Method for preparing spinnable mesophase pitch from hydrogenated tail oil modified coal pitch

Through pressurized polymerization and reduced pressure polymerization reaction of hydrogenated tail oil and medium-temperature coal asphalt under high temperature and high pressure conditions, combined with nitrogen purge, the catalyst residue, high cost of hydrogen supply solvent and complex process in the prior art is solved. In the problem, spinning mesophase asphalt with low softening points and high mesophase content was prepared, achieving the effect of long-distance spinning and cost reduction.

CN118995256APending Publication Date: 2024-11-22ZHENGZHOU ZHONGKE EMERGING IND TECH RES INST +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411121025.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-15
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The existing hydrogenation method for preparing spinned mesophase bitumen has problems such as catalyst residue affecting spinning performance, high cost of hydrogen supply solvents and complex process.

Method used

Pressurized polymerization reaction with hydrogenated tail oil and medium-temperature coal asphalt under high temperature and high pressure conditions, followed by reduced pressure polymerization and nitrogen purge to prepare a spinnable intermediate phase with low softening point and high mesophase content. asphalt.

Benefits of technology

The spinned mesophase asphalt with low softening point and high mesophase content is achieved, with a large and wide-area streamlined optical texture, and can be continuously spinned more than 10 km, reducing cost and process complexity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118995256A_ABST
    Figure CN118995256A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of carbon material preparation, and relates to preparation of spinnable mesophase pitch, in particular to a method for preparing spinnable mesophase pitch from hydrogenated tail oil modified coal pitch, which is used for solving the technical problems of high hydrogenation modification cost, complex process flow and low yield of mesophase pitch at present. The hydrogenation tail oil light component oil is mixed with coal pitch, high-temperature and high-pressure reaction is performed to obtain modified pitch, and the modified pitch is subjected to high-temperature reduced-pressure polymerization and then subjected to nitrogen purging to obtain the high-quality spinnable mesophase pitch. The method is wide in raw material source, low in cost and simple in process flow, and does not need to add a hydrogen donor and a catalyst; the prepared mesophase pitch has a large-wide-area streamline optical texture, the mesophase content is high (gt; 95%), the softening point is low (255-285 DEG C), and continuous melt spinning can be carried out for 10 km or above.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of carbon material preparation, and in particular to a method for preparing spinnable mesophase asphalt by hydrogenating tail oil-modified coal tar pitch. Background Art

[0002] Mesophase pitch is a nematic liquid crystal structure, which is mainly generated by heavy aromatic hydrocarbons through hydrogen transfer reaction, free radical reaction, ring growth reaction and aromatic molecule polycondensation reaction. Coal tar pitch has a large C / H value and is a high-quality raw material for preparing spinnable mesophase pitch. However, since coal tar pitch contains fewer side chains, the violent free radical reaction leads to over-polymerization, and the formed mesophase pitch has a high softening point and poor order, which is not conducive to spinning. By hydrogenating and modifying coal tar pitch, introducing alkane side chains, reducing the viscosity of the reaction system, and improving rheology, it is conducive to forming an ordered structure of the mesophase and preparing a low softening point mesophase pitch. The commonly used hydrogenation methods are catalytic hydrogenation and solvent hydrogenation. The residual catalyst in the catalytic hydrogenation method is difficult to remove, which affects the quality of subsequent products. The solvent hydrogenation method requires the hydrogen supply solvent to have a strong hydrogen supply performance, but it is generally expensive and used in large quantities, resulting in high costs. Patent 202310544069.X uses hydrogen-donating solvents and catalysts to hydrogenate and modify the heavy components of coal tar, and mixes them with the extracted light components. The prepared mesophase asphalt has a high anisotropy content, but the added Fe2O3, Co, Mo and other catalysts are not removed, which will affect the spinning performance of the mesophase asphalt and the mechanical properties of carbon fiber. In addition, the hydrogen-donating solvents such as tetralin and dihydroanthracene used are relatively expensive.

[0003] Patent CN116005298A discloses a method for preparing mesophase asphalt for braided high-performance carbon fibers. Long-chain carbon olefins (C atoms are 20-30) are used to modify the residual oil-based mesophase asphalt under the action of a Lewis catalyst to obtain a mesophase asphalt with better spinning performance, thereby improving the spinning performance of the mesophase asphalt. However, the Lewis acid catalyst is not easy to completely remove, and the patent uses acid washing to remove impurities, which has a complicated process. Summary of the invention

[0004] In view of the above technical problems, the present invention proposes a method for preparing spinnable mesophase asphalt by hydrogenating tail oil modified coal tar, which overcomes the shortcomings of the existing solvent hydrogenation method, such as high cost and complicated process. The prepared mesophase asphalt has a lower softening point and a higher mesophase content, and has a large-area streamlined optical texture, and can be spun continuously for more than 10 km.

[0005] In order to achieve the above object, the technical solution of the present invention is achieved as follows: A method for preparing spinnable mesophase asphalt by modifying coal tar pitch with hydrogenated tail oil comprises the following steps: (1) Mixing the light component oil obtained by vacuum distillation of hydrogenated tail oil with medium-temperature coal tar pitch, and subjecting them to pressure polymerization to obtain modified asphalt; (2) Then the modified asphalt in step (1) is polymerized under reduced pressure and further purged with nitrogen to obtain a spinnable mesophase asphalt.

[0006] The hydrogenated tail oil in step (1) is coal tar hydrocracking tail oil.

[0007] In the step (1), the reduced pressure distillation temperature is 340-360°C and the pressure is 1-40 kPa.

[0008] In the step (1), the mass ratio of the light component oil to the medium-temperature coal tar pitch is (0.5-2): 1; the content of quinoline insoluble matter in the medium-temperature coal tar pitch is <0.1%.

[0009] In the step (1), the pressure polymerization reaction temperature is 400-440°C, the pressure is 3-5 MPa, and the maintenance time is 2-5 h.

[0010] The heating rate of the pressurized polymerization reaction is 5 to 10 °C / min, and the stirring rate is 200 to 300 rmp.

[0011] In the step (2), the reduced pressure polymerization reaction temperature is 380-400°C, the pressure is 1-40 kPa, and the maintenance time is 2-4 h.

[0012] The stirring rate of the reduced pressure polymerization reaction is 200-300 rmp.

[0013] In the step (2), the nitrogen purge temperature is 390 to 420°C, the nitrogen flow rate is 300 to 600 L / h, the stirring rate is 200 to 300 rmp, and the maintenance time is 5 to 24 h.

[0014] The spinnable mesophase pitch prepared by any of the above methods has a softening point of 255-285°C, a mesophase content of >95%, and a large-area streamlined optical texture; the spinnable mesophase pitch can be continuously melt-spun for more than 10 km.

[0015] The light component oil in the hydrogenated tail oil contains more cycloalkane structures and long alkane side chains, and has good hydrogen transfer and hydrogen supply capabilities. It can be used to modify coal tar pitch to prepare spinnable mesophase asphalt. It has two main functions: (1) The light component oil acts as a hydrogen donor to hydrogenate and modify coal tar pitch, thereby increasing the hydrogen-carbon ratio of coal tar pitch and preventing excessive polycondensation of the reaction system; (2) The light component oil exists as a solvent, effectively reducing the viscosity of the reaction system, making the mesophase spheres easier to melt and generating large-basin structure mesophase asphalt.

[0016] The present invention has the following beneficial effects: 1. The present invention utilizes the light component oil of hydrogenated tail oil to have a strong hydrogen supply capacity, and hydrogen transfer occurs between the component molecules of medium-temperature coal tar under high temperature and high pressure conditions, which can increase the hydrogen-carbon ratio of coal tar, improve the rheological properties of asphalt, inhibit excessive condensation of coal tar molecules, and form an intermediate phase ordered crystal structure.

[0017] 2. The light component oil of the hydrogenated tail oil of the present invention contains more alkyl side chains and cycloalkane structures, which can effectively reduce the viscosity of the reaction system, make the small spheres of the mesophase easier to merge, generate a large-scale streamlined mesophase ordered crystal structure, and improve the structural uniformity and graphitization of the mesophase asphalt.

[0018] 3. The hydrogenation tail oil in the preparation method of the present invention is widely available and inexpensive; no catalyst is required, which reduces the subsequent catalyst separation process; the process conditions have low requirements on equipment and the process flow is simple.

[0019] 4. The spinnable mesophase pitch prepared by the method of the present invention has a large-area streamlined optical texture, a high mesophase content, a low softening point, and can be continuously melt-spun for more than 10 km. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0021] Figure 1 This is a polarizing microscope image of the mesophase asphalt prepared in Example 1 of the present invention. DETAILED DESCRIPTION

[0022] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0023] Example 1 The method for preparing spinnable mesophase asphalt by hydrogenating tail oil modified coal tar pitch in this embodiment comprises the following steps: The hydrogenated tail oil was distilled under reduced pressure at 340 °C and 1 KPa to obtain light component oil, which was mixed with medium-temperature coal tar pitch at a mass ratio of 0.5:1 and added into an autoclave, wherein the content of quinoline insoluble matter in the medium-temperature coal tar pitch was less than 0.1%. The autoclave was protected by nitrogen and heated to 400 °C at a rate of 5 °C / min. The autoclave was subjected to pressure polymerization reaction at a constant pressure of 3 MPa for 5 h under stirring at 300 rmp. Then the temperature was lowered to 380 °C and high-temperature gas was released. Under stirring at 200 rpm, the polymerization reaction was carried out at 1 KPa under reduced pressure for 4 h. The stirring rate of the reduced pressure polymerization reaction was 300 rpm. Then nitrogen was introduced, the temperature was raised to 400 °C, the nitrogen flow rate was 300 L / h, the nitrogen was purged for 24 h, and the nitrogen purging stirring rate was 200 rpm. A spinnable mesophase pitch was obtained. The polarizing microscope image of the obtained mesophase pitch is shown in FIG. Figure 1 As shown, it has a large-area streamlined optical texture.

[0024] Example 2 The method for preparing spinnable mesophase asphalt by hydrogenating tail oil modified coal tar pitch in this embodiment comprises the following steps: The hydrogenated tail oil was distilled under reduced pressure at 350 °C and 20 KPa to obtain light component oil, which was mixed with medium-temperature coal tar pitch in a mass ratio of 1:1 and added into an autoclave, wherein the content of quinoline insoluble matter in the medium-temperature coal tar pitch was less than 0.1%. The autoclave was protected by nitrogen and heated to 420 °C at a rate of 8 °C / min. The autoclave was subjected to a polymerization reaction at a constant pressure of 5 MPa for 2 h under stirring at 250 rmp. Then the temperature was lowered to 390 °C and high temperature was released, and the reduced pressure polymerization reaction was carried out at 20KPa for 3 hours, and the stirring rate of the reduced pressure polymerization reaction was 200 rmp; then nitrogen was introduced, the temperature was raised to 410 °C, the nitrogen flow rate was 500 L / h, the purge reaction was carried out for 12 hours, and the nitrogen purge stirring rate was 200-300 rmp; and a spinnable mesophase asphalt was obtained.

[0025] Example 3 The method for preparing spinnable mesophase asphalt by hydrogenating tail oil modified coal tar pitch in this embodiment comprises the following steps: The hydrogenated tail oil was distilled under reduced pressure at 360 °C and 40 KPa to obtain light component oil, which was mixed with medium-temperature coal tar pitch at a mass ratio of 2:1 and added into an autoclave. The content of quinoline insoluble matter in the medium-temperature coal tar pitch was less than 0.1%. The autoclave was purged with nitrogen and heated to 440 °C at a rate of 5 °C / min. The autoclave was stirred at 200 rmp and reacted at a constant pressure of 5 MPa for 5 h. Then the temperature was lowered to 400 °C and high temperature was released, and the reduced pressure polymerization reaction was carried out at 20 KPa for 2 h, and the stirring rate of the reduced pressure polymerization reaction was 200 rmp; then nitrogen was introduced, the temperature was raised to 420 °C, the nitrogen flow rate was 600 L / h, the purge reaction was carried out for 5 h, and the nitrogen purge stirring rate was 300 rmp; and a spinnable mesophase asphalt was obtained.

[0026] Example 4 The method for preparing spinnable mesophase asphalt by hydrogenating tail oil modified coal tar pitch in this embodiment comprises the following steps: The hydrogenated tail oil was distilled under reduced pressure at 350 °C and 40 KPa to obtain light component oil, which was mixed with medium-temperature coal tar pitch at a mass ratio of 2:1 and added into an autoclave. The content of quinoline insoluble matter in the medium-temperature coal tar pitch was less than 0.1%. The autoclave was purged with nitrogen and heated to 420 °C at a rate of 10 °C / min. The autoclave was stirred at 200 rmp and reacted at a constant pressure of 5 MPa for 5 h. Then, the temperature was lowered to 400 °C and high-temperature gas was released, and the reduced-pressure polymerization reaction was carried out at 40 KPa for 2 h, and the stirring rate of the reduced-pressure polymerization reaction was 250 rmp; then nitrogen was introduced, the temperature was raised to 420 °C, the nitrogen flow rate was 600 L / h, the purge reaction was carried out for 8 h, and the nitrogen purge stirring rate was 200 rmp; and a spinnable mesophase asphalt was obtained.

[0027] The properties of the spinnable mesophase pitch prepared in Examples 1-4 are shown in Table 1.

[0028] Table 1: Properties of spinnable mesophase pitch prepared in the examples of the present invention Example 5 The method for preparing spinnable mesophase asphalt by hydrogenating tail oil modified coal tar pitch in this embodiment comprises the following steps: The hydrogenated tail oil was distilled under reduced pressure at 360 °C and 30 KPa to obtain light component oil, which was mixed with medium-temperature coal tar pitch at a mass ratio of 2:1 and added into an autoclave, where the content of quinoline insoluble matter in the medium-temperature coal tar pitch was less than 0.1%. The autoclave was purged with nitrogen and heated to 420 °C at a rate of 10 °C / min. The autoclave was stirred at 200 rmp and reacted at a constant pressure of 4 MPa for 4 h. Then, the temperature was lowered to 400 °C and high-temperature gas was released, and the reduced-pressure polymerization reaction was carried out at 40 KPa for 2 h, and the stirring rate of the reduced-pressure polymerization reaction was 250 rmp; then nitrogen was introduced, the temperature was raised to 420 °C, the nitrogen flow rate was 500 L / h, the purge reaction was carried out for 8 h, and the nitrogen purge stirring rate was 250 rmp; and a spinnable mesophase asphalt was obtained.

[0029] Example 6 The method for preparing spinnable mesophase asphalt by hydrogenating tail oil modified coal tar pitch in this embodiment comprises the following steps: The hydrogenated tail oil was distilled under reduced pressure at 360 °C and 30 KPa to obtain light component oil, which was mixed with medium-temperature coal tar pitch at a mass ratio of 2:1 and added into an autoclave, where the content of quinoline insoluble matter in the medium-temperature coal tar pitch was less than 0.1%. The autoclave was purged with nitrogen and heated to 440 °C at a rate of 10 °C / min. The autoclave was stirred at 200 rmp and reacted at a constant pressure of 4 MPa for 4 hours. Then, the temperature was lowered to 380 °C and high-temperature gas was released, and the reduced-pressure polymerization reaction was carried out at 1 KPa for 4 h, and the stirring rate of the reduced-pressure polymerization reaction was 300 rmp; then nitrogen was introduced, the temperature was raised to 400 °C, the nitrogen flow rate was 500 L / h, the purge reaction was carried out for 8 h, and the nitrogen purge stirring rate was 300 rmp; and a spinnable mesophase asphalt was obtained.

[0030] Example 7 The method for preparing spinnable mesophase asphalt by hydrogenating tail oil modified coal tar pitch in this embodiment comprises the following steps: The hydrogenated tail oil was distilled under reduced pressure at 340 °C and 1 KPa to obtain light component oil, which was mixed with medium-temperature coal tar pitch at a mass ratio of 1:1 and added into an autoclave, where the content of quinoline insoluble matter in the medium-temperature coal tar pitch was less than 0.1%. The autoclave was purged with nitrogen and heated to 420 °C at a rate of 10 °C / min. The autoclave was stirred at 200 rmp and reacted at a constant pressure of 4 MPa for 4 h. Then, the temperature was lowered to 400 °C and high-temperature gas was released, and the reduced-pressure polymerization reaction was carried out at 40 KPa for 2 h, and the stirring rate of the reduced-pressure polymerization reaction was 200 rmp; then nitrogen was introduced, the temperature was raised to 400 °C, the nitrogen flow rate was 300 L / h, the purge reaction was carried out for 24 h, and the nitrogen purge stirring rate was 200 rmp; and a spinnable mesophase asphalt was obtained.

[0031] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing spinnable mesophase pitch by modifying coal tar pitch with hydrogenated tail oil, It is characterized in that The steps include: (1) Mixing the light component oil obtained by vacuum distillation of hydrogenated tail oil with medium-temperature coal tar pitch, and then subjecting it to pressure polymerization to obtain modified asphalt; (2) Then the modified asphalt in step (1) is polymerized under reduced pressure and further purged with nitrogen to obtain a spinnable mesophase asphalt.

2. The method for preparing spinnable mesophase pitch by modifying coal tar pitch with hydrogenated tail oil according to claim 1, Features: The hydrogenated tail oil in step (1) is coal tar hydrocracking tail oil.

3. The method for preparing spinnable mesophase pitch by modifying coal tar pitch with hydrogenated tail oil according to claim 2, Features: In the step (1), the reduced pressure distillation temperature is 340-360°C and the pressure is 1-40 kPa.

4. The method for preparing spinnable mesophase pitch by modifying coal tar pitch with hydrogenated tail oil according to claim 1, Features: In the step (1), the mass ratio of the light component oil to the medium-temperature coal tar pitch is (0.5-2): 1; the content of quinoline insoluble matter in the medium-temperature coal tar pitch is <0.1%.

5. The method for preparing spinnable mesophase pitch by modifying coal tar pitch with hydrogenated tail oil according to claim 1, Features: In the step (1), the pressure polymerization reaction temperature is 400-440°C, the pressure is 3-5 MPa, and the maintenance time is 2-5 hours.

6. The method for preparing spinnable mesophase pitch by modifying coal tar pitch with hydrogenated tail oil according to claim 5, Features: The heating rate of the pressurized polymerization reaction is 5 to 10 °C / min, and the stirring rate is 200 to 300 rmp.

7. The method for preparing spinnable mesophase pitch by modifying coal tar pitch with hydrogenated tail oil according to claim 1, Features: In the step (2), the reduced pressure polymerization reaction temperature is 380-400°C, the pressure is 1-40 kPa, and the maintenance time is 2-4 h.

8. The method for preparing spinnable mesophase pitch by modifying coal tar pitch with hydrogenated tail oil according to claim 7, Features: The stirring rate of the reduced pressure polymerization reaction is 200-300 rmp.

9. The method for preparing spinnable mesophase pitch by modifying coal tar pitch with hydrogenated tail oil according to claim 1, Features: In the step (2), the nitrogen purge temperature is 390 to 420°C, the nitrogen flow rate is 300 to 600 L / h, the stirring rate is 200 to 300 rmp, and the maintenance time is 5 to 24 h.

10. A spinnable mesophase pitch prepared by the method according to any one of claims 1 to 9, Features: The softening point of the spinnable mesophase pitch is 255-285°C, the mesophase content is >95%, and it has a large-area streamlined optical texture; the spinnable mesophase pitch can be continuously melt-spun for more than 10 km.