Steelmaking continuous casting process control method for rare earth high-yield deep drawing steel

By controlling the converter oxygen content, top slag modification and vacuum decarbonization, the problems of oxidation and inclusion formation of rare earth elements during steelmaking and continuous casting are solved, and the stability of high yield of rare earth deep-drawing steel is achieved. Improved supply and production efficiency.

CN118996030APending Publication Date: 2024-11-22BAOTOU IRON & STEEL (GROUP) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411063634.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-05
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

Rare earth elements are prone to oxidation during steelmaking and continuous casting, resulting in process interruption, forming large-size and high-density inclusions, affecting the stability of steel performance and making it difficult to control high yields.

Method used

By controlling the oxygen content at the end point of the converter, the top slag modification after the furnace, RH vacuum decarbonization and slag system treatment, the cleanliness of the steel before rare earth alloying is ensured, and graphite sealing rings and argon protection are used during the casting process, and the constant setting is set Pulling speed and appropriate pouring time ensure high yield of rare earth elements.

Benefits of technology

The stable control of the rare earth content in steel is achieved above 45%, which improves the yield and production efficiency of rare earth elements, avoids process interruption and unstable steel performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118996030A_ABST
    Figure CN118996030A_ABST
Patent Text Reader

Abstract

The invention discloses a steelmaking continuous casting process control method for rare earth high-yield deep drawing steel, which realizes high cleanliness of steel before rare earth alloying through measures such as converter end point oxygen content control, furnace rear top slag modification, RH vacuum decarburization and furnace rear slag system treatment, effectively improves the yield of rare earth elements, and simultaneously improves the yield of the rare earth elements. The production efficiency is improved; the continuous casting is ensured; compared with conventional production, the method has the advantages that the problem of flocculation of the rare earth deep drawing steel is solved, meanwhile, the yield of the rare earth elements in the steel is greatly increased, the yield of the rare earth elements in the steel can be stably controlled to be 45% or above, and therefore successful development and stable supply of the rare earth high-yield deep drawing steel are achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for controlling a steelmaking and continuous casting process of deep drawing steel with high rare earth yield. Background Art

[0002] In recent years, as researchers gradually realize that trace rare earth elements are the only elements in microalloyed steel that can deeply purify molten steel, denature inclusions, improve the internal structure of continuous casting billets, and improve various properties of steel, they have an irreplaceable unique microalloying effect, which has prompted the research on the role of rare earth microalloying to become a hot topic in recent years. Taking advantage of the outstanding role of rare earth in steel grades, the method of replacing single or composite precious metal elements with rare earth elements is often used to design products, and the development of microalloyed steel with different rare earth contents has become a weather vane for product development. For rare earth microalloyed steel, different smelting addition processes and addition timings affect the stability of rare earth element recovery. In addition, since rare earth elements are extremely easy to oxidize, rare earths added to molten steel will block the pouring system, and the continuous casting process will be forced to be interrupted, seriously affecting the smooth process; after rare earths are added, large-sized, high-density rare earth inclusions are easily formed, resulting in unstable steel performance, which is also a problem that needs to be solved in steelmaking and continuous casting processes. Summary of the invention

[0003] The purpose of the present invention is to provide a method for controlling the steelmaking continuous casting process of deep drawing steel with high rare earth yield, especially to control the yield of rare earth content in steel, so as to achieve stable control of the yield of rare earth content in steel at a level above 45%, thereby realizing the successful development and stable supply of deep drawing steel with high rare earth yield.

[0004] In order to solve the above technical problems, the present invention adopts the following technical solutions:

[0005] The present invention provides a method for controlling a rare earth high-yield deep-drawing steelmaking and continuous casting process, comprising the following steps:

[0006] 1). The amount of molten iron added to the converter is 263±3t, and the amount of self-produced scrap steel added is 45±3t;

[0007] 2). The oxygen control requirement for steel tapping in converter is 650-750ppm. If the oxygen in steel tapping is > 1000ppm, add 500±20kg of raw white oxygen reduction post-treatment;

[0008] 3). The target of converter tapping stability control is 1640-1670℃. The temperature of the first quick-change furnace is not less than 1665℃;

[0009] 4). The slag making after the converter requires that 600-800kg of lime be added to the converter before steel is tapped, and 200-250kg of top slag modifier be added. After steel is tapped, aluminum particles are used for top slag modification. Argon stirring is not allowed during the aluminum particle throwing process and after modification;

[0010] 5).RH in-situ conditions require RH vacuum treatment for 5 minutes to determine oxygen, the first furnace is controlled at 1610-1620℃, the continuous casting furnace is controlled at 1600-1610℃, and the oxygen content is controlled at 350-500ppm;

[0011] 6). RH decarburization process: decarburization time is 17 minutes, pure degassing time is 7 minutes, and each blowing is 100Nm 3 The oxygen pure degassing was extended for 1 minute;

[0012] 7). The time interval between RH deoxidation and alloying is 4 minutes, and the rare earth alloy is added during the alloying process;

[0013] 8). After the RH negative pressure is broken, when the molten steel leaves the immersion tube, 50-100kg of aluminum particles are sprinkled on the surface of the slag to modify the top slag;

[0014] 9). Refining final slag components CaO content 40 ~ 55%, Al 2 O 3 Content 20~35%, SiO 2 Content 5-15%, C / A range 1.4-1.8;

[0015] 10). Before pouring, argon is blown in the tundish for a time of >3 min. To ensure the tightness of the long nozzle, use a graphite sealing ring, and the argon flow rate is 2-6 L / min. Pay attention to the tumbling of the molten steel in the impact zone, and the flow rate can be increased appropriately. After temperature measurement and sampling, the covering agent must be added. The casting machine is required to increase N ≤5ppm.

[0016] 11). Set the pulling speed to 1.00-1.20m / min and maintain a constant pulling speed. The pouring time is controlled at 45-50min.

[0017] Furthermore, in the step 1), 263 tons of molten iron and 45 tons of self-produced scrap steel are added to the converter.

[0018] Furthermore, in the step 2), 500 kg of raw white is added for oxygen reduction post-treatment.

[0019] Furthermore, in the step 3), 50-150 kg of aluminum particles are used to modify the top slag after steel is tapped.

[0020] Furthermore, in step 10), the graphite sealing ring is replaced in each furnace.

[0021] Furthermore, the control method achieves stable control of the rare earth content recovery rate in steel at a level above 45%.

[0022] Further, the pouring process was normal.

[0023] Compared with the prior art, the beneficial technical effects of the present invention are:

[0024] The present invention provides a control method for a deep drawing steelmaking and continuous casting process, in particular, a method for controlling the rare earth content yield in steel, so as to achieve a stable control of the rare earth content yield in steel at a level above 45%, thereby achieving the successful development and stable supply of deep drawing steel with high rare earth yield.

[0025] The present invention achieves high cleanliness of steel before rare earth alloying by controlling the oxygen content at the converter end, modifying the top slag after the furnace, RH vacuum decarburization and treating the slag system after the furnace, effectively improving the recovery rate of rare earth elements while improving production efficiency and ensuring continuous casting; compared with conventional production, the use of the method solves the problem of rare earth deep-drawing steel floc flow while highly improving the recovery rate of rare earth elements in steel, and the recovery rate of rare earth elements in steel can be stably controlled to be above 45%. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] The present invention will be further described below in conjunction with the accompanying drawings.

[0027] Figure 1 It is a schematic diagram of the implementation process of the present invention in the steelmaking process. DETAILED DESCRIPTION

[0028] Embodiment 1:

[0029] 1. According to the order situation, this method will be used to produce one heat in January 2024, with 260 tons of molten iron added to the converter and 48 tons of self-produced scrap added;

[0030] 2. The oxygen control requirement for converter steel tapping is 531ppm;

[0031] 3. The target for stable control of converter steel tapping is 1661℃;

[0032] 4. The slag making after the converter requires that 700kg of lime be added to the converter steel and 200kg of top slag modifier be added. After steel is tapped, aluminum particles (150kg) are used for top slag modification. Argon stirring is not allowed during the aluminum particle throwing process and after modification.

[0033] 5.RH in-situ temperature 1618℃, in-situ oxygen content 360ppm;

[0034] 6. During the RH decarburization process, the decarburization time is 17 minutes, the pure degassing time is 7 minutes, the interval between RH deoxidation and alloying is 4 minutes, the rare earth alloy is added during the alloying process, and 50kg of aluminum particles are thrown in by hand after breaking the air;

[0035] 7. The final slag components of refining have a CaO content of 44.27%, Al 2 O 3 Content 31.62%, SiO 2Content 9.96%, C / A range 1.40;

[0036] 8. The argon blowing time of the tundish before pouring is 6 minutes; the new graphite sealing ring of the long nozzle is used, and the argon flow rate is 4L / min; the covering agent must be added after temperature measurement and sampling; the casting machine increases nitrogen by 2ppm;

[0037] 9. Set the pulling speed to 1.00m / min and ensure that the pulling speed is constant; the pouring time is controlled at 51min, and the sensitivity of slag detection for large bags is 5%.

[0038] The specific chemical composition is shown in Table 1 below.

[0039] Table 1 Composition of the deep drawing steel in the middle of the heat (%)

[0040] Brand C Si Mn P S Alt Ti N O Ce Internal control limit 0.0030 0.030 0.20 0.015 0.010 0.055 0.067 0.0040 0.0030 0.0020 Internal control limit - - 0.12 - - 0.025 0.052 - - - St14 0.0014 0.003 0.16 0.010 0.009 0.038 0.059 0.0022 0.0020 0.0012

[0041] The amount of rare earth alloy added in this furnace is 20kg, the rare earth Ce element content in the rare earth alloy is 30%, the detected amount of rare earth Ce element in the middle package is 0.0012%, the total amount of molten steel in this furnace is 227.25 tons, and the rare earth recovery rate is 45.45%.

[0042] Embodiment 2:

[0043] 1. According to the order situation, this method will be used to produce one heat in May 2024, with 267 tons of molten iron added to the converter and 40 tons of self-produced scrap added;

[0044] 2. The oxygen control requirement for converter steel tapping is 371ppm for the final target oxygen;

[0045] 3. The target for stable control of converter steel tapping is 1702℃;

[0046] 4. The slag making after the converter requires that 700kg of lime be added to the converter before steel is tapped, and 250kg of top slag modifier be added. After steel is tapped, aluminum particles (150kg) are used for top slag modification. Argon stirring is not allowed during the aluminum particle throwing process and after modification.

[0047] 5.RH in-situ temperature 1607℃, in-situ oxygen content 217ppm;

[0048] 6. During the RH decarburization process, the decarburization time is 17 minutes, the pure degassing time is 7 minutes, the interval between RH deoxidation and alloying is 4 minutes, the rare earth alloy is added during the alloying process, and 50kg of aluminum particles are thrown in by hand after breaking the air;

[0049] 7. The refining final slag components have a CaO content of 44.61%, an Al2O3 content of 24.99%, a SiO2 content of 10.33%, and a C / A range of 1.78;

[0050] 8. The argon blowing time of the tundish before pouring is 6 minutes; the new graphite sealing ring of the long nozzle is used, and the argon flow rate is 4L / min; the covering agent must be added after temperature measurement and sampling; the casting machine increases nitrogen by 2ppm;

[0051] 9. Set the pulling speed to 1.20m / min and ensure that the pulling speed is constant; the pouring time is controlled at 48min, and the sensitivity of large bag slag detection is 5%.

[0052] The specific chemical composition is shown in Table 2 below.

[0053] Table 2 Composition of the deep drawing steel in the middle of the heat (%)

[0054]

[0055] The amount of rare earth alloy added in this furnace is 20 kg, the rare earth Ce element content in the rare earth alloy is 30%, the detected amount of rare earth Ce element in the middle package is 0.0010%, the total amount of molten steel in this furnace is 280.08 tons, and the rare earth recovery rate is 46.48%.

[0056] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.

Claims

1. A method for controlling a rare earth high-yield deep-drawing steelmaking and continuous casting process, characterized in that: The steps include: 1). The amount of molten iron added to the converter is 263±3t, and the amount of self-produced scrap steel added is 45±3t; 2). The oxygen control requirement for steel tapping in converter is 650-750ppm. If the oxygen in steel tapping is > 1000ppm, add 500±20kg of raw white oxygen reduction post-treatment; 3). The target of converter tapping stability control is 1640-1670℃. The temperature of the first quick-change furnace is not less than 1665℃; 4). The slag making after the converter requires that 600-800kg of lime be added to the converter before steel is tapped, and 200-250kg of top slag modifier be added. After steel is tapped, aluminum particles are used for top slag modification. Argon stirring is not allowed during the aluminum particle throwing process and after modification; 5).RH in-situ conditions require RH vacuum treatment for 5 minutes to determine oxygen, the first furnace is controlled at 1610-1620℃, the continuous casting furnace is controlled at 1600-1610℃, and the oxygen content is controlled at 350-500ppm; 6). RH decarburization process: decarburization time is 17 minutes, pure degassing time is 7 minutes, and each blowing is 100Nm 3 The oxygen pure degassing was extended for 1 minute; 7). The time interval between RH deoxidation and alloying is 4 minutes, and the rare earth alloy is added during the alloying process; 8). After the RH negative pressure is broken, when the molten steel leaves the immersion tube, 50-100kg of aluminum particles are sprinkled on the surface of the slag to modify the top slag; 9). The refining final slag components have a CaO content of 40-55%, an Al2O3 content of 20-35%, a SiO2 content of 5-15%, and a C / A range of 1.4-1.8; 10). Before pouring, argon is blown in the tundish for a time of >3 min. To ensure the tightness of the long nozzle, use a graphite sealing ring, and the argon flow rate is 2-6 L / min. Pay attention to the tumbling of the molten steel in the impact zone, and the flow rate can be increased appropriately. After temperature measurement and sampling, the covering agent must be added. The casting machine is required to increase N ≤5ppm. 11). Set the pulling speed to 1.00-1.20m / min and maintain a constant pulling speed. The pouring time is controlled at 45-50min.

2. The method for controlling the rare earth high-yield deep-drawing steelmaking and continuous casting process according to claim 1, characterized in that: In the step 1), 263 tons of molten iron and 45 tons of self-produced scrap steel are added to the converter.

3. The method for controlling the rare earth high-yield deep-drawing steelmaking and continuous casting process according to claim 1, characterized in that: In the step 2), 500 kg of raw white is added for oxygen reduction treatment.

4. The method for controlling the rare earth high-yield deep-drawing steelmaking and continuous casting process according to claim 1, characterized in that: In the step 3), 50-150 kg of aluminum particles are used to modify the top slag after steel is tapped.

5. The method for controlling the rare earth high-yield deep-drawing steelmaking and continuous casting process according to claim 1, characterized in that: In the step 10), the graphite sealing ring is replaced in each furnace.

6. The method for controlling the rare earth high-yield deep-drawing steelmaking and continuous casting process according to claim 1, characterized in that: The control method can achieve stable control of the recovery rate of rare earth content in steel at a level above 45%.

7. The method for controlling the rare earth high-yield deep-drawing steelmaking and continuous casting process according to claim 6, characterized in that: The pouring process is normal.