Cast cementing coating oil well sand prevention curing material

By using modified carbon fiber and modified polyacrylamide in the sand-proof materials of oil wells, a multi-layer barrier network is formed, which solves the problem of insufficient curing strength of traditional coated sand materials, and achieves improved sand-proofing effect and oil wells in the later stage of high water content development. Stable production.

CN118995166AInactive Publication Date: 2024-11-22SHANDONG HIGH-TECH PETROLEUM TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411079268.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-07
Publication Date
2024-11-22
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Traditional coated sand materials have limitations in curing strength, which is difficult to meet the sand prevention requirements for the strong extraction of liquid after the development of high water content. The complexity of the selection of curing agents increases the difficulty and cost of technical implementation.

Method used

The sand-proof curing materials of the oil wells are used to coat the oil well, including quartz sand and modified carbon fiber as proppants, and the phenoamine curing agent and bisphenol A type unsaturated polyester resin as the glue component, combined with modified polyacrylamide as the permeability Adjuster, forming a multi-layered barrier net to improve curing strength and stability.

Benefits of technology

It significantly improves the curing strength and permeability, ensures the improvement of the sand prevention effect of oil wells, meets the sand prevention needs in the later stage of high water content development of Zhonglao Oilfield, and ensures the stable production and safety of oil wells.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004983245560000091
    Figure BDA0004983245560000091
Patent Text Reader

Abstract

The present invention provides an existing cementing coating oil well sand prevention curing material, which comprises, by weight, 30-36 parts of a proppant and 6-8 parts of a glue solution, wherein the propping agent is prepared from quartz sand and modified carbon fibers in a weight ratio of (5-6): (1-2); the glue solution consists of 40-45 parts of a cementing agent, 6-8 parts of a curing agent, 0.1-2 parts of a coupling agent, 1-2 parts of a permeability regulator, 2-3 parts of a dispersing agent and 50-55 parts of a solvent. According to the present invention, the raw materials are optimized, such that the curing strength is significantly improved, and the oil well sand prevention effect is significantly improved. According to the material, the defect of the traditional precoated sand material in curing strength is overcome, and a new solution is provided for liquid extraction and strong production in the later stage of high-water-content development of middle and old oil fields.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of sand control, and in particular to an existing cementing and coating oil well sand control solidification material. Background Art

[0002] In the process of oil field development, the problem of sand production in oil wells has always been an important factor affecting the production stability and economic benefits of oil fields. Sand production in oil wells will not only lead to a series of problems such as sand burial in oil layers, sand plugging in wellbore, and equipment abrasion, but in severe cases it will even lead to the shutdown or scrapping of oil wells. Therefore, the research and development of oil well sand control technology is of great significance to the petroleum industry. At present, gravel filling composite sand control technology has been widely used in oil fields as an effective sand control method. However, traditional coated sand materials have certain limitations in curing strength, and it is difficult to meet the sand control requirements of liquid extraction and strong recovery in the later stage of high water content development.

[0003] The development of traditional coated sand mainly relies on the softening and bonding of thermoplastic resins at formation temperature, or the use of resin curing agents with specific excitation conditions for curing. However, the curing strength of this method is limited by the activation effect of the curing agent under formation conditions, resulting in the final curing strength being generally average and unable to meet the needs of large-volume intensive production. In addition, the selection of curing agents must take into account the complexity of formation conditions, which increases the difficulty and cost of technical implementation. Based on this, the present invention provides an existing cemented coated oil well sand control curing material. Summary of the invention

[0004] The purpose of the present invention is to provide a ready-bonded coated oil well sand control solidification material, which significantly improves the curing strength while maintaining the permeability, and maintains the curing strength after high-temperature thermal aging, thereby significantly improving the oil well sand control effect.

[0005] The present invention provides a ready-bonded and coated oil well sand control solidification material, which comprises 30-36 parts of proppant and 6-8 parts of glue in parts by weight; wherein:

[0006] The proppant is composed of quartz sand and modified carbon fiber in a weight ratio of (5-6):(1-2);

[0007] The adhesive solution consists of 40-45 parts of a binder, 6-8 parts of a curing agent, 0.1-2 parts of a coupling agent, 1-2 parts of a permeability regulator, 2-3 parts of a dispersant and 50-55 parts of a solvent.

[0008] Furthermore, the quartz sand includes quartz sand with a weight ratio of (3-4): 1 with a particle size of 0.4-0.8 mm and 1 with a particle size of 4-4.5 mm.

[0009] Furthermore, the length of the carbon fiber is 1.5-2 cm, and the preparation method of the modified carbon fiber includes: immersing the carbon fiber in a 1 mol / L concentrated nitric acid solution, acidifying in a constant temperature water bath at 70-80°C for 2-3 hours, washing with deionized water and ethanol until the washing liquid is neutral, and then drying; adding to an ethanol solution of a silane coupling agent, ultrasonically treating for 30-40 minutes, grinding at 65-75°C for 2.5-3.5 hours, washing with deionized water and anhydrous ethanol at least 3 times respectively, and drying at 60-70°C.

[0010] Furthermore, the usage ratio of the acid-treated carbon fiber, the silane coupling agent and the ethanol is (10-20) g: (26-28) mL: (35-45) mL.

[0011] Furthermore, the curing agent is a phenolic amine curing agent, the amine value is 330-375 mg KOH / g, the flash point is 103-113° C., and the density is 0.95-1 Kg / L.

[0012] Furthermore, the binder is bisphenol A type unsaturated polyester resin 3301; and the coupling agent is KH560.

[0013] Furthermore, the permeability regulator is modified polyacrylamide, and the preparation method of the modified polyacrylamide includes: pre-treating zeolite with acid solution and alkaline solution, adding acrylamide, methylenebisacrylamide and the pre-treated zeolite into methanol, ultrasonically treating for 30-40 minutes, drying at a constant temperature of 55-65°C for 6-8 hours, and grinding to obtain the permeability regulator.

[0014] The application of modified polyacrylamide as a permeability regulator in oil well sand control can effectively prevent the migration and invasion of sand particles and reduce the sand production problem in oil wells through its dual functions of improving curing strength and maintaining permeability. At the same time, its ability to maintain strength after high-temperature thermal aging ensures the stability and safety of oil wells during long-term operation, thereby significantly improving the sand control effect of oil wells.

[0015] Furthermore, the usage ratio of acrylamide, methylenebisacrylamide, zeolite and methanol is (4-5) g: (10-12) g: (2.2-2.6) g: (50-60) mL.

[0016] Furthermore, the pretreatment step includes: cleaning the dust on the surface of the zeolite with deionized water, then soaking it in a 10-12% sodium hydroxide solution and a 10-12% hydrochloric acid solution for 1-2 hours respectively to remove the insoluble substances and oil stains on the surface, and finally cleaning the residual sodium hydroxide and hydrochloric acid on the surface with deionized water, and drying it at 55-65°C.

[0017] Furthermore, the dispersant is nano calcium stearate, and the solvent comprises a mixed solution of methanol and ethanol in a volume ratio of 3:1.

[0018] The beneficial effects of the present invention are:

[0019] (1) Quartz sand and modified carbon fiber are used as composite proppants in the raw materials of the present invention, and their physical structure can effectively block the migration of formation sand. Among them, the particle size distribution of quartz sand (0.4-0.8mm and 4-4.5mm) and the length of carbon fiber (1.5-2cm) together constitute a multi-layered barrier network, which can effectively prevent fine to medium-sized formation sand from entering the wellbore. In addition, by acidifying the carbon fiber with concentrated nitric acid and treating it with a silane coupling agent, its surface is modified, which enhances its bonding strength with the glue and further improves the overall strength and stability of the sand-proof material.

[0020] (2) The present invention uses modified polyacrylamide as a permeability regulator. By controlling its preparation process, the permeability of the material can be adjusted to ensure that the normal flow of oil and gas is not affected while effectively blocking the formation sand. In addition, the addition of carbon fiber and the multi-particle size distribution of quartz sand form a certain pore structure after consolidation, which is conducive to the seepage of oil and gas and reduces the seepage resistance.

[0021] (3) Polyacrylamide (PAM) itself is a high molecular polymer with good adhesion, film-forming properties and certain mechanical strength. The present invention uses zeolite-modified modified polyacrylamide as a permeability regulator, and adds zeolite as a filler into the PAM synthesis system. The microporous structure and high specific surface area of ​​zeolite not only provide more reaction sites, but also form a more stable network structure with the PAM molecular chain through physical and chemical effects. This network structure can more effectively resist external force damage during the curing process, thereby improving the curing strength. In addition, due to the unique molecular structure of polyacrylamide and its synergistic effect with zeolite, a layer of film or mesh structure that has a certain strength and allows fluid to pass through is formed without significantly blocking the pores. This can maintain the permeability and improve the curing strength.

[0022] (4) The adhesive of the present invention uses bisphenol A type unsaturated polyester resin as a binder and is matched with phenolic amine curing agent, which ensures the high strength and durability of the material after curing. At the same time, the addition of coupling agent, permeability regulator and dispersant further improves the compatibility and dispersibility between the adhesive and the proppant, and improves the overall performance of the adhesive layer.

[0023] (5) The present invention innovatively uses sand control raw materials, which significantly improves the strength after consolidation. The raw materials in the present invention can enable the coated sand to quickly cement under the physical and chemical conditions of the formation after filling, forming a solid sand retaining ring, which effectively prevents sand from coming out of the formation. The optimized existing cemented coated oil well sand control solidification material has a significantly improved consolidation strength. This improvement meets the sand control requirements for liquid extraction and strong production in the late stage of high water content development in the Zhonglao Oilfield, ensuring the stable production of the oil wells. DETAILED DESCRIPTION

[0024] The technical scheme of the present invention is described clearly and completely below. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in the field without creative work are within the scope of protection of the present invention. It should be noted that the raw materials can be obtained commercially.

[0025] Example 1

[0026] This embodiment provides a ready-bonded coated oil well sand control solidification material, which includes 33 parts of proppant and 7 parts of glue in terms of weight; wherein:

[0027] The proppant is composed of quartz sand and modified carbon fiber in a weight ratio of 5.5:1.5;

[0028] The glue solution is composed of 42 parts of a binder, 7 parts of a curing agent, 1 part of a coupling agent, 1.5 parts of a permeability regulator, 2.5 parts of a dispersant and 52 parts of a solvent;

[0029] Wherein, the quartz sand includes quartz sand with a particle size of 0.7 mm and a particle size of 4.2 mm in a weight ratio of 3.5:1;

[0030] The length of the carbon fiber is 1.7 cm. The preparation method of the modified carbon fiber includes: immersing the carbon fiber in a 1 mol / L concentrated nitric acid solution, acidifying in a constant temperature water bath at 75°C for 2.5 hours, washing with deionized water and ethanol until the washing solution is neutral, and then drying; adding the ethanol solution of silane coupling agent KH550, ultrasonically treating for 35 minutes, grinding at 70°C for 3 hours, washing with deionized water and anhydrous ethanol at least 3 times, and drying at 65°C; the amount ratio of the carbon fiber, silane coupling agent and ethanol after the acidification treatment is 15g:27mL:40mL;

[0031] The curing agent is phenolic amine curing agent Cardolite NX-2003, the amine value is 350 mg KOH / g, the flash point is 108° C., and the density is 0.97 Kg / L.

[0032] The binder is bisphenol A type unsaturated polyester resin 3301; the coupling agent is KH560; the dispersant is nano calcium stearate, and the solvent includes a mixed solution of methanol and ethanol in a volume ratio of 3:1;

[0033] The permeability regulator is modified polyacrylamide. The preparation method of the modified polyacrylamide includes: pre-treating zeolite with an acid solution and an alkaline solution, adding acrylamide, methylenebisacrylamide and the pre-treated zeolite into methanol, ultrasonically treating for 35 minutes, drying at a constant temperature of 60°C for 7 hours, and grinding to obtain the permeability regulator; the amount ratio of acrylamide, methylenebisacrylamide, zeolite and methanol is 4.5g:11g:2.4g:55mL; the pre-treatment step includes: cleaning the dust on the surface of the zeolite with deionized water, and then soaking it in a sodium hydroxide solution with a mass fraction of 11% and a hydrochloric acid with a mass fraction of 11% for 1.5 hours respectively to remove the insoluble substances and oil stains on the surface, and finally cleaning the sodium hydroxide and hydrochloric acid remaining on the surface with deionized water, and drying at 60°C.

[0034] Example 2

[0035] This embodiment provides a ready-bonded coated oil well sand control solidification material, which includes 30 parts of proppant and 6 parts of glue in terms of weight; wherein:

[0036] The proppant is composed of quartz sand and modified carbon fiber in a weight ratio of 5:1;

[0037] The glue solution is composed of 40 parts of a binder, 6 parts of a curing agent, 0.1 parts of a coupling agent, 1 part of a permeability regulator, 2 parts of a dispersant and 50 parts of a solvent;

[0038] Wherein, the quartz sand includes quartz sand with a particle size of 0.4 mm and quartz sand with a particle size of 4 mm in a weight ratio of 3:1;

[0039] The length of the carbon fiber is 1.5 cm. The preparation method of the modified carbon fiber includes: immersing the carbon fiber in a 1 mol / L concentrated nitric acid solution, acidifying in a constant temperature water bath at 70°C for 2 hours, washing with deionized water and ethanol until the washing solution is neutral, and then drying; adding the carbon fiber to an ethanol solution of silane coupling agent KH550, ultrasonically treating for 30 minutes, grinding at 65°C for 2.5 hours, washing with deionized water and anhydrous ethanol at least 3 times, and drying at 60°C; the amount ratio of the carbon fiber, silane coupling agent and ethanol after the acidification treatment is 10g:26mL:35mL;

[0040] The curing agent is phenolic amine curing agent Cardolite NX-2003, the amine value is 330 mg KOH / g, the flash point is 103° C., and the density is 0.95 Kg / L.

[0041] The binder is bisphenol A type unsaturated polyester resin 3301; the coupling agent is KH560; the dispersant is nano calcium stearate, and the solvent includes a mixed solution of methanol and ethanol in a volume ratio of 3:1;

[0042] The permeability regulator is modified polyacrylamide. The preparation method of the modified polyacrylamide includes: pre-treating zeolite with an acid solution and an alkaline solution, adding acrylamide, methylenebisacrylamide and the pre-treated zeolite into methanol, ultrasonically treating for 30 minutes, drying at a constant temperature of 55°C for 6 hours, and grinding to obtain the permeability regulator; the amount ratio of acrylamide, methylenebisacrylamide, zeolite and methanol is 4g:10g:2.2g:50mL; the pre-treatment step includes: cleaning the dust on the surface of the zeolite with deionized water, then soaking it in a sodium hydroxide solution with a mass fraction of 10% and a hydrochloric acid with a mass fraction of 10% for 1 hour respectively to remove the insoluble substances and oil stains on the surface, and finally cleaning the sodium hydroxide and hydrochloric acid remaining on the surface with deionized water, and drying at 55°C.

[0043] Example 3

[0044] This embodiment provides a ready-bonded coated oil well sand control solidification material, which includes 36 parts of proppant and 8 parts of glue in terms of weight; wherein:

[0045] The proppant is composed of quartz sand and modified carbon fiber in a weight ratio of 3:1;

[0046] The glue solution is composed of 45 parts of a binder, 8 parts of a curing agent, 2 parts of a coupling agent, 2 parts of a permeability regulator, 3 parts of a dispersant and 55 parts of a solvent;

[0047] Wherein, the quartz sand includes quartz sand with a particle size of 0.8 mm and a particle size of 4.5 mm in a weight ratio of 4:1;

[0048] The length of the carbon fiber is 2 cm, and the preparation method of the modified carbon fiber comprises: immersing the carbon fiber in a 1 mol / L concentrated nitric acid solution, acidifying in a constant temperature water bath at 80°C for 3 hours, washing with deionized water and ethanol until the washing solution is neutral, and then drying; adding the carbon fiber to an ethanol solution of silane coupling agent KH550, ultrasonically treating for 40 minutes, grinding at 75°C for 3.5 hours, washing with deionized water and anhydrous ethanol at least 3 times, and drying at 70°C; the amount ratio of the carbon fiber, silane coupling agent and ethanol after the acidification treatment is 20g:28mL:45mL;

[0049] The curing agent is phenolic amine curing agent Cardolite NX-2003, the amine value is 375 mg KOH / g, the flash point is 113° C., and the density is 1 Kg / L.

[0050] The binder is bisphenol A type unsaturated polyester resin 3301; the coupling agent is KH560; the dispersant is nano calcium stearate, and the solvent includes a mixed solution of methanol and ethanol in a volume ratio of 3:1;

[0051] The permeability regulator is modified polyacrylamide. The preparation method of the modified polyacrylamide includes: pre-treating zeolite with an acid solution and an alkaline solution, adding acrylamide, methylenebisacrylamide and the pre-treated zeolite into methanol, ultrasonically treating for 40 minutes, drying at a constant temperature of 65°C for 8 hours, and grinding to obtain the permeability regulator; the amount ratio of acrylamide, methylenebisacrylamide, zeolite and methanol is 5g:12g:2.6g:60mL; the pre-treatment step includes: cleaning the dust on the surface of the zeolite with deionized water, and then soaking it in a sodium hydroxide solution with a mass fraction of 12% and a hydrochloric acid with a mass fraction of 12% for 2 hours respectively to remove the insoluble substances and oil stains on the surface, and finally cleaning the sodium hydroxide and hydrochloric acid remaining on the surface with deionized water, and drying at 65°C.

[0052] Comparative Example 1

[0053] This comparative example provides a cemented and coated oil well sand control solidification material. Different from Example 1, the proppant is composed of quartz sand only.

[0054] Comparative Example 2

[0055] This comparative example provides a cemented and coated oil well sand control solidification material, which is different from Example 1 in that the carbon fibers in the proppant are not modified.

[0056] Comparative Example 3

[0057] This comparative example provides a cemented coated oil well sand control solidification material, which is different from Example 1 in that the carbon fiber in the proppant is modified by using a silane coupling agent KH560.

[0058] Comparative Example 4

[0059] This comparative example provides a cemented coated oil well sand control solidification material, which is different from Example 1 in that the carbon fiber in the proppant is modified by using a silane coupling agent KH570.

[0060] Comparative Example 5

[0061] This comparative example provides a cemented coated oil well sand control solidification material. The difference from Example 1 is that during the preparation of the permeability regulator, the zeolite pretreatment step is consistent with the carbon fiber pretreatment step, that is, it is immersed in a 1 mol / L concentrated nitric acid solution, acidified in a constant temperature water bath at 75°C for 2.5 hours, and then washed with deionized water and ethanol until the washing liquid is neutral, and then dried.

[0062] Comparative Example 6

[0063] This comparative example provides a cemented coated oil well sand control solidification material. Different from Example 1, the permeability regulator is unmodified polyacrylamide, that is, no zeolite is added during the preparation process.

[0064] Test example: The raw materials of the cemented coating oil well sand control curing materials in the above-mentioned Examples 1-3 and Comparative Examples 1-6 were blended, cured at a temperature of 40° C. for 24 hours, and prepared into a cylinder with a diameter of 3 cm and a length of 3 cm. The two end faces of the cylinder were flattened, and then the compression resistance test and the permeability test were performed. The results are shown in Table 1 below:

[0065] Table 1

[0066]

[0067] Oil well environments are usually accompanied by extreme conditions such as high temperature and high pressure, which places high demands on the thermal stability and durability of materials. Among them, the zeolite component in the modified polyacrylamide may have a certain thermal stability, which can maintain its structural integrity at high temperatures, thereby supporting the PAM molecular chain and preventing it from degrading due to high temperatures. At the same time, the interaction between PAM and zeolite may enhance the thermal stability of the overall material, so that it can still maintain good curing strength after high-temperature thermal aging.

[0068] Finally, it should be noted that the above embodiments are only used to illustrate the present invention and are not intended to limit the technical solutions described in the present invention. Those skilled in the art should understand that the present invention can still be modified or replaced by equivalents. All technical solutions and improvements that do not depart from the spirit and scope of the present invention should be included in the scope of the claims of the present invention.

Claims

1. A cemented coating oil well sand control solidification material, characterized in that: According to weight, it includes 30-36 parts of proppant and 6-8 parts of glue; wherein, The proppant is composed of quartz sand and modified carbon fiber in a weight ratio of (5-6):(1-2); The adhesive solution consists of 40-45 parts of a binder, 6-8 parts of a curing agent, 0.1-2 parts of a coupling agent, 1-2 parts of a permeability regulator, 2-3 parts of a dispersant and 50-55 parts of a solvent.

2. The instant cementing coating oil well sand control solidification material according to claim 1, characterized in that: The quartz sand includes quartz sand with a weight ratio of (3-4): 1 with a particle size of 0.4-0.8 mm and 1 with a particle size of 4-4.5 mm.

3. The instant cementing coating oil well sand control solidification material according to claim 1, characterized in that: The length of the carbon fiber is 1.5-2 cm. The preparation method of the modified carbon fiber comprises: immersing the carbon fiber in a 1 mol / L concentrated nitric acid solution, acidifying the carbon fiber in a constant temperature water bath at 70-80°C for 2-3 hours, washing the carbon fiber with deionized water and ethanol until the washing liquid is neutral, and then drying the carbon fiber; adding the carbon fiber to an ethanol solution of a silane coupling agent, ultrasonically treating the carbon fiber for 30-40 minutes, grinding the carbon fiber at 65-75°C for 2.5-3.5 hours, washing the carbon fiber with deionized water and anhydrous ethanol for at least 3 times, respectively, and drying the carbon fiber at 60-70°C.

4. The instant cementing coating oil well sand control solidification material according to claim 3, characterized in that: The usage ratio of the acid-treated carbon fiber, the silane coupling agent and the ethanol is (10-20) g: (26-28) mL: (35-45) mL.

5. The instant cementing coating oil well sand control solidification material according to claim 1, characterized in that: The curing agent is a phenolic amine curing agent, the amine value is 330-375 mg KOH / g, the flash point is 103-113° C., and the density is 0.95-1 Kg / L.

6. The instant cementing coating oil well sand control solidification material according to claim 1, characterized in that: The binder is bisphenol A type unsaturated polyester resin 3301; the coupling agent is KH560.

7. The instant cementing and coating oil well sand control solidification material according to claim 1, characterized in that: The permeability regulator is modified polyacrylamide, and the preparation method of the modified polyacrylamide comprises: pre-treating zeolite with an acid solution and an alkaline solution, adding acrylamide, methylenebisacrylamide and the pre-treated zeolite into methanol, ultrasonically treating for 30-40 minutes, drying at a constant temperature of 55-65° C. for 6-8 hours, and grinding to obtain the permeability regulator.

8. The instant cementing coating oil well sand control solidification material according to claim 7, characterized in that: The usage ratio of acrylamide, methylenebisacrylamide, zeolite and methanol is (4-5) g: (10-12) g: (2.2-2.6) g: (50-60) mL.

9. The instant cementing coating oil well sand control solidification material according to claim 7, characterized in that: The pretreatment step includes: cleaning the dust on the surface of the zeolite with deionized water, then soaking it in a sodium hydroxide solution with a mass fraction of 10-12% and a hydrochloric acid with a mass fraction of 10-12% for 1-2 hours respectively to remove the insoluble substances and oil stains on the surface, and finally cleaning the sodium hydroxide and hydrochloric acid remaining on the surface with deionized water, and drying it at 55-65°C.

10. The instant cementing coating oil well sand control solidification material according to claim 1, characterized in that: The dispersant is nano calcium stearate, and the solvent comprises a mixed solution of methanol and ethanol in a volume ratio of 3:1.