wt %.

[0019] As a preferred embodiment of the present invention, the base polymer is composed of a mixture of low-viscosity dual-terminal vinyl polydimethylsiloxane, high-viscosity dual-terminal vinyl polydimethylsiloxane and single-terminal vinyl polydimethylsiloxane;

[0020] The double-terminated vinyl polydimethylsiloxane structural formula is shown in Formula III:

[0021]

[0022] The structural formula of the single-end vinyl polydimethylsiloxane is shown in Formula IV:

[0023]

[0024] As a preferred embodiment of the present invention, the low viscosity dual-end vinyl polydimethylsiloxane has a dynamic viscosity of 50 mPa.s at 25°C;

[0025] The high viscosity dual-terminated vinyl polydimethylsiloxane has a dynamic viscosity of 300-1000 mPa.s at 25°C.

[0026] As a preferred embodiment of the present invention, the silicone resin is vinyl silicone resin;

[0027] The vinyl silicone resin has an M / Q ratio of 0.5-1, a resin content of 20%-70%, a dynamic viscosity of 5000-10000 mPa.s at 25° C., and a vinyl content of 0.4-2wt%.

[0028] As a preferred embodiment of the present invention, the plasticizer is methyl silicone oil, and the dynamic viscosity at 25° C. is 10-10000 mPa.s.

[0029] The color paste is selected from any one or more of blue paste, black paste, red paste and pink paste;

[0030] The thermally conductive filler is selected from any one or more of alumina, magnesium oxide, silicon powder, kaolin, fused quartz powder, boron nitride, silicon carbide, aluminum nitride, and zirconium boride;

[0031] Wherein, the thermally conductive powder is any one or more of particles, fibers, whiskers, and chips.

[0032] As a preferred solution of the present invention, the filler treatment agent is vinyl-modified siloxane, with a dynamic viscosity of 10-60 mPa.s at 25° C. and a vinyl content of 0.5-1.5 wt %.

[0033] As a preferred embodiment of the present invention, the catalyst is a platinum catalyst or dibutyltin dilaurate.

[0034] Wherein, the platinum catalyst is a platinum-based catalyst;

[0035] Wherein, the platinum-based catalyst is selected from one or any several of chloroplatinic acid, platinum tetrachloride, an alcohol solution of chloroplatinic acid, a platinum-olefin complex, a platinum-alkenylsiloxane complex and a platinum-carbonyl complex;

[0036] The cross-linking inhibitor is one or any combination of alkynol compounds, alkenyl ring bodies and alkenyl double heads.

[0037] The present invention also provides a method for preparing a high thermal conductivity organic silicon electronic potting adhesive for a power module, comprising the following steps:

[0038] Add silicone resin, plasticizer, color paste and thermal conductive filler to the base polymer in sequence, stir and blend at 20-35° C. for 60-120 minutes, and then heat and dehydrate at 100-150° C. and stir and blend for 120-180 minutes to obtain base slurry A;

[0039] The base slurry A is cooled to room temperature, and a filler treatment agent and a catalyst are added in sequence, and the mixture is stirred and blended at 20-25° C. for 5-10 minutes to obtain the component A;

[0040] Add silicone resin, plasticizer and thermal conductive filler to the base polymer in sequence, stir and blend at 20-35° C. for 60-120 minutes, and then heat and dehydrate at 100-150° C. and stir and blend for 120-180 minutes to obtain matrix slurry B;

[0041] The base slurry B is cooled to room temperature, and a crosslinking agent, a chain extender, and a crosslinking inhibitor are added in sequence, and the mixture is stirred and blended at 20-25° C. for 5-10 minutes to obtain the B component.

[0042] As a preferred embodiment of the present invention, when preparing the matrix slurry A, the stirring speed is 400-450 r / min at 20-35°C, and the stirring speed is 600-900 r / min at 100-150°C;

[0043] When preparing the A component, the stirring speed is 400-450r / min at 20-25°C;

[0044] When preparing the matrix slurry B, the stirring speed is 400-450 r / min at 20-35° C., and the stirring speed is 600-900 r / min at 100-150° C.;

[0045] When preparing the B component, the stirring speed is 400-450 r / min at 20-25°C.

[0046] The present invention also provides an application of a high thermal conductivity organic silicon electronic potting adhesive for a power module. When used, the component A and the component B can be mixed at a volume ratio or mass ratio of 1: (0.8-1.2).

[0047] Compared with the prior art, the present invention has the following beneficial effects:

[0048] The present invention uses single-terminal vinyl polydimethylsiloxane and double-terminal vinyl polydimethylsiloxane of different viscosities as the base polymer. Low-viscosity double-terminal vinyl polydimethylsiloxane can make the system have a suitable potting viscosity and a high filler filling amount required for high thermal conductivity, thereby ensuring the thermal conductivity of the system; at the same time, high-viscosity double-terminal vinyl polydimethylsiloxane has a longer molecular chain, and the cross-linking density of the three-dimensional network structure is reduced, so that the prepared organic silicone potting glue material has a higher elongation, thereby improving the system's anti-displacement deformation ability; at the same time, the use of single-terminal vinyl polydimethylsiloxane increases the randomness of the system cross-linking, makes the cross-linking more uniform, and further improves the comprehensive mechanical properties of the system.

[0049] The present invention adopts hydrogen-containing silicone oil containing hydrogen in both the end group and the side chain as a crosslinking agent. The crosslinking agent containing hydrogen in both the end group and the side chain undergoes multiple addition crosslinking with the base polymer to form a three-dimensional network structure. Compared with the traditional side chain hydrogen-containing crosslinking agent, the crosslinking agent has multiple directions and a high degree of crosslinking, so that the short branched chain structure in the crosslinked network is more evenly distributed, showing more excellent mechanical properties, tensile properties and fracture toughness.

[0050] The present invention specifically selects hydrogen-containing silicone oil with double end groups as a chain extender. The hydrogen-containing silicone oil with double end groups can be used in combination with a cross-linking agent containing hydrogen in both the end groups and the side chains. The hydrogen-containing silicone oil with double end groups can lengthen the molecular chain of the base polymer linearly while cross-linking the organosilicon potting adhesive material, and reduce the cross-linking density of the three-dimensional network structure, so that the prepared organosilicon potting adhesive material has a higher elongation and achieves a high anti-displacement deformation ability.

[0051] The present invention uses vinyl silicone resin as a reinforcing agent. Vinyl silicone resin can be dissolved in room temperature vulcanized silicone rubber, and will not significantly increase the viscosity of the system after being added. At the same time, the vinyl group can also participate in the hydrosilylation reaction, thereby increasing the crosslinking density of the system and reinforcing the mechanical properties of the system.

[0052] The present invention specifically selects long-chain vinyl-modified siloxane as a filler treatment agent. On the one hand, the treatment agent can completely wrap the filler particles, improve the surface plasticity of the filler particles, and have good compatibility with the matrix interface, and the system fluidity is good. On the other hand, the vinyl in the treatment agent can also participate in the hydrosilylation reaction to form a cross-linked network with the silicone matrix, increase the interface bonding force between the filler and the matrix cross-linked network, and improve the mechanical properties of the silicone potting material.

[0053] The present invention can adjust the viscosity and performance of the product by selecting the viscosity, vinyl position and content of the vinyl polydimethylsiloxane, so that the product can meet the needs of different usage scenarios.

[0054] The present invention discloses a variety of preferred formula materials and proportions, and the obtained high thermal conductivity organic silicon electronic potting glue for power module has excellent comprehensive performance. It has excellent thermal conductivity (thermal conductivity coefficient ≥3.0Wm -1 .K -1 ), low linear thermal expansion coefficient (≤110μm / (m.℃)), excellent flame retardant properties (UL 94V0 level, 2.0mm thickness), high tensile strength and high elongation at break, good shock absorption effect, easy disassembly and repair, and good processing performance.

[0055] The invention discloses a method for preparing a high-thermal-conductivity organic silicon electronic potting adhesive for a power module. The preparation process is simple and easy to control, has little environmental pollution, and is easy to industrialize and expand production. BRIEF DESCRIPTION OF THE DRAWINGS

[0056] In order to more clearly illustrate the implementation methods of the present invention or the technical solutions in the prior art, the following briefly introduces the drawings required for the implementation methods or the description of the prior art. Obviously, the drawings in the following description are only exemplary, and for ordinary technicians in this field, other implementation drawings can be derived from the provided drawings without creative work.

[0057] Figure 1 The present invention provides a flow chart of a method for preparing a high thermal conductivity organic silicon electronic potting adhesive for a power module. DETAILED DESCRIPTION

[0058] The technical scheme in the embodiment of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiment of the present invention. Obviously, the described embodiment is only a part of the embodiment of the present invention, not all of the embodiments. Based on the embodiment of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0059] The invention provides a high-thermal-conductivity organic silicon electronic potting adhesive for a power module, comprising a component A and a component B. When in use, the component A and the component B are mixed for use.

[0060] In parts by weight, the component A includes: 0.5-10 parts of base polymer, 0.15-10 parts of silicone resin, 0.5-5 parts of plasticizer, 0.01-0.2 parts of color paste, 70-120 parts of thermal conductive filler, 2-8 parts of filler treatment agent, and 0.1-2 parts of catalyst.

[0061] In parts by weight, the B component includes: 0.5-10 parts of base polymer, 0.15-10 parts of silicone resin, 0.5-5 parts of plasticizer, 70-120 parts of thermal conductive filler, 0.1-10 parts of crosslinking agent, 0.1-10 parts of chain extender, and 0.01-1 parts of crosslinking inhibitor.

[0062] Different from general potting glue, the potting glue in the present invention uses hydrogen-containing silicone oil containing hydrogen in both the end group and the side chain as a crosslinking agent. The hydrogen content of the crosslinking agent refers to the percentage of the mass of the hydrogen group in the total mass of the molecule, and the end side hydrogen content in the crosslinking agent refers to the hydrogen group being directly connected to the silicon atom. The structural formula of the crosslinking agent is shown in Formula I:

[0063]

[0064] The role of the cross-linking agent is explained in detail below.

[0065] The crosslinking agent containing hydrogen at both the end group and the side chain undergoes addition crosslinking with the base polymer to form a network structure. In particular, the end group containing hydrogen in the structure containing hydrogen at both the end group and the side chain can increase the soft segment and increase the elasticity, and the side chain containing hydrogen can provide a special crosslinking network, which can undergo addition crosslinking with vinyl polydimethylsiloxane, crosslink with vinyl polydimethylsiloxane and vinyl polydimethylsiloxane containing vinyl after chain extension, and crosslink with vinyl polydimethylsiloxane and crosslinked vinyl containing hydrogen at both the end group and the side chain to form a three-dimensional network structure. The crosslinking agent containing hydrogen at both the end group and the side chain makes the crosslinking direction of the crosslinking agent multivariate and the degree of crosslinking high, and the material exhibits excellent mechanical properties, tensile properties and fracture toughness.

[0066] Traditional side chain hydrogen-containing crosslinking agents have a single crosslinking direction and low crosslinking efficiency, and require a higher amount of addition to achieve a sufficient crosslinking effect. However, the increase in dosage leads to increased hardness, poor elasticity, or even loss of elasticity, and poor stress and strain resistance.

[0067] The cross-linking agent used in the present invention contains hydrogen at both the end group and the side chain, and can undergo addition cross-linking with vinyl polydimethylsiloxane at both the chain end and the side chain, with a high degree of cross-linking, so that the short branched chain structure in the cross-linked network is more evenly distributed; and due to the characteristics of the molecular structure and the action of intermolecular forces, the formed cross-linked structure has a higher degree of randomness, forming a special three-dimensional cross-linked network structure, so that the potting glue product exhibits better strength and flexibility.

[0068] Preferably, the cross-linking agent has a dynamic viscosity of 10-500 mPa.s at 25°C, and further preferably, the cross-linking agent has a dynamic viscosity of 30-90 mPa.s at 25°C; for example, the cross-linking agent has a dynamic viscosity of 30 mPa.s, 86 mPa.s at 25°C.

[0069] Preferably, the hydrogen content of the cross-linking agent is 0.01-1 wt %; further preferably, the hydrogen content of the cross-linking agent is 0.7-0.9 wt %; for example, the hydrogen content of the cross-linking agent is 0.81 wt %, 0.82 wt %.

[0070] However, the present application does not simply add a cross-linking agent containing hydrogen at both the end group and the side chain, wherein a specifically selected chain extender can be used in conjunction with a cross-linking agent containing hydrogen at both the end group and the side chain.

[0071] The chain extender is a hydrogen-containing silicone oil with double-end hydrogen, and its structural formula is shown in Formula II:

[0072]

[0073] The double-terminal hydrogen-containing silicone oil makes the silicone potting material cross-linked, while the basic polymer molecular chain is linearly lengthened and the cross-linking density of the three-dimensional network structure is reduced, so that the prepared silicone potting material has a higher elongation and achieves high resistance to displacement deformation.

[0074] Preferably, the chain extender has a kinetic viscosity of 10-500 mPa.s at 25°C; further preferably, the chain extender has a kinetic viscosity of 80-100 mPa.s at 25°C; for example, the chain extender has a kinetic viscosity of 85 mPa.s at 25°C.

[0075] Preferably, the hydrogen content of the chain extender is 0.01-1 wt %; further preferably, the hydrogen content of the chain extender is 0.03-0.05 wt %; for example, the hydrogen content of the chain extender is 0.04 wt %.

[0076] In the present application, hydrogen-containing silicone oil containing hydrogen at both the end groups and the side chains is used as a cross-linking agent, and hydrogen-containing silicone oil containing hydrogen at both the end groups is used as a chain extender. The silicone thermal conductive potting adhesive prepared by cross-linking the base polymer exhibits excellent thermal conductivity, tensile strength and elongation at break, can achieve good shock-absorbing effects during use, and is also easy to disassemble and repair.

[0077] Furthermore, the base polymer is composed of a compound of low-viscosity dual-terminal vinyl polydimethylsiloxane, high-viscosity dual-terminal vinyl polydimethylsiloxane and single-terminal vinyl polydimethylsiloxane.

[0078] Double-terminated vinyl polydimethylsiloxane, the structural formula of which is shown in Formula III:

[0079]

[0080] Preferably, the dynamic viscosity of the dual-end vinyl polydimethylsiloxane at 25°C is 10-2000mPa.s; further preferably, the dynamic viscosity of the dual-end vinyl polydimethylsiloxane at 25°C is 40-1100mPa.s; for example, the dynamic viscosity of the dual-end vinyl polydimethylsiloxane at 25°C is 50mPa.s, 300mPa.s, 500mPa.s, 1000mPa.s.

[0081] Preferably, the vinyl content of the dual-terminal vinyl polydimethylsiloxane is 0.2-3.0wt%; further preferably, the vinyl content of the dual-terminal vinyl polydimethylsiloxane is 0.3-1.9wt%; for example, the vinyl content of the dual-terminal vinyl polydimethylsiloxane is 0.32wt%, 0.43wt%, 0.57wt%, 1.85wt%.

[0082] Single-end vinyl polydimethylsiloxane, the structural formula of which is shown in Formula IV:

[0083]

[0084] Preferably, the single-ended vinyl polydimethylsiloxane has a dynamic viscosity of 500-2500 mPa.s at 25°C; further preferably, the single-ended vinyl polydimethylsiloxane has a dynamic viscosity of 800-2000 mPa.s at 25°C; for example, the single-ended vinyl polydimethylsiloxane has a dynamic viscosity of 1000 mPa.s, 2000 mPa.s at 25°C.

[0085] Preferably, the vinyl content of the single-terminal vinyl polydimethylsiloxane is 0.05-0.5wt%; further preferably, the vinyl content of the single-terminal vinyl polydimethylsiloxane is 0.08-0.3wt%; for example, the vinyl content of the single-terminal vinyl polydimethylsiloxane is 0.1wt%, 0.23wt%.

[0086] In the above description, the dual-end vinyl polydimethylsiloxane with a viscosity lower than or equal to 50 mPa.s is a low-viscosity dual-end vinyl polydimethylsiloxane, and the dual-end vinyl polydimethylsiloxane with a viscosity higher than or equal to 300 mPa.s is a high-viscosity dual-end vinyl polydimethylsiloxane.

[0087] Further, the low viscosity dual-terminated vinyl polydimethylsiloxane has a dynamic viscosity of 50 mPa.s at 25°C;

[0088] The high viscosity dual-terminated vinyl polydimethylsiloxane has a dynamic viscosity of 300-1000 mPa.s at 25°C.

[0089] Preferably, the mass ratio of the low-viscosity dual-end vinyl polydimethylsiloxane with a dynamic viscosity of 50 mPa.s at 25°C to the high-viscosity dual-end vinyl polydimethylsiloxane with a dynamic viscosity of 300 mPa.s at 25°C is 25:(0.5-10); more preferably, it is 25:9.

[0090] Preferably, the mass ratio of the low-viscosity dual-end vinyl polydimethylsiloxane with a dynamic viscosity of 50 mPa.s at 25°C to the high-viscosity dual-end vinyl polydimethylsiloxane with a dynamic viscosity of 1000 mPa.s at 25°C is 25:(0.5-10); more preferably, it is 25:9.

[0091] A high filling amount of thermally conductive filler is a simple means to achieve high thermal conductivity, high flame retardancy and low linear thermal expansion coefficient, but it is inevitable that a high filling amount will inevitably lead to a corresponding increase in the viscosity of the system, a decrease in fluidity, uneven or unbalanced matrix cross-linking network and cross-linking density, and a corresponding deterioration in the mechanical properties of the system. In the same formula, under the condition of ensuring a certain filler filling amount to ensure thermal conductivity, the viscosity and performance of the product can be regulated by selecting the viscosity of vinyl polydimethylsiloxane and the position and content of the vinyl. That is, while ensuring that the potting compound has high thermal conductivity, high flame retardancy and low linear thermal expansion coefficient, different vinyl polydimethylsiloxanes can change the final viscosity, tensile strength, elongation at break, etc. of the potting compound to a certain extent, so that it can adapt to the needs of different usage scenarios.

[0092] It is also further explained that low-viscosity double-ended vinyl polydimethylsiloxane, high-viscosity double-ended vinyl polydimethylsiloxane and single-ended vinyl polydimethylsiloxane are indeed compounded as the base polymer, hydrogen-containing silicone oil with hydrogen in both the end group and the side chain is used as a cross-linking agent, and hydrogen-containing silicone oil with hydrogen in the double end group is used as a chain extender, which can change the viscosity and mechanical properties of the entire potting glue system while ensuring that it has a higher thermal conductivity, a higher flame retardant level and a lower linear thermal expansion coefficient.

[0093] That is, the low-viscosity double-terminal vinyl polydimethylsiloxane, high-viscosity double-terminal vinyl polydimethylsiloxane and single-terminal vinyl polydimethylsiloxane are compounded as the base polymer, the hydrogen-containing silicone oil containing hydrogen on both the end group and the side chain is used as a cross-linking agent, and the hydrogen-containing silicone oil containing hydrogen on the double end group is used as a chain extender. As a potting compound formula, it can be adapted to the potting compound with a high concentration of fillers, and the influence of the filler concentration on the tensile properties and fracture toughness of the potting compound is reduced, so that the potting compound can take into account both thermal conductivity and mechanical properties.

[0094] The present invention selects vinyl polydimethylsiloxane with specific viscosity and vinyl content as raw material to regulate the viscosity of the potting glue product to meet different usage requirements. The present invention can regulate the viscosity and performance of the product by selecting the viscosity, vinyl position and content of the vinyl polydimethylsiloxane, so that it can adapt to the needs of different usage scenarios. Low-viscosity double-ended vinyl polydimethylsiloxane can make the system have a suitable potting viscosity and a high filler filling amount required for high thermal conductivity, ensuring the thermal conductivity of the system; at the same time, high-viscosity double-ended vinyl polydimethylsiloxane has a longer molecular chain, which can improve the mechanical properties of the system; at the same time, the use of single-ended vinyl polydimethylsiloxane can increase the randomness of the system cross-linking and make the cross-linking more uniform, further improving the comprehensive mechanical properties of the system.

[0095] In the system of the present invention, a potting glue product with a dynamic viscosity below 10000 mPa.s can be obtained, which has good operating performance during use. At the same time, the product maintains a high thermal conductivity, has good tensile strength and elongation at break, and has good comprehensive performance.

[0096] In the present invention, the silicone resin can be selected within any range, but in order to improve the mechanical properties of the silicone rubber, preferably, the silicone resin is a vinyl MQ silicone resin; further preferably, the silicone resin has an M / Q ratio of 0.5-1, a resin content of 20%-70%, a dynamic viscosity at 25°C of 5000-10000 mPa.s, and a vinyl content of 0.4-2wt%; for example, the silicone resin has an M / Q ratio of 0.8, a resin content of 50%, a dynamic viscosity at 25°C of 6300-7300 mPa.s, and a vinyl content of 0.94-0.98wt%.

[0097] MQ silicone resin can be used as a reinforcing agent for addition-type silicone rubber to improve the mechanical properties of silicone rubber. MQ silicone resin is a kind of silicone rubber composed of monofunctional silicon oxygen units (R3SiO 1 / 2 M) and tetrafunctional silicon-oxygen unit (SiO 4 / 2 MQ silicone resin is a special polysiloxane formed by hydrolysis and condensation of MQ silicone resin. Compared with traditional reinforcing fillers, MQ silicone resin has the following advantages and characteristics: it can be dissolved in room temperature vulcanized silicone rubber, and the viscosity of the system will not be significantly increased after addition. At the same time, MQ silicone resin containing vinyl or silane groups can also participate in silane hydrogen addition reaction, thereby increasing the crosslinking density of the system and reinforcing the mechanical properties of the system.

[0098] There are three main types of MQ silicone resins commonly used in addition-type liquid silicone rubber: (1) MQ silicone resins containing vinyl groups; (2) MQ silicone resins containing Si-H bonds; and (3) MQ silicone resins containing Me2SiO segments and vinyl groups. In MQ silicone resins, the molar ratio of M to Q determines the size of the resin molecular configuration. The smaller the M ratio, the larger the resin configuration. To ensure that the solubility of silicone resins in addition-type rubbers is appropriate, the molar ratio of M to Q is usually (0.5-1.0):1. The greatest influence of MQ silicone resins on addition-type vulcanized silicone rubber is its dosage and its vinyl content.

[0099] In the present invention, the plasticizer can be selected within any range, but in order to improve the mechanical properties of the silicone rubber, preferably, the plasticizer is methyl silicone oil; further preferably, the dynamic viscosity of the methyl silicone oil at 25°C is 10-10000 mPa.s; for example, the dynamic viscosity of the methyl silicone oil at 25°C is 50 mPa.s, 100 mPa.s, 500 mPa.s.

[0100] In the present invention, the color paste can be selected within any range. Preferably, the color paste is selected from any one or more of blue paste, black paste, red paste and pink paste.

[0101] In the present invention, the thermally conductive filler can be selected within any range, but in order to improve the thermal conductivity of the silicone rubber, preferably, the thermally conductive filler is selected from any one or more of alumina, magnesium oxide, silica powder, kaolin, fused quartz powder, boron nitride, silicon carbide, aluminum nitride, and zirconium boride.

[0102] Wherein, the thermally conductive filler is any one or more of particles, fibers, whiskers, and chips.

[0103] In the present invention, the filler treatment agent can be selected within any range, but in order to improve the fluidity and mechanical properties of the silicone rubber, preferably, the filler treatment agent is a long-chain vinyl-modified siloxane; further preferably, the filler treatment agent has a dynamic viscosity of 10-60 mPa.s at 25°C and a vinyl content of 0.5-1.5 wt%; for example, the filler treatment agent has a dynamic viscosity of 27-30 mPa.s at 25°C and a vinyl content of 0.8 wt%.

[0104] The surface of the thermally conductive inorganic filler is coated with an organic treatment agent, which can improve the interface compatibility between the filler particles and the organic matrix. When the molecular chain of the organic treatment agent is long enough, the organic matter can completely wrap the filler particles, and can also better entangle with the organic matrix polymer chain, effectively improving the interface compatibility between the filler particles and the matrix, and improving the fluidity of the system. On the one hand, the long-chain vinyl-modified siloxane used in the present invention can completely wrap the filler particles, so that the filler particles and the matrix interface are well compatible, and the system fluidity is good. On the other hand, the vinyl in the treatment agent can also participate in the hydrosilylation reaction to form a cross-linked network with the silicone matrix, increase the interface bonding force between the filler and the matrix cross-linked network, and improve the mechanical properties of the silicone potting compound.

[0105] In the present invention, the catalyst can be selected within any range, but in order to improve the mechanical properties of the silicone potting compound, preferably, the catalyst is a platinum catalyst or dibutyltin dilaurate.

[0106] Wherein, the platinum catalyst is selected from platinum-based catalysts.

[0107] Wherein, the platinum-based catalyst is selected from one or any several of chloroplatinic acid, platinum tetrachloride, alcohol solution of chloroplatinic acid, platinum-olefin complex, platinum-alkenylsiloxane complex and platinum-carbonyl complex.

[0108] Further preferably, the platinum catalyst is selected from one or more of Karstedt's catalyst (1,3-divinyl-1,1,3,3-tetramethyldisiloxane platinum (0), CAS: 68478-92-2), an isopropanol solution of chloroplatinic acid (Speier's catalyst), a tetrahydrofuran-coordinated platinum catalyst and a divinyltetramethylsiloxane-coordinated platinum catalyst.

[0109] In the two-component addition-type silicone thermally conductive potting adhesive, the catalyst is preferably a platinum-based catalyst, selected from one or more of chloroplatinic acid, platinum tetrachloride, an alcohol solution of chloroplatinic acid, a platinum-olefin complex, a platinum-alkenylsiloxane complex and a platinum-carbonyl complex, and the amount used is not particularly limited.

[0110] Preferably, the platinum content in the platinum catalyst is 2000-200000 ppm; more preferably, it is 3000 ppm.

[0111] In the present invention, the crosslinking inhibitor can be selected within any range, but in order to improve the mechanical properties of the silicone rubber, preferably, the crosslinking inhibitor is one or any combination of acetylenic alcohol compounds, alkenyl ring bodies and alkenyl double heads.

[0112] Further preferably, the crosslinking inhibitor is selected from one or more of 2-methyl-3-butyn-2-ol, 2-methyl-1-hexyn-3-ol, 3,5-dimethyl-1-hexyn-3-ol, 1-ethynyl-1-cyclohexanol, 2-phenyl-3-butyn-2-ol, ethynylcyclohexanol, and tetramethyltetravinylcyclotetrasiloxane. The amount of the inhibitor is not particularly limited.

[0113] The high thermal conductivity organic silicon electronic potting adhesive for the power module provided by the present invention has excellent comprehensive properties of high thermal conductivity, low linear thermal expansion coefficient, high flame retardancy, high tensile strength and high elongation at break.

[0114] like Figure 1 As shown, the present invention provides a method for preparing a high thermal conductivity organic silicon electronic potting adhesive for a power module, comprising the following steps:

[0115] Add silicone resin, plasticizer, color paste and thermal conductive filler to the base polymer in sequence, stir and blend at 20-35° C. for 60-120 minutes, and then heat and dehydrate at 100-150° C. and stir and blend for 120-180 minutes to obtain base slurry A;

[0116] The base slurry A is cooled to room temperature, and a filler treatment agent and a catalyst are added in sequence, and the mixture is stirred and blended at 20-25° C. for 5-10 minutes to obtain the component A;

[0117] Add silicone resin, plasticizer and thermal conductive filler to the base polymer in sequence, stir and blend at 20-35° C. for 60-120 minutes, and then heat and dehydrate at 100-150° C. and stir and blend for 120-180 minutes to obtain matrix slurry B;

[0118] The base slurry B is cooled to room temperature, and a crosslinking agent, a chain extender, and a crosslinking inhibitor are added in sequence, and the mixture is stirred and blended at 20-25° C. for 5-10 minutes to obtain the B component.

[0119] Preferably, the specific operation of stirring and blending is: when preparing matrix slurry A or matrix slurry B, stirring and blending at a speed of 400-450r / min at 20-35°C for 60-120 minutes; then heating to 100-150°C, gradually increasing the stirring speed to 600-900r / min, stirring and blending for 120-180 minutes.

[0120] Preferably, after the matrix slurry A or the matrix slurry B is cooled to room temperature, the corresponding additives are added, and the mixture is stirred and blended at 20-25° C. and a speed of 400-450 r / min for 5-10 minutes to obtain the component A or the component B.

[0121] Preferably, the matrix slurry A or matrix slurry B is subsequently added after being cooled to below 30°C.

[0122] The invention can prepare the high thermal conductivity organic silicon electronic potting glue for power module through a simple stirring process, the above raw materials can be directly mixed, and the reaction process does not require long-term high temperature, and the production safety is high. In addition, the preparation method of the invention takes a short time, is conducive to saving energy consumption and space costs, and has great industrial value.

[0123] Another aspect of the present invention provides an application of the above-mentioned high thermal conductivity silicone electronic potting glue for power modules. When the potting glue is used for potting, the volume ratio or mass ratio of component A to component B is 1: (0.8-1.2).

[0124] Due to the special formula composition, the specific gravity of component A and component B is basically the same. In actual use, they can be blended in either volume ratio or mass ratio, which also improves the convenience of use.

[0125] Preferably, during the application, the volume ratio or mass ratio of component A to component B is 1:1.

[0126] The present invention specifically limits the dosage ratio of component A to component B to 1: (0.8-1.2). Under this ratio, the degree of crosslinking of the organic silicone thermally conductive flame-retardant potting glue is moderate and has good mechanical properties. If the dosage of component B is too small, the degree of crosslinking is low, resulting in the potting glue being too soft and the mechanical properties being poor; if the dosage of component B is too high, the crosslinking agent that does not participate in the crosslinking may precipitate from the system, affecting the stability and potting effect, and the hardness of the potting glue is correspondingly high, and the mechanical properties are poor.

[0127] The performance of the potting glue is described in detail by way of examples below:

[0128] The high thermal conductivity organosilicon electronic potting glue prepared from the silicone rubber composition of the present invention is tested for thermal conductivity according to ASTM D5470-17, a test method for thermal conductivity of thermally conductive electrical insulating materials. The linear thermal expansion coefficient is tested according to ASTM E831-19, a test method for linear thermal expansion of solid materials by thermomechanical analysis. The flame retardant properties are tested according to UL 94-2023, a test for plastic flammability of parts in devices and appliances. The tensile strength and elongation at break are tested according to GB / T528-2009, a test method for tensile testing of vulcanized rubber or thermoplastic rubber (dumbbell-shaped specimens). The hardness of the material is tested according to GB / T531.1-2008. The viscosity of the material is tested according to GB / T2794-2022.

[0129] Embodiment 1:

[0130] Component A:

[0131] (1) By weight, 1.25 g of a dual-terminal vinyl polydimethylsiloxane with a dynamic viscosity of 50 mPa.s at 25°C and a vinyl content of 1.85 wt% (purchased from Beijing Hangping Silicone Chemical Co., Ltd.), 0.2 g of a dual-terminal vinyl polydimethylsiloxane with a dynamic viscosity of 1000 mPa.s at 25°C and a vinyl content of 0.32 wt% (purchased from Zhejiang Runhe Silicone New Materials Co., Ltd., model RH-Vi1305), and a dynamic viscosity of 1000 mPa.s at 25°C were weighed. 0.05 g of single-end vinyl polydimethylsiloxane with a vinyl content of 0.23 wt% (purchased from Zhejiang Runhe Silicone New Materials Co., Ltd., model RH-Vi305B), 4.75 g of vinyl silicone resin, 2.5 g of plasticizer, 0.04 g of color paste, and 82.5 g of thermal conductive filler were stirred and blended at 20-35° C. and 400 r / min for 60 minutes; then the temperature was raised to 110° C., the stirring speed was gradually increased to 650 r / min, and the stirring was blended for 120 minutes to obtain matrix slurry A.

[0132] After cooling the base slurry A to below 30° C., 3 g of a vinyl filler treatment agent and 1.5 g of a platinum catalyst were added, and the mixture was stirred and blended at 20-25° C. and a speed of 400 r / min for 10 minutes to obtain the A component.

[0133] Component B:

[0134] (1) By weight, weigh 1.25 g of a dual-terminal vinyl polydimethylsiloxane with a dynamic viscosity of 50 mPa.s at 25°C and a vinyl content of 1.85 wt% (purchased from Beijing Hangping Silicone Chemical Co., Ltd.), 0.2 g of a dual-terminal vinyl polydimethylsiloxane with a dynamic viscosity of 1000 mPa.s at 25°C and a vinyl content of 0.32 wt% (purchased from Zhejiang Runhe Silicone New Materials Co., Ltd., model RH-Vi1305), and 0.5 g of a dual-terminal vinyl polydimethylsiloxane with a dynamic viscosity of 1000 mPa.s at 25°C and a vinyl content of 0.32 wt% (purchased from Zhejiang Runhe Silicone New Materials Co., Ltd., model RH-Vi1305). a.s, 0.05 g of single-end vinyl polydimethylsiloxane with a vinyl content of 0.23 wt% (purchased from Zhejiang Runhe Silicone New Materials Co., Ltd., model RH-Vi305B), 4.75 g of vinyl silicone resin, 2.5 g of plasticizer, and 82.5 g of thermal conductive filler were stirred and blended at 20-35° C. and 400 r / min for 60 minutes; then the temperature was raised to 110° C., the stirring speed was gradually increased to 650 r / min, and the stirring was blended for 120 minutes to obtain matrix slurry B.

[0135] After cooling the base slurry B to below 30° C., 0.83 g of a crosslinking agent, 1.5 g of a chain extender, and 0.05 g of a crosslinking inhibitor were added, and the mixture was stirred and blended at 20-25° C. and a speed of 400 r / min for 10 minutes to obtain the B component.

[0136] The vinyl silicone resin is vinyl MQ silicone resin with an M / Q ratio of 0.8, a resin content of 50%, a dynamic viscosity of 6800 mPa.s at 25° C., and a vinyl content of 0.96 wt %, purchased from Zhejiang Runhe Silicone New Materials Co., Ltd., model RH-S11H.

[0137] The plasticizer was methyl silicone oil with a dynamic viscosity of 50 mPa.s at 25°C, purchased from Hubei Sihai Chemical Co., Ltd.

[0138] The color paste is pink color paste purchased from Hefei Lantu Pigment Co., Ltd., model 1657R.

[0139] The thermal conductive filler is alumina, purchased from Guangdong Hengjing New Materials Co., Ltd., model EL-G302.

[0140] Vinyl filler treating agent, with a dynamic viscosity of 27-30 mPa.s at 25° C. and a vinyl content of 0.8 wt %, was purchased from Zhejiang Runhe Organic Silicone New Materials Co., Ltd., model RH-RMS-23M.

[0141] The platinum catalyst is a Karstedt platinum catalyst with a platinum content of 3000 ppm, purchased from Guangzhou Siyou New Material Technology Co., Ltd., model PT-3000.

[0142] The crosslinking agent is hydrogen-containing silicone oil containing hydrogen in both the terminal group and the side chain, with a dynamic viscosity of 30 mPa.s at 25° C. and a hydrogen content of 0.82%. It was purchased from Zhejiang Runhe Silicone New Materials Co., Ltd. and the model number is RH-LHC-3.

[0143] The chain extender is a double-terminal hydrogen-containing silicone oil with a dynamic viscosity of 85 mPa.s at 25° C. and a hydrogen content of 0.04%. It was purchased from Zhejiang Runhe Silicone New Materials Co., Ltd. and the model number is RH-DH37.

[0144] The cross-linking inhibitor was ethynyl cyclohexanol, purchased from Guangzhou Siyou New Material Technology Co., Ltd., model number YZJ-1.

[0145] When used, take equal parts of component A and component B and mix them evenly at room temperature, then degas for 20 minutes under a vacuum degree of 0.1 MPa to obtain a high thermal conductivity organic silicone electronic potting glue. The thermal conductivity of the potting glue cured product is 3.0 Wm -1 .K -1 The flame retardant grade is UL 94V-0, the linear thermal expansion coefficient is 106μm / (m.℃), the Shore A hardness is 70, the tensile strength is 2.4MPa, and the elongation at break is 29%.

[0146] Embodiment 2:

[0147] This embodiment provides a high thermal conductivity organic silicon electronic potting adhesive for a power module and a preparation method and application thereof. The implementation method is the same as that of embodiment 1, except that:

[0148] Component A includes 0.45 g of dual-end vinyl polydimethylsiloxane with a dynamic viscosity of 1000 mPa.s at 25°C and a vinyl content of 0.32 wt%, 1.8 g of single-end vinyl polydimethylsiloxane with a dynamic viscosity of 1000 mPa.s at 25°C and a vinyl content of 0.23 wt%, 0.25 g of vinyl silicone resin, 1.5 g of plasticizer, 110.5 g of thermal conductive filler, 6 g of vinyl filler treating agent, and 1.25 g of platinum catalyst.

[0149] Component B includes 0.45 g of dual-end vinyl polydimethylsiloxane with a dynamic viscosity of 1000 mPa.s at 25°C and a vinyl content of 0.32 wt%, 1.8 g of single-end vinyl polydimethylsiloxane with a dynamic viscosity of 1000 mPa.s at 25°C and a vinyl content of 0.23 wt%, 0.25 g of vinyl silicone resin, 1.5 g of plasticizer, 110.5 g of thermal conductive filler, 0.4 g of cross-linking agent, and 4 g of chain extender.

[0150] When used, take equal parts of component A and component B and mix them evenly at room temperature, then degas for 20 minutes under a vacuum degree of 0.1 MPa to obtain a high thermal conductivity silicone electronic potting glue for power modules. The thermal conductivity of the potting glue cured product is 3.2 Wm -1 .K -1 The flame retardant grade is UL 94V-0, the linear thermal expansion coefficient is 108μm / (m.℃), the Shore A hardness is 70, the tensile strength is 1.5MPa, and the elongation at break is 38%.

[0151] Embodiment 3:

[0152] This embodiment provides a high thermal conductivity organic silicon electronic potting adhesive for a power module and a preparation method and application thereof. The implementation method is the same as that of embodiment 2, except that:

[0153] Component A includes 1.25 g of vinyl silicone resin, 106 g of thermal conductive filler, and 1.5 g of platinum catalyst.

[0154] Component B includes 1.25 g of vinyl silicone resin, 106 g of thermal conductive filler, 0.61 g of crosslinking agent, and 2 g of chain extender.

[0155] When used, take equal parts of component A and component B and mix them evenly at room temperature, then degas for 20 minutes under a vacuum degree of 0.1 MPa to obtain a high thermal conductivity organic silicone electronic potting glue. The thermal conductivity of the potting glue cured product is 3.1 Wm -1 .K -1The flame retardant grade is UL 94V-0, the linear thermal expansion coefficient is 107μm / (m.℃), the Shore A hardness is 71, the tensile strength is 2.4MPa, and the elongation at break is 27%.

[0156] Embodiment 4:

[0157] This embodiment provides a high thermal conductivity organic silicon electronic potting adhesive for a power module and a preparation method and application thereof. The implementation method is the same as that of embodiment 2, except that:

[0158] Component A contains 0.75 g of vinyl silicone resin and 1.0 g of platinum catalyst.

[0159] Component B contains 0.75 g of vinyl silicone resin, 0.5 g of crosslinking agent, and 3 g of chain extender.

[0160] When used, take equal parts of component A and component B and mix them evenly at room temperature, then degas for 20 minutes under a vacuum degree of 0.1 MPa to obtain a high thermal conductivity organic silicone electronic potting glue. The thermal conductivity of the potting glue cured product is 3.2 Wm -1 .K -1 The flame retardant grade is UL 94V-0, the linear thermal expansion coefficient is 104μm / (m.℃), the Shore A hardness is 70, the tensile strength is 2.4MPa, and the elongation at break is 33%.

[0161] Embodiment 5:

[0162] This embodiment provides a high thermal conductivity organic silicon electronic potting adhesive for a power module and a preparation method and application thereof. The implementation method is the same as that of embodiment 2, except that:

[0163] Component A includes 0.05 g of dual-end vinyl polydimethylsiloxane with a dynamic viscosity of 1000 mPa.s at 25°C and a vinyl content of 0.32 wt%, 0.2 g of single-end vinyl polydimethylsiloxane with a dynamic viscosity of 1000 mPa.s at 25°C and a vinyl content of 0.23 wt%, and 4.75 g of vinyl silicone resin.

[0164] Component B includes 0.05 g of dual-end vinyl polydimethylsiloxane with a dynamic viscosity of 1000 mPa.s at 25°C and a vinyl content of 0.32 wt%, 0.2 g of single-end vinyl polydimethylsiloxane with a dynamic viscosity of 1000 mPa.s at 25°C and a vinyl content of 0.23 wt%, 4.75 g of vinyl silicone resin, 1.03 g of a cross-linking agent, and 2.0 g of a chain extender.

[0165] When used, take equal parts of component A and component B and mix them evenly at room temperature, then degas for 20 minutes under a vacuum degree of 0.1 MPa to obtain a high thermal conductivity organic silicone electronic potting glue. The thermal conductivity of the potting glue cured product is 3.2 Wm-1 .K -1 The flame retardant grade is UL 94V-0, the linear thermal expansion coefficient is 107μm / (m.℃), the Shore A hardness is 53, the tensile strength is 1.6MPa, and the elongation at break is 48%.

[0166] Embodiment 6:

[0167] This embodiment provides a high thermal conductivity organic silicon electronic potting adhesive for a power module and a preparation method and application thereof. The implementation method is the same as that of embodiment 2, except that:

[0168] In component A, a dual-terminal vinyl polydimethylsiloxane with a dynamic viscosity of 300 mPa.s at 25°C and a vinyl content of 0.57 wt% (purchased from Zhejiang Runhe Silicone New Materials Co., Ltd., model RH-Vi1323) was selected to replace the dual-terminal vinyl polydimethylsiloxane with a dynamic viscosity of 1000 mPa.s at 25°C and a vinyl content of 0.32 wt%, and the dosage remained unchanged. Others remained unchanged.

[0169] In component B, a dual-terminal vinyl polydimethylsiloxane with a dynamic viscosity of 300 mPa.s at 25°C and a vinyl content of 0.57 wt% (purchased from Zhejiang Runhe Organic Silicone New Materials Co., Ltd., model RH-Vi1323) was selected to replace the dual-terminal vinyl polydimethylsiloxane with a dynamic viscosity of 1000 mPa.s at 25°C and a vinyl content of 0.32 wt%, and the dosage remained unchanged. Others remained unchanged.

[0170] When used, take equal parts of component A and component B and mix them evenly at room temperature, then degas for 20 minutes under a vacuum degree of 0.1 MPa to obtain a high thermal conductivity organic silicone electronic potting glue. The thermal conductivity of the potting glue cured product is 3.2 Wm -1 .K -1 The flame retardant grade is UL 94V-0, the linear thermal expansion coefficient is 108μm / (m.℃), the Shore A hardness is 71, the tensile strength is 1.4MPa, and the elongation at break is 35%.

[0171] Comparative Example 1:

[0172] This embodiment provides a high thermal conductivity organic silicon electronic potting adhesive for a power module and a preparation method and application thereof. The implementation method is the same as that of embodiment 1, except that:

[0173] Component A contains 1.3 g of dual-terminal vinyl polydimethylsiloxane with a dynamic viscosity of 50 mPa.s at 25°C and a vinyl content of 1.85 wt%, and no single-terminal vinyl polydimethylsiloxane RH-Vi305B. Other components remain unchanged.

[0174] Component B contains 1.3 g of dual-terminal vinyl polydimethylsiloxane with a dynamic viscosity of 50 mPa.s at 25°C and a vinyl content of 1.85 wt%, and no single-terminal vinyl polydimethylsiloxane RH-Vi305B. Other components remain unchanged.

[0175] When used, take equal parts of component A and component B and mix them evenly at room temperature, then degas for 20 minutes under a vacuum degree of 0.1 MPa to obtain a high thermal conductivity silicone electronic potting glue for power modules. The thermal conductivity of the potting glue cured product is 3.0 Wm -1 .K -1 The flame retardant grade is UL 94V-0, the linear thermal expansion coefficient is 106μm / (m.℃), the Shore A hardness is 73, the tensile strength is 1.4MPa, and the elongation at break is 25%.

[0176] Comparative Example 2:

[0177] This embodiment provides a high thermal conductivity organic silicon electronic potting adhesive for a power module and a preparation method and application thereof. The implementation method is the same as that of embodiment 1, except that:

[0178] Component A contains 1.5 g of dual-terminal vinyl polydimethylsiloxane with a dynamic viscosity of 50 mPa.s at 25°C and a vinyl content of 1.85 wt%, and contains no dual-terminal vinyl polydimethylsiloxane RH-Vi1305 and single-terminal vinyl polydimethylsiloxane RH-Vi305B. Other components remain unchanged.

[0179] Component B contains 1.5 g of dual-terminal vinyl polydimethylsiloxane with a dynamic viscosity of 50 mPa.s at 25°C and a vinyl content of 1.85 wt%, and no dual-terminal vinyl polydimethylsiloxane RH-Vi1305 and single-terminal vinyl polydimethylsiloxane RH-Vi305B. Other components remain unchanged.

[0180] When used, take equal parts of component A and component B and mix them evenly at room temperature, then degas for 20 minutes under a vacuum degree of 0.1 MPa to obtain a high thermal conductivity silicone electronic potting glue for power modules. The thermal conductivity of the potting glue cured product is 3.0 Wm -1 .K -1 The flame retardant grade is UL 94V-0, the linear thermal expansion coefficient is 106μm / (m.℃), the Shore A hardness is 75, the tensile strength is 1.2MPa, and the elongation at break is 20%.

[0181] Comparative Example 3:

[0182] This embodiment provides a high thermal conductivity organic silicon electronic potting adhesive for a power module and a preparation method and application thereof. The implementation method is the same as that of embodiment 4, except that:

[0183] The plasticizer methyl silicone oil in component A is 7.5g, and there is no vinyl filler treatment agent.

[0184] There was no change in component B.

[0185] When used, take equal parts of component A and component B and mix them evenly at room temperature, then degas for 20 minutes under a vacuum degree of 0.1 MPa to obtain a high thermal conductivity silicone electronic potting glue for power modules. The thermal conductivity of the potting glue cured product is 3.0 Wm -1 .K -1 The flame retardant grade is UL 94V-0, the linear thermal expansion coefficient is 104μm / (m.℃), the Shore A hardness is 75, the tensile strength is 2.0MPa, and the elongation at break is 27%.

[0186] Comparative Example 4:

[0187] This embodiment provides a high thermal conductivity organic silicon electronic potting adhesive for a power module and a preparation method and application thereof. The implementation method is the same as that of embodiment 4, except that:

[0188] There is no change in component A.

[0189] In component B, the amount of hydrogen-containing silicone oil RH-LHC-3 containing hydrogen in both the terminal group and the side chain is 3.5 g, and the amount of hydrogen-containing silicone oil RH-DH37 containing hydrogen in both the terminal groups without a chain extender is 3.5 g.

[0190] When used, take equal parts of component A and component B and mix them evenly at room temperature, then degas for 20 minutes under a vacuum degree of 0.1 MPa to obtain a high thermal conductivity silicone electronic potting glue for power modules. The thermal conductivity of the potting glue cured product is 3.2 Wm -1 .K -1 The flame retardant grade is UL 94V-0, the linear thermal expansion coefficient is 104μm / (m.℃), the Shore A hardness is 72, the tensile strength is 2.4MPa, and the elongation at break is 29%.

[0191] Comparative Example 5:

[0192] This embodiment provides a high thermal conductivity organic silicon electronic potting adhesive for a power module and a preparation method and application thereof. The implementation method is the same as that of embodiment 4, except that:

[0193] There is no change in component A.

[0194] In component B, unilateral hydrogen-containing silicone oil is selected as the crosslinking agent, with the same quality, dynamic viscosity of 60 mPa.s at 25° C., and hydrogen content of 0.55%. It is purchased from Zhejiang Runhe Silicone New Materials Co., Ltd. and the model is RH-H503.

[0195] When used, take equal parts of component A and component B and mix them evenly at room temperature, then degas for 20 minutes under a vacuum degree of 0.1 MPa to obtain a high thermal conductivity silicone electronic potting glue for power modules. The thermal conductivity of the potting glue cured product is 3.2 Wm -1 .K -1 The flame retardant grade is UL 94V-0, the linear thermal expansion coefficient is 104μm / (m.℃), the Shore A hardness is 68, the tensile strength is 2.2MPa, and the elongation at break is 30%.

[0196] Comparative Example 6:

[0197] This embodiment provides a high thermal conductivity organic silicon electronic potting adhesive for a power module and a preparation method and application thereof. The implementation method is the same as that of embodiment 4, except that:

[0198] In component A, 1.2 g of double-terminated vinyl polydimethylsiloxane (purchased from Zhejiang Runhe Organic Silicone New Materials Co., Ltd., model RH-Vi1305) with a dynamic viscosity of 1000 mPa.s at 25° C. and a vinyl content of 0.32 wt% was contained, and no vinyl silicone resin was present. Other contents remained unchanged.

[0199] In component B, 1.2 g of double-terminated vinyl polydimethylsiloxane (purchased from Zhejiang Runhe Organic Silicone New Materials Co., Ltd., model RH-Vi1305) with a dynamic viscosity of 1000 mPa.s at 25° C. and a vinyl content of 0.32 wt% was contained, and no vinyl silicone resin was present. Other contents remained unchanged.

[0200] When used, take equal parts of component A and component B and mix them evenly at room temperature, then degas for 20 minutes under a vacuum degree of 0.1 MPa to obtain a high thermal conductivity silicone electronic potting glue for power modules. The thermal conductivity of the potting glue cured product is 3.2 Wm -1 .K -1 The flame retardant grade is UL 94V-0, the linear thermal expansion coefficient is 104μm / (m.℃), the Shore A hardness is 68, the tensile strength is 1.5MPa, and the elongation at break is 25%.

[0201] The performance test results of the above embodiments and comparative examples are shown in Table 1 and Table 2, respectively.

[0202] Table 1

[0203]

[0204] Table 2

[0205]

[0206]

[0207] As can be seen from Table 1, a high thermal conductivity organic silicon electronic potting glue for power module of the present invention and a preparation method thereof are designed to use low viscosity double-end vinyl polydimethylsiloxane, high viscosity double-end vinyl polydimethylsiloxane and single-end vinyl polydimethylsiloxane as base polymers, hydrogen-containing silicone oil containing hydrogen at both the end group and the side chain as a cross-linking agent, hydrogen-containing silicone oil containing hydrogen at both the end group and the side chain as a chain extender, silicone resin as a reinforcing agent, and long-chain vinyl modified siloxane as a filler treatment agent. The organic silicon thermal conductive potting glue prepared by cross-linking with the base polymer exhibits excellent thermal conductivity, tensile strength and elongation at break, can play a good shock absorbing effect during use, and is also convenient for disassembly and repair.

[0208] Table 1 is compared with Table 2 as follows:

[0209] In Example 1 and Comparative Example 1, the tensile strength of Comparative Example 1 is significantly reduced. This is because there is no single-end vinyl polydimethylsiloxane RH-Vi305B in the formulation system of Comparative Example 1. It can be seen that the single-end vinyl polydimethylsiloxane in Example 1 plays a role in increasing the random degree of crosslinking of the system and making the crosslinking more uniform, further improving the comprehensive mechanical properties of the system.

[0210] In Example 1 and Comparative Example 2, the tensile strength and elongation at break of Comparative Example 2 are further reduced compared with Comparative Example 1, and the mechanical properties are reduced significantly. This is because there is neither single-end vinyl polydimethylsiloxane RH-Vi305B nor high-viscosity double-end vinyl polydimethylsiloxane RH-Vi1305 in the formula system of Comparative Example 2, and only low-viscosity double-end vinyl polydimethylsiloxane is contained, so the degree of reduction in its mechanical properties is high. This is because the high-viscosity double-end vinyl polydimethylsiloxane has a longer molecular chain, and the cross-linking density of the three-dimensional network structure is reduced, so that the prepared organic silicone potting material has a higher elongation, thereby achieving high resistance to displacement deformation. At the same time, the use of single-end vinyl polydimethylsiloxane increases the random degree of cross-linking of the system, makes the cross-linking more uniform, and further improves the comprehensive mechanical properties of the system. It can be seen that the use of double-end vinyl polydimethylsiloxanes of different viscosities in combination, and the use of single-end vinyl polydimethylsiloxane in combination has a better effect.

[0211] In Example 4 and Comparative Example 3, it can be seen that the tensile strength and elongation at break of Comparative Example 3 have decreased to a certain extent. This is because the long-chain vinyl-modified siloxane treatment agent is replaced by a methyl silicone oil plasticizer. It can be seen that the long-chain vinyl-modified siloxane can indeed increase the interfacial bonding force between the filler and the matrix cross-linked network and improve the fluidity and mechanical properties of the silicone potting compound.

[0212] In Example 4 and Comparative Example 4, the elongation at break of Comparative Example 4 is lower. This is because the hydrogen-containing silicone oil with double-end hydrogen as a chain extender is not added. It can be seen that the hydrogen-containing silicone oil with double-end hydrogen can indeed reduce the crosslinking density of the three-dimensional network structure to a certain extent and improve the elongation of the silicone potting material.

[0213] In Example 4 and Comparative Example 5, the elongation at break of Comparative Example 5 decreased to a certain extent. This is because the unilateral hydrogen-containing silicone oil was selected as the cross-linking agent, the cross-linking degree became lower, and its performance became worse. This shows that the cross-linking agent containing hydrogen in both the end group and the side chain used in the present invention can form a special three-dimensional cross-linked network structure, so that the potting glue product has better mechanical strength and flexibility.

[0214] In Example 4 and Comparative Example 6, the elongation at break of Comparative Example 6 decreased, and the tensile strength decreased significantly. This is because no vinyl silicone resin was used in Comparative Example 6, and the vinyl silicone resin mainly participated in the hydrosilylation reaction in the system to strengthen the cross-linked network of the system. This proves that the vinyl silicone resin can increase the cross-linking density of the system and strengthen the mechanical properties of the system.

[0215] The present invention can also achieve regulation of product viscosity and performance by selecting the viscosity, vinyl position and content of vinyl polydimethylsiloxane, and can adapt to the needs of different usage scenarios; the specific selection of the filler treatment agent ensures the mechanical strength and potting effect of the potting glue, as well as the thermal conductivity.

[0216] The high thermal conductivity organic silicon electronic potting glue for the power module of the present invention has excellent thermal conductivity, and the thermal conductivity coefficient is 3.0Wm -1 .K -1 The above can meet the high-efficiency heat dissipation requirements of high-power devices such as power modules. The potting adhesive of the present invention has excellent thermal fatigue resistance, and the linear thermal expansion coefficient is below 110 μm / (m.℃), which can meet the long-term and high-efficiency resistance to heat accumulation stress damage requirements of high-power devices such as power modules.

[0217] The present invention uses both single-terminal vinyl polydimethylsiloxane and double-terminal vinyl polydimethylsiloxane with different viscosities, which can improve the randomness of the system cross-linking, make the cross-linking more uniform, and further improve the comprehensive mechanical properties of the system. The potting glue has good toughness, can maintain good tensile strength and elongation at break, has good shock absorption effect, and can protect the device being potted.

[0218] The potting adhesive of the present invention has good elasticity, is easy to disassemble and repair, and has little secondary damage to the device.

[0219] The potting glue of the present invention has moderate viscosity, good processing performance, and is convenient for potting operations in various complex scenarios. The potting glue of the present invention has good flame retardant performance, and 2.0 mm can achieve UL 94V0 level flame retardant effect, and can be prepared by a simple process, which is beneficial to industrial expansion of production.

[0220] The high thermal conductivity organic silicon electronic potting glue for power module of the present embodiment and its preparation method have a high thermal conductivity (≥3.0Wm -1 .K -1 ), low linear thermal expansion coefficient (≤110μm / (m.℃), high flame retardancy (UL 94V0 level, 2.0mm thickness), high tensile strength, high elongation at break, good shock absorption effect, easy disassembly and repair, good processing performance; at the same time, the preparation of this potting glue does not require high temperature and high pressure treatment, low cost, simple and easy to control preparation process, low environmental pollution, and easy to expand industrial production.

[0221] The above embodiments are only exemplary embodiments of the present application and are not intended to limit the present application. The protection scope of the present application is defined by the claims. Those skilled in the art may make various modifications or equivalent substitutions to the present application within the substantial protection scope of the present application, and such modifications or equivalent substitutions shall also be deemed to fall within the protection scope of the present application.

Claims

1. A high thermal conductivity silicone electronic potting glue for power modules, It is characterized in that It includes component A and component B; In parts by weight, the component A includes: 0.5-10 parts of base polymer, 0.15-10 parts of silicone resin, 0.5-5 parts of plasticizer, 0.01-0.2 parts of color paste, 70-120 parts of thermal conductive filler, 2-8 parts of filler treatment agent, and 0.1-2 parts of catalyst; In parts by weight, the B component includes: 0.5-10 parts of base polymer, 0.15-10 parts of silicone resin, 0.5-5 parts of plasticizer, 70-120 parts of thermal conductive filler, 0.1-10 parts of crosslinking agent, 0.1-10 parts of chain extender, and 0.01-1 parts of crosslinking inhibitor; Wherein, the crosslinking agent is a hydrogen-containing silicone oil containing hydrogen in both the end group and the side chain, and the structural formula is shown in Formula I: The chain extender is a hydrogen-containing silicone oil with hydrogen at both ends, and the structural formula is shown in Formula II: When the hydrogen-containing silicone oil containing hydrogen in both the end group and the side chain is mixed with the base polymer, an addition cross-linking reaction is carried out to form a three-dimensional network structure; The double-terminal hydrogen-containing silicone oil lengthens the molecular chain of the base polymer and reduces the cross-linking density of the three-dimensional network structure; The hydrogen-containing silicone oil containing hydrogen in both the end group and the side chain has a dynamic viscosity of 10-500 mPa.s at 25°C and a hydrogen content of 0.01-1 wt%; The dual-end hydrogen-containing silicone oil has a dynamic viscosity of 10-500 mPa.s at 25° C. and a hydrogen content of 0.01-1 wt %.

2. A high thermal conductivity organic silicon electronic potting glue for power module and a preparation method thereof according to claim 1, It is characterized in that The base polymer is composed of a mixture of low-viscosity dual-terminal vinyl polydimethylsiloxane, high-viscosity dual-terminal vinyl polydimethylsiloxane and single-terminal vinyl polydimethylsiloxane; The double-terminated vinyl polydimethylsiloxane structural formula is shown in Formula III: The structural formula of the single-end vinyl polydimethylsiloxane is shown in Formula IV:

3. A high thermal conductivity organic silicon electronic potting glue for power module and a preparation method thereof according to claim 2, It is characterized in that The low viscosity double-terminated vinyl polydimethylsiloxane has a dynamic viscosity of 50 mPa.s at 25°C; The high viscosity dual-terminated vinyl polydimethylsiloxane has a dynamic viscosity of 300-1000 mPa.s at 25°C.

4. A high thermal conductivity silicone electronic potting adhesive for power module and a preparation method thereof according to claim 1, It is characterized in that The silicone resin is vinyl silicone resin; The vinyl silicone resin has an M / Q ratio of 0.5-1, a resin content of 20%-70%, a dynamic viscosity of 5000-10000 mPa.s at 25° C., and a vinyl content of 0.4-2wt%.

5. The high thermal conductivity organic silicon electronic potting glue for power module and its preparation method according to claim 1, It is characterized in that The plasticizer is methyl silicone oil, and the dynamic viscosity at 25°C is 10-10000mPa.s; The color paste is selected from any one or more of blue paste, black paste, red paste and pink paste; The thermally conductive filler is selected from any one or more of alumina, magnesium oxide, silicon powder, kaolin, fused quartz powder, boron nitride, silicon carbide, aluminum nitride, and zirconium boride; Wherein, the thermally conductive filler is any one or more of particles, fibers, whiskers, and chips.

6. A high thermal conductivity organic silicon electronic potting adhesive for power module and a preparation method thereof according to claim 1, It is characterized in that The filler treatment agent is vinyl-modified siloxane, with a dynamic viscosity of 10-60 mPa.s at 25° C. and a vinyl content of 0.5-1.5 wt %.

7. A high thermal conductivity organic silicon electronic potting adhesive for power module and a preparation method thereof according to claim 1, It is characterized in that The catalyst is a platinum catalyst or dibutyltin dilaurate. Wherein, the platinum catalyst is a platinum-based catalyst; Wherein, the platinum-based catalyst is selected from one or any several of chloroplatinic acid, platinum tetrachloride, an alcohol solution of chloroplatinic acid, a platinum-olefin complex, a platinum-alkenylsiloxane complex and a platinum-carbonyl complex; The cross-linking inhibitor is one or any combination of alkynol compounds, alkenyl ring bodies and alkenyl double heads.

8. A method for preparing the high thermal conductivity organic silicon electronic potting adhesive for power module according to any one of claims 1 to 7, It is characterized in that The steps include: Add silicone resin, plasticizer, color paste and thermal conductive filler to the base polymer in sequence, stir and blend at 20-35° C. for 60-120 minutes, and then heat and dehydrate at 100-150° C. and stir and blend for 120-180 minutes to obtain base slurry A; The base slurry A is cooled to room temperature, and a filler treatment agent and a catalyst are added in sequence, and the mixture is stirred and blended at 20-25° C. for 5-10 minutes to obtain the component A; Add silicone resin, plasticizer and thermal conductive filler to the base polymer in sequence, stir and blend at 20-35° C. for 60-120 minutes, and then heat and dehydrate at 100-150° C. and stir and blend for 120-180 minutes to obtain matrix slurry B; The base slurry B is cooled to room temperature, and a crosslinking agent, a chain extender, and a crosslinking inhibitor are added in sequence, and the mixture is stirred and blended at 20-25° C. for 5-10 minutes to obtain the B component.

9. A method for preparing a high thermal conductivity organic silicon electronic potting adhesive for a power module according to claim 8, It is characterized in that When preparing the matrix slurry A, the stirring speed is 400-450 r / min at 20-35° C., and the stirring speed is 600-900 r / min at 100-150° C.; When preparing the A component, the stirring speed is 400-450r / min at 20-25°C; When preparing the matrix slurry B, the stirring speed is 400-450 r / min at 20-35° C., and the stirring speed is 600-900 r / min at 100-150° C.; When preparing the B component, the stirring speed is 400-450 r / min at 20-25°C.

10. An application of the high thermal conductivity organic silicon electronic potting adhesive for a power module as claimed in any one of claims 1 to 7, It is characterized in that When used, the A component and the B component can be mixed in a volume ratio or mass ratio of 1: (0.8-1.2).