Modified propping agent for fracturing and preparation method thereof

By coating the ceramic particle proppant with organic resin and nanosilica coating, and graft modification with hexamethyldisiloxane, the problem of insufficient proppant flow diversion ability in the prior art is solved, and the problem of achieving the Efficient oil and gas extraction and fracturing fluid discharge have improved the development effect of shale oil and gas reservoirs.

CN118995189APending Publication Date: 2024-11-22SICHUAN CHUANQING UNDERGROUND TECHNOLOGY CO LTD
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
CN202411032069.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The existing proppants for fracturing are insufficient under high closing stress, which limits the efficiency of post-pressure fracturing fluid and oil and gas extraction. Especially in shale oil and gas reservoirs, it is difficult to improve the remote end with lower diversion capacity. The flow diversion effect of the crack.

Method used

Ceramic particles are used as proppant matrix, the surface is coated with organic resin and nanosilicon dioxide coating, and modified by hexamethyldisiloxane graft to form a hydrophobic and gas-philic coating to improve the flow diversion of proppant Ability and suspension.

Benefits of technology

The flow-guiding ability and suspension of the modified proppant in the fracturing fluid have been significantly improved, which has improved the oil and gas output and the discharge rate of the fracturing fluid. The preparation method is simple, the coating is stable, and it is not easy to peel.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118995189A_ABST
    Figure CN118995189A_ABST
Patent Text Reader

Abstract

The invention relates to an oil and gas exploitation material, and particularly provides a modified proppant for fracturing, which comprises a proppant matrix made of ceramic particles, the surface of the proppant matrix is coated with a coating, and hexamethyldisiloxane is grafted on the coating. The invention further provides a preparation method of the modified propping agent for fracturing. The invention has the beneficial effects of good hydrophobicity, strong flow conductivity, improved suspension property, simple preparation, and difficult peeling of the coating.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of oil and gas mining materials, in particular to a modified proppant for fracturing and a preparation method thereof. Background Art

[0002] Hydraulic fracturing is currently one of the most common technical means to improve the production capacity, development effect and benefits of low-permeability oil and gas reservoirs and unconventional oil and gas reservoirs. This technology relies on a surface high-pressure pump group to inject fluid into the well at a speed that exceeds the absorption capacity of the formation, and uses the high pressure at the bottom of the well to break the reservoir rock and produce cracks. In order to prevent the pressure from dropping after the pump is stopped and the cracks from closing by themselves, proppants are often mixed into the liquid injected after the formation is broken. The proppant enters the cracks along with the fluid, so that when the cracks close, they form propped cracks and stay in the cracks permanently, so that the oil and gas seepage environment can be improved for a long time.

[0003] In the volume fracturing of shale oil and gas reservoirs, due to the limited width of hydraulic fractures and the poor permeability of proppants, small-size proppants (70-140 mesh) or even micro-size proppants (200-400 mesh) are often used. These proppants form a dense stack under high closure stress; and because the proppant itself has a small particle size, the gaps between the particles are also small, and the conductivity (i.e., permeability) of the formed proppant filling layer is much lower than that of conventional proppants (20-40 mesh and 40-70 mesh). The low conductivity has greatly restricted the timely return of the fracturing fluid after fracturing and the subsequent oil and gas production.

[0004] There are not many effective solutions to the above problems. In engineering practice, a small amount of 40 / 70 mesh proppant is mainly added at the end of construction to improve the conductivity of the proppant filling layer near the wellbore, but the conductivity of the distal fracture is not improved. Summary of the invention

[0005] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a modified proppant with good hydrophobicity, strong flow conductivity, improved suspension, simple preparation, and coating that is not easy to peel off, and a preparation method thereof.

[0006] The purpose of the present invention is achieved through the following technical solutions:

[0007] (First aspect)

[0008] A modified proppant for fracturing comprises a proppant matrix made of ceramic particles, a coating coated on the surface of the proppant matrix, and hexamethyldisiloxane grafted on the coating.

[0009] Furthermore, the coating comprises an organic resin and an inorganic filler; the inorganic filler is nano-silicon dioxide, the organic resin is an organic compound containing hydroxyl groups, and hexamethyldisiloxane is grafted with the organic resin and the nano-silicon dioxide via the hydroxyl groups.

[0010] Furthermore, the mass ratio of the organic resin to the inorganic filler is (20:1) to (5:1).

[0011] Furthermore, the saturated swelling rate of the organic resin is not higher than 10%.

[0012] Furthermore, the proppant matrix is ​​mesoporous alumina ceramic particles, and the porosity of the alumina ceramic particles is not less than 10% and not more than 30%.

[0013] (Second aspect)

[0014] A method for preparing a modified proppant for fracturing:

[0015] Prepare mesoporous ceramic particles as a proppant matrix, prepare an organic resin containing hydroxyl groups, prepare a nano-silica dispersion, and prepare a polar small molecule solution of hexamethyldioxysilane;

[0016] By filtering, the organic resin solution forms an organic liquid film on the surface of the proppant matrix;

[0017] Then, the nano-silicon dioxide dispersion forms a liquid film containing inorganic fillers on the surface of the organic filter membrane by filtering; the organic liquid film and the liquid film of the inorganic filler together form a coating;

[0018] Then, the proppant substrate with the coating layer is modified by using hexamethyldisiloxane to obtain a modified proppant.

[0019] Furthermore, the method of filtering the organic resin solution to form an organic liquid film on the surface of the proppant substrate refers to filtering the organic resin solution for 1 to 20 minutes under a pressure of 0.01 to 0.3 MPa to form an organic liquid film on the surface of the proppant substrate;

[0020] And / or, the method of filtering the inorganic filler dispersion to form a liquid film containing the inorganic filler on the surface of the organic liquid film refers to filtering for 0.5 to 10 minutes at a pressure of 0.01 to 0.5 MPa to form a liquid film containing the inorganic filler on the surface of the organic liquid film;

[0021] And / or, the concentration of the organic resin solution is 0.1 to 10% by mass;

[0022] And / or, the concentration of the inorganic filler in the inorganic filler dispersion is 0.1 to 10% by mass.

[0023] Furthermore, the use of hexamethyldisiloxane to modify the coated proppant substrate refers to: dispersing the coated proppant substrate in a solution of polar small molecules of hexamethyldisiloxane, stirring the modification reaction at 30-80° C. for 2-12 hours; wherein the concentration of the hexamethyldisiloxane solution is 0.5-3% by mass fraction.

[0024] The present invention has the following advantages:

[0025] (1) In the modified proppant for fracturing provided:

[0026] a. The coating applied on the surface of the proppant substrate modified by hexamethyldisiloxane makes the proppant surface hydrophobic, increases the contact angle with water, and thus reduces the capillary resistance of the water phase (injected fracturing fluid and native formation water) when flowing in the gap of the proppant filling layer, thereby improving the conductivity of the proppant filling layer, and ultimately increasing the discharge rate of the water phase (injected fracturing fluid and native formation water), thereby increasing the oil and gas production;

[0027] b. Using mesoporous alumina ceramic particles as the proppant matrix, the density of the entire proppant is reduced without affecting the compressive strength, and the suspension and migration capabilities of the proppant are improved; at the same time, the mesoporous structure can also increase the modified specific surface area and enhance the surface modification effect;

[0028] c. The inventors unexpectedly discovered that the hexamethyldisiloxane on the surface of the modified proppant has a certain affinity for air and can be adsorbed and combined with microbubbles in the fracturing fluid (liquid nitrogen is injected during the fracturing construction process, and the liquid nitrogen vaporizes to form microbubbles). The buoyancy of the bubbles improves the suspension state of the proppant in the fracturing fluid and also improves the ability of the proppant to be transported over long distances in the fracture.

[0029] (2) In the provided method for preparing a modified proppant for a fracturing fluid:

[0030] The preparation method has simple operation steps, and the organic resin is solidified on the surface of the proppant, so that the obtained coating has a strong bonding force with the proppant matrix and is not easy to peel off. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 This is a photograph of the modified proppant of Example 2 added to a slick water fracturing fluid at a concentration of 15%, stirred at 5500 r / min for 90 seconds using a high-speed stirrer, and then left to stand for observation. DETAILED DESCRIPTION

[0032] The present invention is further described below, but the protection scope of the present invention is not limited to the following description.

[0033] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0034] The present application provides a modified proppant for fracturing, comprising a proppant substrate, a coating coated on the proppant substrate, and hexamethyldisiloxane grafted on the coating;

[0035] And / or, the ceramic particles are common metal oxide ceramic particles, such as aluminum oxide particles, and the ceramic particles are micron-sized particles, such as having a particle size of 10 to 800 μm, preferably 20 to 500 μm, and more preferably 40 to 200 μm;

[0036] and / or, a coating of organic resin and inorganic filler; the thickness of the coating applied on the proppant substrate is 0.01 to 5 μm, preferably 0.1 to 3 μm, and more preferably 0.2 to 0.5 μm;

[0037] And / or, the organic resin is an organic polymer containing hydroxyl groups, for example, the organic polymer containing hydroxyl groups may be one or more hydroxyl-modified resins such as hydroxyl-modified epoxy resins, polyphenolic hydroxyl-containing phenolic resins, hydroxyl-modified polyolefin resins, hydroxyl-modified polyacrylic resins, etc., for example, the organic polymer containing hydroxyl groups may be polyhydroxyamine-modified epoxy resins, polyhydroxy ether-modified epoxy resins;

[0038] And / or, the inorganic material is nano-silicon dioxide, and the inorganic filler is dispersed on the interface of the coating away from the proppant substrate; it should be noted that the inorganic filler is dispersed on the interface of the coating away from the proppant substrate means that the inorganic filler is not evenly distributed in the coating, nor is it completely distributed on the surface of the organic resin layer, but is embedded in the surface of the organic resin layer, and may be partially distributed inside the coating and partially distributed on the surface of the coating away from the proppant substrate;

[0039] Hexamethyldisiloxane is partially or completely grafted onto the coating via hydroxyl groups; the organic polymer containing hydroxyl groups reacts with hexamethyldisiloxane during the modification process to achieve hydrophobic modification of the surface of the organic polymer and improve the hydrophobicity of the proppant surface; in addition, the use of hexamethyldisiloxane to modify the inorganic filler nanosilica can not only improve the hydrophobicity of the proppant matrix, but also increase the specific surface area of ​​the proppant to form a rough surface, thereby further improving the hydrophobicity and conductivity of the proppant.

[0040] In some embodiments, the mass ratio of the organic resin to the inorganic filler is (20:1) to (5:1). Preferably, the mass ratio of the organic resin to the inorganic filler is (15:1) to (8:1).

[0041] In some embodiments, the proppant matrix is ​​mesoporous aluminum oxide particles, and the porosity of the mesoporous aluminum oxide particles is not less than 10% and not more than 30%, which can further increase the modified specific surface area. It should be noted that the porosity of the mesoporous aluminum oxide particles should not be too high to avoid a significant decrease in the strength of the proppant and easy crushing.

[0042] In some embodiments, the organic resin is a resin that can swell, but the swelling rate of the resin should not be too high. Excessive swelling can easily lead to a decrease in the conductivity of the proppant packing layer. The saturated swelling rate of the organic resin is not higher than 30%. Further, the saturated swelling rate of the organic resin is not higher than 20%, and more preferably, the saturated swelling rate of the organic resin is not higher than 10%.

[0043] The present application also provides a method for preparing a modified proppant for fracturing:

[0044] Prepare mesoporous ceramic particles as a proppant matrix, prepare an organic resin containing hydroxyl groups, prepare a nano-silica dispersion, and prepare a polar small molecule solution of hexamethyldioxysilane;

[0045] By filtering, the organic resin solution forms an organic liquid film on the surface of the proppant matrix;

[0046] Then, the nano-silicon dioxide dispersion forms a liquid film containing inorganic fillers on the surface of the organic filter membrane by filtering; the organic liquid film and the liquid film of the inorganic filler together form a coating;

[0047] Then, the proppant substrate with the coating layer is modified by using hexamethyldisiloxane to obtain a modified proppant.

[0048] In some embodiments, the organic resin solution is filtered to form an organic liquid film on the surface of the proppant substrate, which means: filtering the organic resin solution for 1 to 20 minutes at a pressure of 0.01 to 0.3 MPa to form an organic liquid film on the surface of the proppant substrate;

[0049] And / or, using filtration to form a layer of liquid film containing inorganic filler on the surface of the organic liquid film by the inorganic filler dispersion, means: filtering for 0.5 to 10 minutes under a pressure of 0.01 to 0.5 MPa, so that the inorganic filler dispersion forms a layer of liquid film containing inorganic filler on the surface of the organic liquid film;

[0050] and / or, the concentration of the organic resin solution is 0.1 to 10% by mass;

[0051] And / or, the concentration of the inorganic filler in the inorganic filler dispersion liquid is 0.1 to 10% by mass.

[0052] In some embodiments, modifying the coated proppant substrate with hexamethyldisiloxane means: dispersing the coated proppant substrate in a polar small molecule solution of hexamethyldisiloxane, stirring the modification reaction at 30 to 80° C. for 2 to 12 hours; wherein the concentration of the hexamethyldisiloxane solution is 0.5 to 3% by mass.

[0053] It should be noted that when hexamethyldisiloxane is used to modify the coated proppant substrate, the hexamethyldisiloxane is added in excess so that the hydroxyl groups in the coating of the proppant are completely or nearly completely grafted with the hexamethyldisiloxane, thereby increasing the hydrophobic properties of the proppant as much as possible.

[0054] The specific embodiments are further described below by examples:

[0055] (Example 1)

[0056] This embodiment provides a modified proppant for fracturing, which is prepared by the following method:

[0057] S1: using isopropanol as solvent, preparing a bisphenol epoxy resin solution with a concentration of 0.5% by mass, a nano-silicon dioxide dispersion with a concentration of 0.5% by mass (the average particle size of the nano-silicon dioxide is 20 nm), and a hexamethyldisiloxane solution with a concentration of 1% by mass for standby use;

[0058] S2: placing mesoporous aluminum oxide particles (particle size 40-200 μm, porosity 20%) on an ultrafiltration device, filtering the mesoporous aluminum oxide particles with a bisphenol epoxy resin solution at a pressure of 0.1 MPa and a temperature of 35° C. for 15 min, and then filtering with a nano-silicon dioxide dispersion at a pressure of 0.2 MPa and a temperature of 25° C. for 5 min;

[0059] S3: immersing the coated proppant substrate in S2 into a hexamethyldisiloxane solution and stirring the modified reaction at 50°C for 5h;

[0060] S4: Filter and vacuum dry the particles after the reaction for 1 hour to obtain a modified proppant.

[0061] (Example 2)

[0062] This embodiment provides a modified proppant for fracturing, which is prepared by the following method:

[0063] S1: using isopropanol as solvent, preparing a bisphenol epoxy resin solution with a concentration of 5% by mass, a nano-silicon dioxide dispersion with a concentration of 5% by mass (the average particle size of the nano-silicon dioxide is 20 nm), and a hexamethyldisiloxane solution with a concentration of 3% by mass for later use;

[0064] S2: placing mesoporous aluminum oxide particles (particle size 40-200 μm, porosity 20%) on an ultrafiltration device, filtering the mesoporous aluminum oxide particles with a bisphenol epoxy resin solution at a pressure of 0.05 MPa and a temperature of 35° C. for 20 min, and then filtering with a nano-silicon dioxide dispersion at a pressure of 0.1 MPa and a temperature of 25° C. for 8 min;

[0065] S3: immersing the coated proppant substrate in S2 into a hexamethyldisiloxane solution and stirring the modification reaction at 30°C for 12 hours;

[0066] S4: Filter and vacuum dry the particles after the reaction for 1 hour to obtain a modified proppant.

[0067] (Example 3)

[0068] This embodiment provides a modified proppant for fracturing, which is prepared by the following method:

[0069] S1: using isopropanol as solvent, preparing a bisphenol epoxy resin solution with a concentration of 1% by mass, a nano-silicon dioxide dispersion with a concentration of 1% by mass (the average particle size of the nano-silicon dioxide is 20 nm), and a hexamethyldisiloxane solution with a concentration of 2% by mass for later use;

[0070] S2: placing mesoporous aluminum oxide particles (particle size 40-200 μm, porosity 20%) on an ultrafiltration device, filtering the mesoporous aluminum oxide particles with a bisphenol epoxy resin solution at a pressure of 0.2 MPa and a temperature of 30° C. for 15 min, and then filtering with a nano-silicon dioxide dispersion at a pressure of 0.4 MPa and a temperature of 25° C. for 5 min;

[0071] S3: immersing the coated proppant substrate in S2 into a hexamethyldisiloxane solution and stirring the modified reaction at 80°C for 1 hour;

[0072] S4: Filter and vacuum dry the particles after the reaction for 1 hour to obtain a modified proppant.

[0073] (Test example)

[0074] Comparative Example 1

[0075] Compared with Example 1, step S3 is omitted in this comparative example, and the remaining steps are the same as those in Example 1, thereby obtaining a comparative modified proppant 1.

[0076] Comparative Example 2

[0077] Compared with Example 1, step S2 is omitted in this comparative example, and the remaining steps are the same as those in Example 1, thereby obtaining a comparative modified proppant 2.

[0078] Comparative Example 3

[0079] Compared with Example 1, this comparative example omits the step S2 of "then filtering with the nano-silica dispersion at a pressure of 0.4 MPa and a temperature of 25° C. for 5 min", and the remaining steps are the same as those in Example 1, to obtain a comparative modified proppant 3.

[0080] The modified proppants of Examples 1 to 3 and the modified proppants of Comparative Examples 1 to 3 were subjected to hydrophobicity measurement and flow conductivity measurement, respectively. The hydrophobicity measurement was characterized by the contact angle between the modified proppant tablet and distilled water, and the flow conductivity measurement was characterized by the water flow rate of the modified proppant in the sand filling pipe displacement experiment. The characterization results are shown in Table 1 below:

[0081] Table 1 Contact angle and flow conductivity of Examples 1 to 3 and Comparative Examples 1 to 3

[0082] Water contact angle (°) <![CDATA[Water output flow rate( mL / min)]]> Example 1 51.7 26.9 Example 2 96.4 57.4 Example 3 66.8 30.9 Comparative Example 1 27.5 10.1 Comparative Example 2 33.1 12.4 Comparative Example 3 40.4 21.6

[0083] In Table 1, by comparing Examples 1 to 3 with Comparative Example 1, it can be seen that the contact angle and water flow rate of the modified proppant are greatly improved; from Comparative Examples 1 to 3, it can be seen that the modification effect of the proppant matrix after being treated with organic resin and nano-silicon dioxide is better than the modification effect of directly using the proppant matrix. It can be seen that the modified proppant for fracturing provided by the present application has good hydrophobicity and flow conductivity, thereby improving the flowback rate and oil and gas recovery rate.

[0084] The modified proppant of Example 2 was added to the slick water fracturing fluid at a concentration of 15%, and stirred at 5500 r / min for 90 seconds using a high-speed stirrer and then left to stand for observation. High-speed stirring will produce a large number of bubbles, which can simulate the microbubbles produced by the liquid nitrogen injected during fracturing construction. The results are shown in Figure 1 .

[0085] from Figure 1 It can be seen that after 10 minutes of static sedimentation, most of the modified proppant of Example 2 is suspended in the slick water fracturing fluid, and only a small amount of sedimentation occurs. The proppant is relatively fluffy due to the adsorption of bubbles. It can be seen that the surface of the modified proppant has a certain affinity for air, and can adsorb and combine with microbubbles in the fracturing fluid, and improve the suspension state of the proppant in the fracturing fluid with the help of the buoyancy of the bubbles, thereby improving the suspension of the proppant and the ability of long-distance transportation in the fracture.

[0086] The above embodiments only express preferred implementation modes, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the present invention. It should be pointed out that, for ordinary technicians in this field, several modifications and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention.

Claims

1. A modified proppant for fracturing, Features: The invention comprises a proppant matrix made of ceramic particles, a coating is coated on the surface of the proppant matrix, and hexamethyldisiloxane is grafted on the coating.

2. A modified proppant for fracturing and a preparation method thereof according to claim 1, Features: The coating comprises organic resin and inorganic filler; The organic resin is an organic compound containing hydroxyl groups, the inorganic filler is nano silicon dioxide; and the hexamethyldisiloxane is grafted onto the coating via hydroxyl groups.

3. A modified proppant for fracturing and a preparation method thereof according to claim 2, Features: The mass ratio of the organic resin to the inorganic filler is (20:1) to (5:1).

4. A modified proppant for fracturing and a preparation method thereof according to claim 3, Features: The saturated swelling rate of the organic resin is not higher than 10%.

5. A modified proppant for fracturing and a preparation method thereof according to claim 1 or 3, Features: The proppant matrix is ​​mesoporous aluminum oxide ceramic particles, and the porosity of the aluminum oxide ceramic particles is not less than 10% and not more than 30%.

6. A method for preparing a modified proppant for fracturing, Features: Prepare mesoporous ceramic particles as a proppant matrix, prepare an organic resin containing hydroxyl groups, prepare a nano-silica dispersion, and prepare a polar small molecule solution of hexamethyldioxysilane; By filtering, the organic resin solution forms an organic liquid film on the surface of the proppant matrix; Then, the nano-silicon dioxide dispersion forms a liquid film containing inorganic fillers on the surface of the organic filter membrane by filtering; the organic liquid film and the liquid film of the inorganic filler together form a coating; Then, the proppant substrate with the coating layer is modified by using hexamethyldisiloxane to obtain a modified proppant.

7. The method for preparing a modified proppant for fracturing according to claim 6, Features: The method of filtering the organic resin solution to form an organic liquid film on the surface of the proppant substrate refers to filtering the organic resin solution for 1 to 20 minutes under a pressure of 0.01 to 0.3 MPa to form an organic liquid film on the surface of the proppant substrate. And / or, the method of filtering the inorganic filler dispersion to form a liquid film containing the inorganic filler on the surface of the organic liquid film refers to filtering for 1 to 10 minutes at a pressure of 0.01 to 0.5 MPa to form a liquid film containing the inorganic filler on the surface of the organic liquid film; And / or, the concentration of the organic resin solution is 0.1 to 10% by mass; And / or, the concentration of the inorganic filler in the inorganic filler dispersion is 0.1 to 10% by mass.

8. The method for preparing a modified proppant for fracturing according to claim 7, Features: The method of modifying the coated proppant substrate with hexamethyldisiloxane refers to: dispersing the coated proppant substrate in a polar small molecule solution of hexamethyldisiloxane, stirring the modification reaction at 30 to 80° C. for 2 to 12 hours; wherein the concentration of the hexamethyldisiloxane solution is 0.5 to 3% by mass.

Citation Information

Patent Citations

  • Slurry compositions and methods for making same

    CN101268150A

  • Functional resin tectorial membrane proppant and preparation method thereof

    CN101531893A

  • Hydrophobic proppant and preparation method thereof

    CN102443387A

  • Oil and gas well proppants of silicone-resin-modified phenolic resins

    CN104769075A

  • Oil-based shale debris proppant and preparation method thereof

    CN111004620A