Preparation method of silicon-carbon steel, silicon-carbon steel and application of silicon-carbon steel
By adopting a step-by-step deoxidation method during RH refining, the oxygen content and inclusions in low-carbon and low-silicon steel are reduced, and the Si and Al content control problems in the preparation of low-carbon and low-silicon steels are solved, stamping performance and surface quality are improved, and the stamping performance and surface quality are achieved. Preparation of high-quality silicon carbon steel.
Patent Information
- Application Number
- CN202411015568.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-11-22
AI Technical Summary
It is difficult to control the Si and Al content during the refining process of low-carbon and low-silicon steel, resulting in poor stamping performance, poor surface quality and production interruption.
采用分步脱氧方法,在RH精炼过程中先进行预脱氧处理,然后进行脱氧合金化处理,通过加入硅铁和铝块,降低钢中的氧含量并减少夹杂物,提高钢水洁净度。
High-quality preparation of low-carbon and low-silicon steel is achieved, with good stamping performance, surface quality and ductility, avoiding production interruptions and improving the overall performance of the steel.
Smart Images

Figure CN118996052A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of metal casting technology, and in particular to a preparation method of silicon carbon steel, silicon carbon steel and applications thereof. Background Art
[0002] As we all know, the carbon content in low-carbon, low-silicon steel is 0.02% to 0.05%. The relatively high carbon content leads to poor stamping performance of the product, which cannot meet the requirements of products with large stamping volume. In order to ensure the coatability of the cold-rolled substrate during the galvanizing process, the silicon content in the steel is required to be ≤0.03%. However, when silicon deoxidation is used in LF refining, the Si content in the steel can easily exceed 0.03%, so aluminum deoxidation can only be used in the LF refining process. However, when aluminum deoxidation is used, the aluminum in the steel will reduce SiO2 in the slag during the slag stirring process, thereby increasing the Si content in the steel and causing the Si element composition in the steel to exceed the standard. Therefore, in the LF refining process, the Si content needs to be controlled below 0.03%, and the SiO2 content in the slag needs to be below 10%.
[0003] As for the preparation of low-carbon, low-silicon steel, the Al content in low-carbon, low-silicon steel is low, the Al2O3 inclusions in the steel are more, and the SiO2 content in the slag is low, resulting in a higher melting point of the slag, poor fluidity, and poor effect of adsorbing inclusions, which further leads to poor cleanliness of the molten steel. In addition, when the molten steel containing more Al2O3 inclusions is directly put on the continuous casting stage, the inclusions will quickly accumulate and form nodules at the continuous casting plug rod and the water nozzle, blocking the flow of molten steel and causing production interruption. Therefore, the current low-carbon, low-silicon steel needs to be treated with calcium before the end of LF, so that the high-melting point solid Al2O3 inclusions are transformed into low-melting point liquid calcium aluminate inclusions, so as to ensure the smoothness of the continuous casting process. However, the use of calcium treatment will pollute the molten steel and increase the size of the inclusions in the steel, especially the B-type string inclusions. Such inclusions will not only cause surface quality problems of hot-rolled coils and cold-rolled coils, but also easily cause cracking in the product during the stamping process. Summary of the invention
[0004] In order to solve the above problems, the present application proposes a method for preparing silicon carbon steel, silicon carbon steel and its application. The preparation method adopts a step-by-step deoxidation method to reduce the oxygen content in the steel during the refining process, while not polluting the molten steel, improving the cleanliness of the molten steel, and thus improving the product quality of the steel; the number of inclusions in the steel after deoxidation is small. The carbon content in the silicon carbon steel is below 0.02%, and it has good stamping performance, surface quality and ductility.
[0005] This application is implemented through the following technical solutions:
[0006] In a first aspect, the present application proposes a method for preparing silicon carbon steel, comprising the following steps:
[0007] In the RH refining step, ferrosilicon is added after decarburization for pre-deoxidation treatment, and then aluminum blocks are added for deoxidation and alloying treatment; wherein the amount of ferrosilicon added is 0.4kg / t to 0.8kg / t.
[0008] The preparation method of silicon carbon steel proposed in the first aspect of the present application adopts a step-by-step deoxidation method of pre-deoxidation treatment and deoxidation alloying treatment to reduce the oxygen content in the steel, while not polluting the molten steel, improving the cleanliness of the molten steel, and thus improving the product quality of the steel; the number of inclusions in the steel after deoxidation is relatively small.
[0009] kg / t refers to the mass kg added to every t (ton) of molten steel.
[0010] In some possible implementations, the amount of ferrosilicon added is 0.56 kg / t to 0.8 kg / t, preferably 0.56 kg / t. Within this amount range, the prepared silicon carbon steel has good stamping performance, no cracking occurs during the stamping process, and the elongation of the silicon carbon steel can reach 41%.
[0011] In some possible implementations, the mass fractions of the components in the ferrosilicon are: silicon 75% to 77%, iron 20% to 25%, and the rest are unavoidable impurities. In this case, the oxygen content in the molten steel will be significantly reduced, the remaining free oxygen is about 100 ppm, and the deoxidation reaction product is SiO2 inclusions, which are easy to float and remove.
[0012] Preferably, the mass fractions of the components in the ferrosilicon are: 76% silicon, 23% iron, and the rest are inevitable impurities. This is a common ferrosilicon in steel metallurgy, with low cost and wide use. After being added to molten steel, it can fully react with oxygen in steel.
[0013] In some possible implementations, the pre-deoxidation treatment step includes: RH cycle; the RH cycle time is 2 minutes to 5 minutes. In this case, after the RH cycle, the free oxygen content in the steel (water) is about 100 ppm.
[0014] In some possible implementations, the amount of aluminum block added is 0.20 kg / t to 0.40 kg / t. Within this range, the remaining free oxygen in the molten steel will react completely with aluminum and be completely removed, the total amount of Al2O3 inclusions generated is small, and most of them will float up and be removed in the RH pure cycle.
[0015] Furthermore, the added amount of the aluminum block is 0.30 kg / t.
[0016] In some possible implementations, the deoxidation alloying treatment step includes: RH pure cycle; the time of the pure cycle is 4 minutes to 6 minutes. In this case, the RH pure cycle can remove Al2O3 inclusions in the steel.
[0017] In the second aspect, the present application proposes a silicon carbon steel prepared by the silicon carbon steel preparation method proposed in the present application, wherein the mass fraction of carbon in the silicon carbon steel is less than 0.02%, the mass fraction of silicon is less than 0.05%, and the mass fraction of aluminum is 0.015% to 0.06%.
[0018] The silicon carbon steel proposed in the second aspect of the present application has good stamping performance, surface quality and steel cleanliness because the carbon content is less than 0.02%.
[0019] In some possible implementations, the mass fraction of carbon in the silicon carbon steel is 0.016% to 0.02%, the mass fraction of silicon is 0.036% to 0.05%, and the mass fraction of aluminum is 0.029% to 0.06%.
[0020] In some possible implementations, the mass fraction of carbon in the silicon carbon steel is 0.016%, the mass fraction of silicon is 0.036%, and the mass fraction of aluminum is 0.029%. The silicon carbon steel with this mass fraction has good stamping performance, no cracking occurs during the stamping process, and the elongation of the silicon carbon steel can reach 41%.
[0021] In some possible implementations, the mass fraction of carbon in the silicon carbon steel is 0.018%, the mass fraction of silicon is 0.031%, and the mass fraction of aluminum is 0.025%. The silicon carbon steel with this mass fraction has good stamping performance, no cracking occurs during the stamping process, and the elongation of the silicon carbon steel can reach 45%.
[0022] In some possible implementations, the mass fraction of carbon in the silicon carbon steel is 0.017%, the mass fraction of silicon is 0.042%, and the mass fraction of aluminum is 0.031%. The silicon carbon steel with this mass fraction has good stamping performance, no cracking occurs during the stamping process, and the elongation of the silicon carbon steel can reach 44%.
[0023] On the third aspect, the present application proposes an application of the silicon carbon steel provided by the present application in the fields of bridges, buildings, wire products or automobile bodies. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] In order to more clearly illustrate the embodiments of the present drawings or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present drawings. For ordinary technicians in this field, other drawings can be obtained based on the structures shown in these drawings without paying any creative work.
[0025] Figure 1a A diagram of a continuous casting water outlet in the method for preparing silicon carbon steel in Example 1 of the present application;
[0026] Figure 1b This is a diagram of the continuous casting water outlet in the method for preparing silicon carbon steel in Comparative Example 1 of the present application.
[0027] The purpose, features and advantages of this figure will be further described in conjunction with the embodiments with reference to the accompanying drawings. DETAILED DESCRIPTION
[0028] In order to make the purpose, technical solutions and advantages of the present application clearer, the present application is described and illustrated below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present application and are not intended to limit the present application. Based on the embodiments provided in the present application, all other embodiments obtained by ordinary technicians in the field without making creative work are within the scope of protection of the present application.
[0029] Obviously, the following descriptions are only some examples or embodiments of the present application. For ordinary technicians in this field, the present application can also be applied to other similar scenarios without creative work. In addition, it can also be understood that although the efforts made in this development process may be complicated and lengthy, for ordinary technicians in the field related to the content disclosed in this application, some changes in design, manufacturing or production based on the technical content disclosed in this application are just conventional technical means, and should not be understood as insufficient content disclosed in this application.
[0030] However, unnecessary detailed descriptions may be omitted. For example, detailed descriptions of well-known matters and repeated descriptions of substantially the same structures may be omitted. This is to avoid the following description from becoming unnecessarily lengthy and to facilitate understanding by those skilled in the art. In addition, the following description is provided for those skilled in the art to fully understand the present application and is not intended to limit the subject matter described in the claims.
[0031] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.
[0032] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.
[0033] The "range" disclosed in the present application is defined in the form of a lower limit and an upper limit, and a given range is defined by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundaries of the particular range. The range defined in this way can be inclusive or exclusive of the end values, and can be arbitrarily combined, that is, any lower limit can be combined with any upper limit to form a range. For example, if a range of 60 to 120 and 80 to 110 is listed for a particular parameter, it is understood that a range of 60 to 110 and 80 to 120 is also expected. In addition, if the minimum range values 1 and 2 are listed, and if the maximum range values 3, 4 and 5 are listed, the following ranges can all be expected: 1 to 3, 1 to 4, 1 to 5, 2 to 3, 2 to 4 and 2 to 5. In the present application, unless otherwise specified, the numerical range "ab" represents an abbreviation of any real number combination between a and b, where a and b are both real numbers. For example, the numerical range "0-5" means that all real numbers between "0-5" are listed in this document, and "0-5" is just an abbreviation of these numerical combinations. In addition, when a parameter is expressed as an integer ≥ 2, it is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.
[0034] If there is no special explanation, all steps of the present application can be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), which means that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), which means that step (c) may be added to the method in any order. For example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.
[0035] If there is no special explanation, the "include" and "comprising" mentioned in this application are open-ended or closed-ended. For example, the "include" and "comprising" may mean that other components not listed may also be included or only the listed components may be included or only the listed components may be included.
[0036] If not specifically stated, in this application, the term "or" is inclusive. For example, the phrase "A or B" means "A, B, or both A and B". More specifically, any of the following conditions satisfies the condition "A or B": A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).
[0037] Example 1
[0038] This embodiment provides a method for preparing silicon carbon steel, comprising the following steps:
[0039] (1) Converter steelmaking: A 210t converter is used to smelt molten steel, with a steel output of 215 tons and a converter end oxygen of 680ppm.
[0040] (2) RH refining:
[0041] ① Decarburization: Decarburize the molten steel under the extreme vacuum of 10Pa to 100Pa of RH (the vacuum degree fluctuates during the RH treatment and has no fixed value). The decarburization time is 3 minutes. The carbon content in the steel at the end of decarburization is 0.015%, and the oxygen content at the end of decarburization is 355ppm.
[0042] ② Pre-deoxidation: After decarburization, 120kg (about 0.56kg / t) of ferrosilicon is added for pre-deoxidation. After adding ferrosilicon, RH circulation is carried out for 3 minutes. At this time, the free oxygen content in the steel is 95ppm. Among them, the mass fraction of silicon in ferrosilicon is 76%, and the mass fraction of iron is 23%.
[0043] ③ Deoxidation and alloying: After pre-deoxidation, add 80kg aluminum block for deoxidation and alloying, followed by 5min of RH pure cycle.
[0044] (3) The steel after leaving the station is subjected to steps including continuous casting and rolling to obtain silicon carbon steel.
[0045] Example 2
[0046] Example 2 proposes a method for preparing silicon carbon steel, and the steps are basically the same as those of Example 1, except that in the pre-deoxidation step, the mass of ferrosilicon added is 86 kg (0.4 kg / t).
[0047] Example 3
[0048] Example 3 proposes a method for preparing silicon carbon steel. The steps are basically the same as those of Example 1, except that in the pre-deoxidation step, the mass of ferrosilicon added is 172 kg (0.8 kg / t).
[0049] Comparative Example 1
[0050] Comparative Example 1 proposes a method for preparing silicon carbon steel, comprising the following steps:
[0051] (1) Converter steelmaking: A 210t converter is used to smelt molten steel, with a steel output of 215 tons and a converter end oxygen of 680ppm.
[0052] (2) RH refining:
[0053] ① Decarburization: Decarburize the molten steel under the extreme vacuum degree of 10Pa~100Pa of RH. The decarburization time is 3min. The carbon content in the steel at the end of decarburization is 0.015%, and the oxygen content at the end point of decarburization is 355ppm.
[0054] ② Deoxidation and alloying: directly add 80kg aluminum block for deoxidation and alloying, followed by 5min of RH pure cycle.
[0055] (3) The steel after leaving the station is subjected to steps including continuous casting and rolling to obtain silicon carbon steel.
[0056] Comparative Example 2
[0057] Comparative Example 2 proposes a method for preparing silicon carbon steel, comprising the following steps:
[0058] (1) Converter steelmaking: A 210t converter is used to smelt molten steel, with a steel output of 215 tons and a converter end oxygen of 680ppm.
[0059] (2) LF refining:
[0060] ① During the LF refining process, aluminum blocks were added in three batches for deoxidation and alloying, with a total addition amount of 80 kg.
[0061] ② In the later stage of LF smelting, calcium treatment operation is carried out. 350m of pure calcium line is fed, soft blowing is carried out for 8 minutes, and then casting is carried out on the stage to obtain silicon carbon steel.
[0062] (3) The steel after leaving the station is subjected to steps including continuous casting and rolling to obtain silicon carbon steel.
[0063] Comparative Example 3
[0064] Comparative Example 3 proposes a method for preparing silicon carbon steel, and the steps are basically the same as those of Example 1, except that in the pre-deoxidation step, the mass of ferrosilicon added is 215 kg (1 kg / t).
[0065] Comparative Example 4
[0066] Comparative Example 4 proposes a method for preparing silicon carbon steel, and the steps are basically the same as those of Example 1, except that in the pre-deoxidation step, the mass of ferrosilicon added is 64.5 kg (0.3 kg / t).
[0067] In order to verify the progress of the embodiments of the present application, during the preparation of silicon carbon steel in Example 1 and Comparative Example 1, the aluminum oxide inclusions in the molten steel after deoxidation and alloying treatment were detected and rated as shown in Table 1 below. At the same time, the nozzle was observed to be free of nodules, as shown in the attached manual. Figure 1a and 1b As shown; the composition, elongation, cracking incidence and surface defect incidence of the silicon carbon steel prepared in Examples 1 to 3 and Comparative Examples 1 to 4 were tested, and the results are shown in Table 2 below.
[0068] Table 1
[0069]
[0070] It can be seen from Table 1 above and Figure 1 of the specification that:
[0071] (1) From the inclusion ratings of RH outlet and tundish molten steel of Example 1 and Comparative Example 1 in Table 1, it can be seen that when comparative example 1 is used for aluminum deoxidation RH outlet, a large number of clustered Al2O3 inclusions are still present in the molten steel, and the D-type inclusion rating reaches 5.0; while the D-type inclusion rating in the steel obtained by silicon-aluminum step-by-step deoxidation in Example 1 is only 1.5, and no Al2O3 aggregation is found. In addition, the D-type inclusion rating of the tundish molten steel of Example 1 is reduced to 2.0 and 1.0, respectively. It can be seen that the preparation method of silicon-carbon steel in the embodiment of the present application can effectively reduce the number of inclusions in the molten steel and improve the quality and safety of silicon-carbon steel.
[0072] (2) Attached to the instruction manual Figure 1a and 1b It can be seen that Example 1 of the present application has undergone pre-deoxidation treatment. Therefore, the oxygen content in the steel is very low before adding aluminum deoxidation, and the number of inclusions generated by deoxidation is relatively small, and the nodule formation at the continuous casting nozzle is good; while the method of Comparative Example 1 does not use ferrosilicon for pre-deoxidation before aluminum deoxidation, and the aluminum oxide inclusions generated by deoxidation in the steel are relatively large, and the nodule formation at the nozzle is very serious during the continuous casting of molten steel.
[0073] Table 2
[0074] Carbon content Silicon content Aluminum content Elongation Cracking incidence Surface defect incidence Example 1 0.016% 0.036% 0.029% 41% 0% 0% Example 2 0.018% 0.031% 0.025% 45% 0% 0% Example 3 0.017% 0.042% 0.031% 44% 0% 0% Comparative Example 1 0.015% 0.032% 0.028% 42% 0% 8.8% Comparative Example 2 0.033% 0.044% 0.031% 29% 3.27% 4.5% Comparative Example 3 0.016% 0.057% 0.032% 43% 1.21% 0% Comparative Example 4 0.019% 0.022% 0.023% 39% 0% 3.5%
[0075] Note: The cracking and surface defects of the steel in Table 2 are observed with the naked eye. If there is no cracking visually, the cracking rate is 0%, and if there is no surface defect visually, the surface defect rate is 0%.
[0076] It can be seen from Table 2 above:
[0077] The elongation of the silicon carbon steel of Examples 1 to 3 is more than 41%, and the cracking incidence and surface defect incidence are both 0. It can be seen that the silicon carbon steel prepared by the method for preparing silicon carbon steel of the embodiment of the present application not only has a very low carbon content, but also has good stamping performance (cracking incidence), surface quality (surface defect incidence) and ductility (elongation).
[0078] It should be noted that the present application is not limited to the above-mentioned embodiments. The above-mentioned embodiments are only examples, and the embodiments having the same structure as the technical idea and exerting the same effect within the scope of the technical solution of the present application are all included in the technical scope of the present application. In addition, without departing from the scope of the main purpose of the present application, various modifications that can be thought of by those skilled in the art to the embodiments and other methods of combining some of the constituent elements in the embodiments are also included in the scope of the present application.
Claims
1. A method for preparing silicon carbon steel, characterized in that: The preparation method comprises the following steps: In the RH refining step, ferrosilicon is added after decarburization for pre-deoxidation treatment, and then aluminum blocks are added for deoxidation and alloying treatment; wherein the amount of ferrosilicon added is 0.4kg / t to 0.8kg / t.
2. The method for preparing silicon carbon steel according to claim 1, characterized in that: The added amount of the ferrosilicon is 0.56kg / t to 0.8kg / t.
3. The method for preparing silicon carbon steel according to claim 1, characterized in that: The mass fractions of the components in the ferrosilicon are: silicon 75% to 77%, iron 20% to 25%, and the rest are inevitable impurities.
4. The method for preparing silicon carbon steel according to claim 1, characterized in that: The steps of the pre-deoxidation treatment include: RH cycle; The RH cycle time is 2 min to 5 min.
5. The method for preparing silicon carbon steel according to claim 1, characterized in that: The added amount of the aluminum block is 0.20kg / t to 0.40kg / t.
6. The method for preparing silicon carbon steel according to claim 5, characterized in that: The added amount of the aluminum block is 0.30kg / t to 0.40kg / t.
7. The method for preparing silicon carbon steel according to any one of claims 1 to 6, characterized in that: The deoxidation alloying treatment comprises: RH pure cycle; the time of the pure cycle is 4 minutes to 6 minutes.
8. A silicon carbon steel prepared by the method for preparing silicon carbon steel according to any one of claims 1 to 7, characterized in that: The mass fraction of carbon in the silicon carbon steel is less than 0.02%, the mass fraction of silicon is less than 0.05%, and the mass fraction of aluminum is 0.015% to 0.06%.
9. The silicon carbon steel according to claim 8, characterized in that: The mass fraction of carbon in the silicon carbon steel is 0.016% to 0.02%, the mass fraction of silicon is 0.036% to 0.05%, and the mass fraction of aluminum is 0.029% to 0.06%.
10. Use of the silicon carbon steel according to claim 8 or 9 in the fields of bridges, buildings, wire products or automobile bodies.